Method for bleaching cotton-type knitted fabric at low temperature
By preparing a metal complex of sodium (E)-3-(((1,3-dihydroxy-2-(hydroxymethyl)propan-2-yl)imino)methyl)-4-hydroxybenzenesulfonate It solves the problems of high energy consumption and insufficient catalyst stability of the traditional high-temperature bleaching process, realizes low-temperature and efficient bleaching of cotton knitted fabrics, and improves whiteness and bursting strength retention rate.
Patent Information
- Application Number
- CN202410825728.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The traditional bleaching process of cotton knitted fabrics results in high energy consumption and large loss of fabric bursting strength at high temperatures. Moreover, the stability and catalytic efficiency of existing low-temperature bleaching catalysts are insufficient, which affects industrial application.
Preparation of a metal complex of sodium (E)-3-(((1,3-dihydroxy-2-(hydroxymethyl)propan-2-yl)imino)methyl)-4-hydroxybenzenesulfonate , used to bleach cotton knitted fabrics under low temperature conditions, and improve its stability and catalytic performance by adjusting the structure and chemical microenvironment of the catalyst.
It achieves efficient bleaching of cotton knitted fabrics at low temperatures, reduces energy consumption, improves whiteness and bursting strength retention, and significantly improves the stability and catalytic capacity of the catalyst.
Smart Images

Figure CN118854656A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of textile printing and dyeing, and in particular relates to a method for low-temperature bleaching of cotton knitted fabrics. Background Art
[0002] In the bleaching process of cotton knitted fabrics, the traditional process usually uses hydrogen peroxide, sodium hydroxide and surfactants at a high temperature of 100°C. Hydrogen peroxide can destroy the pigment of the fabric under the action of sodium hydroxide to achieve the purpose of bleaching; at the same time, hydrogen peroxide can also destroy the accompanying substances of the fabric such as pectin, wax, grease, etc., and remove them through surfactants. High temperature causes energy waste, which does not meet the current low-carbon and green industry development requirements. It also leads to a large loss of bursting strength and a high weight loss rate of the bleached fabric, affecting product quality.
[0003] Researchers are committed to the development of low-temperature bleaching technology to reduce energy consumption and ensure the bleaching effect of fabrics. People have tried to add activators and catalysts to the hydrogen peroxide bleaching system. Typical bleaching activators are tetraacetylethylenediamine (TAED), sodium nonanoyloxybenzenesulfonate (NOBS) and N-[4-(triethylammoniummethylene)benzoyl]caprolactam chloride (TBCC). The bleaching effect is better when using activators, but the amount of activators used is large and the price is high. At present, it has not been mass-produced in China. Schiff base metal complexes are better as catalysts, but most Schiff base complexes have poor water solubility and are difficult to apply to systems with water as the reaction medium. Reference 1 (Li Jingyan, Song Min, Zhang Linping, Mao Zhiping. Application of Schiff base metal complexes in low-temperature bleaching of cotton fabrics [J]. Journal of Donghua University (Natural Science Edition), 2012, 38(1): 55-59) synthesized Schiff base copper complex CuL1 as a catalyst for hydrogen peroxide bleaching. The solution pH was 9.5. After steaming at 80℃ for 60min, the whiteness of the bleached fabric could reach 71.2%, and it had a high strength retention rate. Reference 2 (Wu Chenren, Lv Wangyang, Chen Wenxing. Application of copper complexes in low-temperature neutral bleaching of cotton knitted fabrics [J]. Journal of Textile Research, 2019, 40(1): 91-96) used iminodiacetic acid, divalent copper ions and pyridine derivatives to prepare a low-temperature bleaching catalyst. Under neutral conditions, the whiteness of the bleached fabric reached 75.03% after treatment at 60℃ for 60min, but the bursting strength retention rate was about 89%. The stability and catalytic efficiency of metal complex catalysts are important factors affecting their practical applications.
[0004] Metal complexes are used as catalysts for bleaching in the textile printing and dyeing industry. They draw on the structural characteristics and properties of natural enzymes (hence metal complexes are also called enzyme-mimicking catalysts). Their catalytic function mainly depends on the chemical structure of the active site, but the chemical microenvironment of the active site has a great influence on its stability and catalytic efficiency. Introducing other functional groups, regulating the catalyst structure and the chemical microenvironment of the active site, and enhancing resistance to the application environment such as solution pH, impurities, etc. are crucial to improving the stability and catalytic ability of metal complexes. Summary of the invention
[0005] In view of the deficiencies of the prior art, the present invention prepares a metal complex of sodium (E)-3-(((1,3-dihydroxy-2-(hydroxymethyl)propan-2-yl)imino)methyl)-4-hydroxybenzenesulfonate, which is used to enhance the stability and catalytic performance of the metal complex, and bleach cotton knitted fabrics under low temperature conditions to reduce energy consumption. At the same time, the present invention also specifically provides a method for low-temperature bleaching of cotton knitted fabrics.
[0006] To achieve the above object, the present invention first provides a method for preparing a metal complex of sodium (E)-3-(((1,3-dihydroxy-2-(hydroxymethyl)propan-2-yl)imino)methyl)-4-hydroxybenzenesulfonate, specifically:
[0007] Step 1: In a three-necked flask reaction vessel equipped with a stirrer and a condenser reflux tube, slowly add 98% concentrated sulfuric acid to the salicylaldehyde solution under ice-water bath conditions, continue stirring until the addition is complete, and react at 30-55°C for 18-24 hours. Then add an appropriate amount of ice water, and then add anhydrous sodium carbonate. Stop stirring after the reaction solution becomes clear, and let it stand for 18-48 hours. Filter under reduced pressure, recrystallize with 70% mass fraction ethanol aqueous solution, then wash with anhydrous ethanol, and vacuum dry to obtain sulfonated salicylaldehyde. The molar ratio of salicylaldehyde to 98% concentrated sulfuric acid and anhydrous sodium carbonate is 1:(20-30):(10-15);
[0008] Step 2: In a three-necked flask reaction vessel equipped with a stirrer and a condenser reflux tube, sulfonated salicylaldehyde and tris(hydroxymethyl)aminomethane are mixed and stirred at a molar ratio of 1:1 to 1.5:1 under the condition of 60 to 95% ethanol concentration, and reacted at a temperature of 40 to 75° C. for 4 to 8 hours. After cooling, the mixture is precipitated and filtered, and washed with anhydrous ethanol to obtain a yellow Schiff base solid of salicylaldehyde tris(hydroxymethyl)aminomethane, the structural formula of which is:
[0009]
[0010] Step 3: In a three-necked flask reaction vessel equipped with a stirrer and a condensation reflux device, add 80% ethanol-dissolved salicylaldehyde tris(hydroxymethyl)aminomethane) and 80% ethanol-dissolved metal salt in a molar ratio of 1:(1-2), then add sodium bicarbonate to adjust the pH to 9-10, and react at a temperature of 30-65°C for 4-16 hours. After the reaction is completed, cool to room temperature and filter, recrystallize with a 70% methanol solution, filter, wash with anhydrous methanol, and vacuum dry to obtain a Schiff base metal complex with the general structural formula:
[0011]
[0012] M is Cu, Fe, or Mn
[0013] The invention provides a method for low-temperature bleaching of a cotton knitted fabric, and provides the following specific technical scheme: adding the cotton knitted fabric into a bleaching solution, bleaching the fabric at a certain bath ratio, washing the bleached fabric with water, and drying the fabric, wherein the low-temperature bleaching solution comprises: hydrogen peroxide, a copper complex, an iron complex or a manganese complex of a catalyst (E)-3-(((1,3-dihydroxy-2-(hydroxymethyl)prop-2-yl)imino)methyl)-4-hydroxybenzenesulfonate sodium, sodium hydroxide, a penetrant, a scouring agent, and a stabilizer.
[0014] Preferably, the cotton knitted fabric is pure cotton knitted fabric or polyester-cotton blended knitted fabric.
[0015] Preferably, the bath ratio is 1:8 to 1:30.
[0016] Preferably, the bleaching temperature is 60-85°C, and the bleaching time is 30-70 minutes.
[0017] Preferably, the bleaching solution comprises 30% (mass fraction) hydrogen peroxide 8-18 g / L, metal complex catalyst 6-80 μmol / L, sodium hydroxide 1-3 g / L, penetrant 0.5-2 g / L, scouring agent 0.5-3 g / L, and stabilizer 0.5-2 g / L.
[0018] Preferably, the penetrant is JFC.
[0019] Preferably, the scouring agent is one or a composite of E1009, E1305, E1310, AEO-9.
[0020] Preferably, the stabilizer is one or a complex of sodium silicate, diethylamine pentaacetic acid, trisodium citrate.
[0021] The beneficial effects of the present invention are as follows:
[0022] The prepared metal complex catalyst has more polar groups, phenolic hydroxyl or alcoholic hydroxyl, which can participate in the coordination of metal ions, and alcoholic hydroxyl can also participate in the coordination of metal ions; it has a stereo conformation, which improves the stability of the metal complex in the bleaching solution. The catalyst can bleach cotton knitted fabrics at low temperatures, save energy and reduce production costs; the bleached fabric has high whiteness and bursting strength retention rates.
[0023] Mechanism: The metal complex catalyst has a typical Schiff base structure, so it can form a six-membered ring complex with metal ions. There are multiple hydroxyl groups around the active center, which are in a peripheral stereo conformation with the sodium benzenesulfonate structure. It has a certain negative charge and can resist the capture of the metal ions in the active center by anions in the solution environment, as well as the coating of the metal ions in the active center by grease, pectin, wax, etc. that fall off the fabric after bleaching in the solution. However, it does not affect the neutral hydrogen peroxide molecules approaching the active center, thereby improving the stability of the metal complex catalyst. In addition, theoretical calculations have shown that the negative charge of the oxygen atom of the alcohol hydroxyl group in the ligand of this structure is equivalent to that of the oxygen atom of the phenolic hydroxyl group, and the former is even more negative. Therefore, it can also form a five-membered ring complex with metal ions. The remaining alcohol hydroxyl groups and the sodium p-hydroxybenzenesulfonate structure are located outside the active center and form a stereo conformation structure, which can also maintain its stability in the bleaching solution. Taking copper complexes as an example, Figure 1 The characteristic peak of the hydroxyl group of the Schiff base ligand is at 3397 cm -1 , after forming a copper complex, it appears at 3416cm -1 , indicating that the alcohol hydroxyl group is coordinated; the characteristic peak of C=N increases from 1632cm -1 Move to 1602cm -1 The characteristic peak of phenolic hydroxyl group is 1520cm -1 Move to 1534cm -1 The above results prove that the copper complex has both six-membered ring coordination and five-membered ring coordination. Figure 2 As shown, the control group is a bleaching system using a copper complex as a catalyst but without adding any quencher, L-histidine is a quencher of singlet oxygen, dimethyl sulfoxide (DMSO) is a quencher of hydroxyl radicals, and p-benzoquinone is a quencher of superoxide radicals. It can be seen that after adding the quencher, the whiteness of the bleached fabrics is reduced. Different from the catalytic mechanism of other copper complexes as low-temperature bleaching catalysts (Document 2, forming copper oxygen radicals), the copper complex provided by the present invention catalyzes hydrogen peroxide to form singlet oxygen, hydroxyl radicals, superoxide radicals, etc., and the bleaching mechanism dominated by singlet oxygen and superoxide radicals improves the bleaching performance of the bleaching solution system on fabrics. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 FTIR spectra of Schiff base ligand and Schiff base copper complex
[0025] Figure 2 Whiteness of fabrics after adding quenchers to different bleaching systems DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Embodiment 1:
[0028] (1) 32S pure cotton knitted fabric (140g / m 2 );
[0029] (2) Bleaching prescription: 30% hydrogen peroxide 8 g / L, copper complex 30 μmol / L, sodium hydroxide 3 g / L, penetrant JFC 2 g / L, scouring agent E1009 3 g / L, stabilizer sodium silicate 1 g / L;
[0030] (3) Low-temperature bleaching process: Accurately weigh a certain mass of fabric, immerse it in bleaching solution, bath ratio 1:30, 85℃, 30min, wash with water, and dry.
[0031] Embodiment 2:
[0032] (1) 21S pure cotton knitted fabric (180g / m 2 );
[0033] (2) Bleaching prescription: 30% hydrogen peroxide 18 g / L, copper complex 80 μmol / L, sodium hydroxide 2.5 g / L, penetrant JFC 0.5 g / L, scouring agent E1310 0.5 g / L, stabilizer diethylamine pentaacetic acid 2 g / L;
[0034] (3) Low-temperature bleaching process: Accurately weigh a certain mass of fabric, immerse it in bleaching solution, bath ratio 1:8, 70℃, 55min, wash with water, and dry.
[0035] Embodiment 3:
[0036] (1) 40S pure cotton knitted fabric (160g / m 2 );
[0037] (2) Bleaching prescription: 30% hydrogen peroxide 9 g / L, copper complex 6 μmol / L, sodium hydroxide 2 g / L, penetrant JFC 0.5 g / L, scouring agent E1009 1.5 g / L, stabilizer diethylamine pentaacetic acid 1 g / L;
[0038] (3) Low-temperature bleaching process: Accurately weigh a certain mass of fabric, immerse it in bleaching solution, bath ratio 1:10, 70℃, 50min, wash with water, and dry.
[0039] Embodiment 4:
[0040] (1) T / C65 / 35, 150D / 21S polyester-cotton knitted fabric (145g / m 2 );
[0041] (2) Bleaching prescription: 30% hydrogen peroxide 14 g / L, copper complex 10 μmol / L, sodium hydroxide 1 g / L, penetrant JFC 1 g / L, scouring agent AEO-9 1 g / L, stabilizer trisodium citrate 0.5 g / L;
[0042] (3) Low-temperature bleaching process: Accurately weigh a certain mass of fabric, immerse it in bleaching solution, bath ratio 1:16, 70℃, 50min, wash with water, and dry.
[0043] Embodiment 5:
[0044] (1) T / C50 / 50, 130D / 40S polyester-cotton knitted fabric (160g / m 2 );
[0045] (2) Bleaching prescription: 30% hydrogen peroxide 12 g / L, copper complex 45 μmol / L, sodium hydroxide 2 g / L, penetrant JFC 1 g / L, scouring agent E1305 1 g / L, stabilizer trisodium citrate 1 g / L;
[0046] (3) Low-temperature bleaching process: Accurately weigh a certain mass of fabric, immerse it in bleaching solution, bath ratio 1:20, 60℃, 70min, wash with water, and dry.
[0047] Comparative Example 1:
[0048] (1) 32S pure cotton knitted fabric (140g / m 2 );
[0049] (2) Bleaching prescription: 30% hydrogen peroxide 8g / L, sodium hydroxide 3g / L, penetrant JFC 2g / L, scouring agent E10093g / L, stabilizer sodium silicate 1g / L;
[0050] (3) Low-temperature bleaching process: Accurately weigh a certain mass of fabric, immerse it in bleaching solution, bath ratio 1:30, 85℃, 30min, wash with water, and dry.
[0051] Comparative Example 2:
[0052] (1) 21S pure cotton knitted fabric (180g / m 2 );
[0053] (2) Bleaching prescription: 30% hydrogen peroxide 18 g / L, sodium hydroxide 2.5 g / L, penetrant JFC 0.5 g / L, scouring agent E1310 0.5 g / L, stabilizer diethylamine pentaacetic acid 2 g / L;
[0054] (3) Low-temperature bleaching process: Accurately weigh a certain mass of fabric, immerse it in bleaching solution, bath ratio 1:8, 70℃, 55min, wash with water, and dry.
[0055] Comparative Example 3:
[0056] (1) 40S pure cotton knitted fabric (160g / m 2 );
[0057] (2) Bleaching prescription: 30% hydrogen peroxide 9 g / L, sodium hydroxide 2 g / L, penetrant JFC 0.5 g / L, scouring agent E1009 1.5 g / L, stabilizer diethylamine pentaacetic acid 1 g / L;
[0058] (3) Low-temperature bleaching process: Accurately weigh a certain mass of fabric, immerse it in bleaching solution, bath ratio 1:10, 70℃, 50min, wash with water, and dry.
[0059] Embodiment 4:
[0060] (1) T / C65 / 35, 150D / 21S polyester-cotton knitted fabric (145g / m 2 );
[0061] (2) Bleaching prescription: 30% hydrogen peroxide 14g / L, sodium hydroxide 1g / L, penetrant JFC 1g / L, scouring agent AEO-91g / L, stabilizer trisodium citrate 0.5g / L;
[0062] (3) Low-temperature bleaching process: Accurately weigh a certain mass of fabric, immerse it in bleaching solution, bath ratio 1:16, 70℃, 50min, wash with water, and dry.
[0063] Embodiment 5:
[0064] (1) T / C50 / 50, 130D / 40S polyester-cotton knitted fabric (160g / m 2 );
[0065] (2) Bleaching prescription: 30% hydrogen peroxide 12 g / L, sodium hydroxide 2 g / L, penetrant JFC 1 g / L, scouring agent E13051 g / L, stabilizer trisodium citrate 1 g / L;
[0066] (3) Low-temperature bleaching process: Accurately weigh a certain mass of fabric, immerse it in bleaching solution, bath ratio 1:20, 60℃, 70min, wash with water, and dry.
[0067] The fabrics bleached according to the above experimental examples and comparative examples were tested for fabric whiteness and bursting strength retention rate. The results are shown in Table 1.
[0068] Table 1 Performance indexes of bleached fabrics
[0069]
[0070] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0071] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for low temperature bleaching of cotton knitted fabrics, Features: The cotton knitted fabric is added into a bleaching solution, bleached at a certain bath ratio, and the bleached fabric is washed and dried, wherein the low-temperature bleaching solution comprises: hydrogen peroxide, a copper complex, an iron complex or a manganese complex of a catalyst (E)-3-(((1,3-dihydroxy-2-(hydroxymethyl)prop-2-yl)imino)methyl)-4-hydroxybenzenesulfonate sodium, sodium hydroxide, a penetrant, a scouring agent, and a stabilizer.
2. A method for low-temperature bleaching of cotton knitted fabric according to claim 1, Features: The cotton type knitted fabric is pure cotton knitted fabric or polyester-cotton blended knitted fabric.
3. A method for low-temperature bleaching of cotton knitted fabric according to claim 1, Features: The bath ratio is 1:8-1:
30.
4. A method for low-temperature bleaching of cotton knitted fabric according to claim 1, Features: The bleaching temperature is 60-85° C., and the bleaching time is 30-70 minutes.
5. A method for low temperature bleaching of cotton knitted fabric according to claim 1, Features: The bleaching solution comprises 30% (mass fraction) hydrogen peroxide 8-18 g / L, metal complex catalyst 6-80 μmol / L, sodium hydroxide 1-3 g / L, penetrant 0.5-2 g / L, scouring agent 0.5-3 g / L and stabilizer 0.5-2 g / L.
6. A method for low temperature bleaching of cotton knitted fabric according to claim 5, Features: The penetrant is JFC.
7. A method for low-temperature bleaching of cotton knitted fabric according to claim 5, Features: The scouring agent is one or a composite of E1009, E1305, E1310 and AEO-9.
8. A method for low temperature bleaching of cotton knitted fabric according to claim 5, Features: The stabilizer is one or a complex of several of sodium silicate, diethylamine pentaacetic acid and trisodium citrate.