High-flame-retardant waterborne polyurethane microfiber leather and preparation method thereof
Through the modification of melamine and the use of biomass materials, highly flame-retardant water-based polyurethane microfiber leather is prepared, which solves the problems of poor flame retardant effect and insufficient durability in the existing technology, and achieves excellent flame retardancy of polyurethane synthetic leather. performance and heat resistance, meeting high-level fire safety requirements.
Patent Information
- Application Number
- CN202411319679.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing flame-retardant polyurethane synthetic leather has poor flame-retardant effect and insufficient durability. The flame-retardant layer is easy to fall off during long-term use, resulting in low fire safety factor.
By modifying melamine and combining sodium alginate and lignin, a modified melamine formaldehyde resin is prepared to form a highly flame-retardant water-based polyurethane microfiber leather, which is coated on a base fabric and hot-pressed to form a durable flame-retardant coating.
The flame retardant and heat-resistant properties of polyurethane microfiber leather are significantly improved, meeting the flame retardant requirements of B1 level, extending the durability of the flame retardant effect, and ensuring the safety of the material in long-term use.
Smart Images

Figure CN118854697A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a highly flame-retardant waterborne polyurethane ultra-fine leather and a preparation method thereof. Background Art
[0002] Microfiber synthetic leather is a composite material with a three-dimensional microporous structure. It feels close to real leather and is usually made of microfiber needle-punched nonwoven fabric and water-based polyurethane as raw materials through an impregnation process. Water-based polyurethane is a polymer material with water as the medium. It is widely used in the field of synthetic leather because of its low odor, non-toxicity and non-polluting characteristics.
[0003] Waterborne polyurethane synthetic leather (WPU) is a type of microfiber synthetic leather, and is composed of waterborne polyurethane. Because of its appearance similar to natural leather, and its excellent gloss, feel, wear resistance, folding resistance, and aging resistance, it is widely used in the automotive, home furnishing, clothing, footwear, and luggage industries. However, its limiting oxygen index (LOI) is only about 18%, which is very easy to burn, and the combustion releases a large amount of heat, smoke, and toxic gases, which seriously threatens human health and safety, which limits the application of polyurethane synthetic leather. Therefore, improving the flame retardant properties of polyurethane synthetic leather, reducing the surface combustion rate of the material, promoting self-extinguishing of combustion, and preventing the fire from further expanding is one of the research directions of WPU functionalization, which can not only meet the market demand for functional synthetic leather products, but also provide certain guarantees for the safety of personnel.
[0004] At present, there are two main ways to prepare flame-retardant polyurethane synthetic leather. One is to coat the surface of synthetic leather with a flame-retardant layer, and the other is to add flame-retardant materials to the surface layer of synthetic leather. The presence of flame-retardant materials prevents the flame from spreading to the base fabric, preventing the synthetic leather from burning. However, once the base fabric begins to burn, the synthetic leather will no longer have flame-retardant properties, which may cause irreparable losses to the user. In addition, the flame-retardant layer coated on the surface of the synthetic leather and the flame retardant in the surface layer will slowly fall off during long-term use, the effect will decay, the flame-retardant effect will disappear, and the fire safety factor will be low. Therefore, the research and development of a highly flame-retardant water-based polyurethane microfiber leather has important social and economic significance. Summary of the invention
[0005] In view of this, the present invention provides a highly flame-retardant water-based polyurethane microfiber leather and a preparation method thereof, the purpose of which is to solve the technical problems of poor flame retardant effect and poor flame retardant durability of existing flame retardant polyurethane synthetic leather.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions: The present invention provides a method for preparing a highly flame-retardant waterborne polyurethane ultra-fine leather, comprising the following steps: S1, mixing melamine, paraformaldehyde and a modifier and reacting them to obtain a modified melamine formaldehyde resin; S2, mixing the modified melamine formaldehyde resin, diol, diisocyanate, crosslinking agent and catalyst and reacting them to obtain an intermediate; S3, mixing the intermediate and the chain extender and reacting them to obtain a prepolymer; S4, mixing the prepolymer, polyamine, water and ethylenediamine and reacting them to obtain a modified melamine formaldehyde resin-based polyurethane emulsion; S5. Apply the modified melamine formaldehyde resin-based polyurethane emulsion on the substrate and pre-bake to form a coating, and then hot-press the coating and the base fabric and sequentially perform aging, cooling, peeling, and winding to obtain a highly flame-retardant water-based polyurethane microfiber leather.
[0007] Furthermore, in the step S1, the mass ratio of melamine, paraformaldehyde and modifier is 1-2:3-8:3-6; the reaction temperature is 50-80°C, and the reaction time is 30-60 min.
[0008] Furthermore, in step S2, the mass ratio of the modified melamine formaldehyde resin, the diol, the diisocyanate and the cross-linking agent is 10-20:30-70:30-70:1-10; the amount of the catalyst is 3-5% of the total mass of the modified melamine formaldehyde resin, the diol, the diisocyanate and the cross-linking agent; the reaction temperature is 65-80°C, and the reaction time is 90-150 min.
[0009] Furthermore, in step S3, the mass ratio of the intermediate to the chain extender is 20-80:4-20; the reaction temperature is 65-80° C., and the reaction time is 60-180 min.
[0010] Furthermore, in step S4, the mass ratio of polyamine, water and ethylenediamine is 2-4:25-45:1-3; the reaction temperature is 40-50° C., and the reaction time is 60-120 min.
[0011] Furthermore, the mass ratio of the chain extender in step S3 to the polyamine in step S4 is 4-20:2-4.
[0012] Furthermore, in step S5, the pre-baking temperature is 80-120°C, and the pre-baking time is 3-8 minutes; the hot pressing bonding temperature is 80-140°C, and the hot pressing bonding time is 90-180 seconds; the aging temperature is 120-140°C, and the aging time is 8-10 minutes.
[0013] Furthermore, in step S5, the substrate includes release paper; the base fabric includes ultrafine fiber needle-punched nonwoven fabric, ultrafine fiber spunlace nonwoven fabric or melt-blown nonwoven fabric; and the thickness of the coating is 0.5-1.0 mm.
[0014] Further, the modifier includes one or more of glycerol, sodium alginate and lignin; The diol includes one or more of polyester diol, polycarbonate diol and polyether diol; The diisocyanate includes one or more of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, 1,6-hexamethylene diisocyanate, xylylene diisocyanate and naphthalene-1,5-diisocyanate; The cross-linking agent includes dimethylol propionic acid; The catalyst includes one or more of inorganic metal chloride, dibutyltin laurate, dibutyltin diacetate and stannous octoate; The chain extender includes one or more of 2, 2, 3, 3, 4, 4-hexafluoro-1, 5-pentanediol, ethylene glycol, diethylene glycol, 1, 4-butanediol, 2, 3-butanediol, 1, 6-hexanediol, neopentyl glycol, diethylene glycol, glycerol, sorbitol, trimethylolpropane, dimethylolcyclohexane, pentaerythritol diacrylate, dipentaerythritol tetraacrylate, trimethylolpropane monoacrylate and dimethylolpropionic acid; The polyamine includes one or more of diethylenetriamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine and isophoronediamine.
[0015] The present invention also provides a highly flame-retardant waterborne polyurethane ultra-fine leather prepared by the method for preparing the highly flame-retardant waterborne polyurethane ultra-fine leather.
[0016] It can be seen from the above technical solution that compared with the prior art, the beneficial effects of the present invention are as follows: Melamine flame retardants are mostly added to polymers by physical blending. During use, the flame retardant elements are prone to migration, and the flame retardant effect gradually decays. The present invention first modifies melamine to make up for the defects of melamine formaldehyde resin, such as easy cross-linking and curing, high hardness, and high brittleness. In addition, melamine is modified with sodium alginate and lignin, realizing the high-value utilization of biomass resources, which is safe and environmentally friendly.
[0017] The modified melamine formaldehyde resin prepared by the present invention has good compatibility with waterborne polyurethane, and the emulsion prepared by the modified melamine formaldehyde resin has stable performance. The addition of modified melamine improves the flame retardant performance, heat resistance and durability of the emulsion, and has good market prospects. The emulsion is coated on a base fabric to form a polyurethane microfiber leather with excellent flame retardant performance, heat resistance and durability. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a burning state diagram of the highly flame-retardant waterborne polyurethane microfiber leather prepared in Example 1 when exposed to flame;
[0019] Figure 2 This is a diagram showing the burning state of the waterborne polyurethane microfiber leather prepared in the comparative example when it comes into contact with flame. DETAILED DESCRIPTION
[0020] The present invention provides a method for preparing a highly flame-retardant waterborne polyurethane ultra-fine leather, comprising the following steps: S1, mixing melamine, paraformaldehyde and a modifier and reacting them to obtain a modified melamine formaldehyde resin; S2, mixing the modified melamine formaldehyde resin, diol, diisocyanate, crosslinking agent and catalyst and reacting them to obtain an intermediate; S3, mixing the intermediate and the chain extender and reacting them to obtain a prepolymer; S4, mixing the prepolymer, polyamine, water and ethylenediamine and reacting them to obtain a modified melamine formaldehyde resin-based polyurethane emulsion; S5. Apply the modified melamine formaldehyde resin-based polyurethane emulsion on the substrate and pre-bake to form a coating, and then hot-press the coating and the base fabric and sequentially perform aging, cooling, peeling, and winding to obtain a highly flame-retardant water-based polyurethane microfiber leather.
[0021] In the present invention, in the step S1, the mass ratio of melamine, paraformaldehyde and modifier is 1-2:3-8:3-6, preferably 1:4-7:4-5, and more preferably 1:5-6:4; the reaction temperature is 50-80°C, preferably 60-70°C, and more preferably 65°C; the reaction time is 30-60min, preferably 40-50min, and more preferably 45min.
[0022] In the present invention, in step S2, the mass ratio of modified melamine formaldehyde resin, diol, diisocyanate and crosslinking agent is 10-20:30-70:30-70:1-10, preferably 12-18:40-60:40-60:2-8, and more preferably 14-16:50-55:50-55:4-6; the amount of catalyst is 3-5% of the total mass of modified melamine formaldehyde resin, diol, diisocyanate and crosslinking agent, and more preferably 4%; the reaction temperature is 65-80°C, and more preferably 70-75°C; the reaction time is 90-150min, and more preferably 100-140min, and more preferably 110-120min.
[0023] In the present invention, in step S3, the mass ratio of the intermediate to the chain extender is 20-80:4-20, preferably 30-70:8-16, and more preferably 40-60:10-15; the reaction temperature is 65-80°C, preferably 70-75°C; the reaction time is 60-180 min, preferably 80-150 min, and more preferably 100-120 min.
[0024] In the present invention, in step S4, the mass ratio of polyamine, water and ethylenediamine is 2-4:25-45:1-3, preferably 3:30-40:2, and more preferably 3:30:2; the reaction temperature is 40-50°C, preferably 42-48°C, and more preferably 44-46°C; the reaction time is 60-120 min, preferably 70-110 min, and more preferably 80-100 min.
[0025] In the present invention, the mass ratio of the chain extender in step S3 to the polyamine in step S4 is 4-20:2-4, preferably 8-16:3, and more preferably 10-15:3.
[0026] In the present invention, in the step S5, the pre-baking temperature is 80-120°C, preferably 90-110°C, and more preferably 100°C; the pre-baking time is 3-8 min, preferably 4-7 min, and more preferably 5-6 min; the hot pressing bonding temperature is 80-140°C, preferably 90-130°C, and more preferably 100-120°C; the hot pressing bonding time is 90-180s, preferably 100-160s, and more preferably 120-140s; the aging temperature is 120-140°C, preferably 125-135°C, and more preferably 130°C; the aging time is 8-10min, and preferably 9min.
[0027] In the present invention, in step S5, the substrate includes release paper, and the release paper is preferably flat paper or embossed paper; the base fabric includes ultrafine fiber needle-punched non-woven fabric, ultrafine fiber spunlace non-woven fabric or melt-blown non-woven fabric; the thickness of the coating is 0.5~1.0mm, preferably 0.6~0.9mm, and more preferably 0.7~0.8mm.
[0028] In the present invention, in step S5, coating is preferably performed by scraping.
[0029] In the present invention, the modifier includes one or more of glycerol, sodium alginate and lignin; The diol includes one or more of polyester diol, polycarbonate diol and polyether diol; the polyester diol includes one or more of polycaprolactone diol, polybutylene succinate diol, polyhexamethylene glycol butylene glycol ester diol, polyethylene terephthalate diol and polybutylene terephthalate diol, preferably polycaprolactone diol; the number average molecular weight of the polyester diol is 1500-2500 g / mol, preferably 1800-2200 g / mol; The polycarbonate diol comprises one or more of polycarbonate butanediol, polycarbonate hexanediol, polycarbonate decanediol and polycarbonate cyclohexanedimethanol diol, preferably polycarbonate butanediol; the number average molecular weight of the polycarbonate diol is 1500-2500 g / mol, preferably 1800-2200 g / mol; The polyether diol comprises one or more of polytetrahydrofuran diol, polyethylene glycol diol and polypropylene glycol diol, preferably polytetrahydrofuran diol; the number average molecular weight of the polyether diol is 1500-2500 g / mol, preferably 1800-2200 g / mol.
[0030] The diisocyanate includes one or more of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, 1,6-hexamethylene diisocyanate, xylylene diisocyanate and naphthalene-1,5-diisocyanate; The cross-linking agent includes dimethylol propionic acid; The catalyst includes one or more of an inorganic metal chloride, dibutyltin laurate, dibutyltin diacetate and stannous octoate; the inorganic metal chloride is preferably one or more of zinc chloride, tin tetrachloride, stannous chloride and germanium chloride; The chain extender includes one or more of 2, 2, 3, 3, 4, 4-hexafluoro-1, 5-pentanediol, ethylene glycol, diethylene glycol, 1, 4-butanediol, 2, 3-butanediol, 1, 6-hexanediol, neopentyl glycol, diethylene glycol, glycerol, sorbitol, trimethylolpropane, dimethylolcyclohexane, pentaerythritol diacrylate, dipentaerythritol tetraacrylate, trimethylolpropane monoacrylate and dimethylolpropionic acid; The polyamine includes one or more of diethylenetriamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine and isophoronediamine.
[0031] The present invention also provides a highly flame-retardant waterborne polyurethane ultra-fine leather prepared by the method for preparing the highly flame-retardant waterborne polyurethane ultra-fine leather.
[0032] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0033] Example 1 In parts by weight, under the protection of N2, 20 parts of melamine, 80 parts of paraformaldehyde and 60 parts of propylene glycol are placed in a four-necked flask, the temperature is raised to 60°C, the reaction is carried out for 30 minutes, and the modified melamine formaldehyde resin is obtained by cooling.
[0034] 10 parts of modified melamine formaldehyde resin, 30 parts of polycaprolactone diol (number average molecular weight 2500g / mol), 30 parts of isophorone diisocyanate, 1 part of cross-linking agent dimethylol propionic acid, 3% of the total mass of zinc chloride are added dropwise, and the reaction is carried out at 65°C for 120 minutes to obtain an intermediate, and then 4 parts of chain extender ethylene glycol are added and the reaction is continued for 120 minutes to obtain a prepolymer; the temperature is lowered to 45°C, 2 parts of triethylamine are added, and 25 parts of water and 1 part of ethylenediamine are added under stirring and reacted for 120 minutes to obtain a modified melamine formaldehyde resin-based waterborne polyurethane emulsion.
[0035] The modified melamine formaldehyde resin-based water-based polyurethane emulsion is scraped onto the surface of the flat paper and pre-baked at 100°C for 5 minutes to obtain a coating; then it is laminated with a microfiber needle-punched non-woven fabric base at 100°C for 90 seconds; finally, it is aged at 120°C for 8 minutes, cooled to room temperature, and then peeled and rolled to obtain a highly flame-retardant water-based polyurethane microfiber leather.
[0036] Example 2 The same as Example 1, except that the amount of paraformaldehyde used is 70 parts.
[0037] Example 3 The same as Example 1, except that the amount of paraformaldehyde used is 60 parts.
[0038] Example 4 The same as Example 1, except that the amount of modified melamine formaldehyde resin used is 15 parts.
[0039] Example 5 The same as Example 1, except that the amount of modified melamine formaldehyde resin used is 20 parts.
[0040] Example 6 The same as Example 1, except that sodium alginate is used to replace glycerol.
[0041] Example 7 The same as Example 1, except that lignin is used to replace glycerol.
[0042] Comparative Example In parts by weight, under N2 protection, 30 parts of polycaprolactone diol (number average molecular weight 2500g / mol), 30 parts of isophorone diisocyanate, 1 part of cross-linking agent dimethylolpropionic acid, 3% of the total mass of zinc chloride are added dropwise, and the reaction is carried out at 65°C for 120 minutes to obtain an intermediate, and then 4 parts of chain extender ethylene glycol are added and the reaction is continued for 120 minutes to obtain a prepolymer; the temperature is lowered to 45°C, 2 parts of triethylamine are added, and 25 parts of water and 1 part of ethylenediamine are added under stirring and reacted for 120 minutes to obtain a formaldehyde resin-based waterborne polyurethane emulsion.
[0043] The formaldehyde resin-based water-based polyurethane emulsion is scraped onto the surface of the flat paper and pre-baked at 100°C for 5 minutes to obtain a coating; then it is laminated with a microfiber needle-punched non-woven fabric base at 100°C for 90 seconds; finally, it is aged at 120°C for 8 minutes, cooled to room temperature, and then peeled and rolled to obtain the water-based polyurethane microfiber leather.
[0044] Performance Testing The flame retardant properties of the waterborne polyurethane microfiber leathers prepared in Examples 1 to 7 and the comparative examples were tested, and the test results are shown in Table 1. The flame retardant test standards refer to GB / T 5455-1997 "Vertical method for testing the burning performance of textiles" and GB / T 5454-1997 "Oxygen index method for testing the burning performance of textiles". In order to test the stability of the flame retardant properties of the microfiber leathers prepared in Examples 1 to 7 and the comparative examples, they were exposed to simulated sunlight for a period of time, and the LOI value of the microfiber leather was tested in combination with GB / T 5455-1997 and GB / T5454-1997, and the results are shown in Table 1.
[0045] Table 1 Performance test results of waterborne polyurethane microfiber leather project Flame retardant grade LOI value (%) Light 48h Light 12h Example 1 B1 29.3 29.0 28.5 Example 2 B1 30.2 29.8 29.5 Example 3 B1 27.4 27 27.1 Example 4 B1 29.5 29 28.5 Example 5 B1 29.8 29.4 29.4 Example 6 B1 28.5 28.5 28.5 Example 7 B1 27 26.5 26 Comparative Example B2 17 17 16
[0046] Figure 1 This is a burning state diagram of the highly flame-retardant waterborne polyurethane microfiber leather prepared in Example 1 when exposed to flame; Figure 2 The figure is a combustion state diagram of the waterborne polyurethane microfiber leather prepared in the comparative example when it is exposed to flame. Figure 1 , Figure 2 Combined with Table 1, it can be seen that the water-based polyurethane ultra-fine leather prepared by adding modified melamine formaldehyde resin flame retardant can meet the flame retardant B1 grade requirement, and the melamine modified with biomass materials sodium alginate and lignin can also give the polyurethane ultra-fine leather excellent flame retardant properties, so that the highly flame retardant water-based polyurethane ultra-fine leather prepared by the present invention can be applied to products with flame retardant requirements.
[0047] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing highly flame-retardant waterborne polyurethane microfiber leather, characterized in that: The following steps are involved: S1, mixing melamine, paraformaldehyde and a modifier and reacting them to obtain a modified melamine formaldehyde resin; S2, mixing the modified melamine formaldehyde resin, diol, diisocyanate, crosslinking agent and catalyst and reacting them to obtain an intermediate; S3, mixing the intermediate and the chain extender and reacting them to obtain a prepolymer; S4, mixing the prepolymer, polyamine, water and ethylenediamine and reacting them to obtain a modified melamine formaldehyde resin-based polyurethane emulsion; S5. Apply the modified melamine formaldehyde resin-based polyurethane emulsion on the substrate and pre-bake to form a coating, and then hot-press the coating and the base fabric and sequentially perform aging, cooling, peeling, and winding to obtain a highly flame-retardant water-based polyurethane microfiber leather.
2. The method for preparing highly flame-retardant waterborne polyurethane microfiber leather according to claim 1, characterized in that: In the step S1, the mass ratio of melamine, paraformaldehyde and modifier is 1-2:3-8:3-6; the reaction temperature is 50-80° C., and the reaction time is 30-60 min.
3. The method for preparing highly flame-retardant waterborne polyurethane microfiber leather according to claim 1, characterized in that: In the step S2, the mass ratio of the modified melamine formaldehyde resin, the diol, the diisocyanate and the cross-linking agent is 10-20:30-70:30-70:1-10; the amount of the catalyst is 3-5% of the total mass of the modified melamine formaldehyde resin, the diol, the diisocyanate and the cross-linking agent; the reaction temperature is 65-80° C., and the reaction time is 90-150 min.
4. The method for preparing the highly flame-retardant waterborne polyurethane microfiber leather according to claim 2 or 3, characterized in that: In the step S3, the mass ratio of the intermediate to the chain extender is 20-80:4-20; the reaction temperature is 65-80° C., and the reaction time is 60-180 min.
5. The method for preparing highly flame-retardant waterborne polyurethane microfiber leather according to claim 4, characterized in that: In step S4, the mass ratio of polyamine, water and ethylenediamine is 2-4:25-45:1-3; the reaction temperature is 40-50° C., and the reaction time is 60-120 min.
6. The method for preparing highly flame-retardant waterborne polyurethane microfiber leather according to claim 5, characterized in that: The mass ratio of the chain extender in step S3 to the polyamine in step S4 is 4-20:2-4.
7. The method for preparing the highly flame-retardant waterborne polyurethane microfiber leather according to claim 2, 3 or 6, characterized in that: In the step S5, the pre-baking temperature is 80-120° C., and the pre-baking time is 3-8 min; the hot pressing bonding temperature is 80-140° C., and the hot pressing bonding time is 90-180 s; the aging temperature is 120-140° C., and the aging time is 8-10 min.
8. The method for preparing highly flame-retardant waterborne polyurethane microfiber leather according to claim 7, characterized in that: In the step S5, the substrate includes release paper; the base fabric includes ultrafine fiber needle-punched nonwoven fabric, ultrafine fiber spunlace nonwoven fabric or melt-blown nonwoven fabric; and the thickness of the coating is 0.5-1.0 mm.
9. The method for preparing the highly flame-retardant waterborne polyurethane microfiber leather according to claim 5 or 8, characterized in that: The modifier includes one or more of glycerol, sodium alginate and lignin; The diol includes one or more of polyester diol, polycarbonate diol and polyether diol; The diisocyanate includes one or more of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, 1,6-hexamethylene diisocyanate, xylylene diisocyanate and naphthalene-1,5-diisocyanate; The cross-linking agent includes dimethylol propionic acid; The catalyst includes one or more of inorganic metal chloride, dibutyltin laurate, dibutyltin diacetate and stannous octoate; The chain extender includes one or more of 2, 2, 3, 3, 4, 4-hexafluoro-1, 5-pentanediol, ethylene glycol, diethylene glycol, 1, 4-butanediol, 2, 3-butanediol, 1, 6-hexanediol, neopentyl glycol, diethylene glycol, glycerol, sorbitol, trimethylolpropane, dimethylolcyclohexane, pentaerythritol diacrylate, dipentaerythritol tetraacrylate, trimethylolpropane monoacrylate and dimethylolpropionic acid; The polyamine includes one or more of diethylenetriamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine and isophoronediamine.
10. Highly flame retardant waterborne polyurethane ultra-fine leather prepared by the method for preparing highly flame retardant waterborne polyurethane ultra-fine leather according to any one of claims 1 to 9.
Citation Information
Patent Citations
Fire-retardant hydrolysis-resistance solvent-free polyurethane synthetic leather resin and preparation method and application thereof
CN106008892A
Melamine derivative modified waterborne polyurethane flame-retardant anti-microbial resin and preparation method thereof
CN109517130A
Lignin-based intumescent flame retardant modified polyurethane elastomer containing nitrogen and phosphorus and preparation method of elastomer
CN112724361A
Lignin-based polyurethane film and preparation method thereof
CN112724430A
Water-based environment-friendly high-flame-retardant solvent-free embossed grain-absorbed synthetic leather and preparation method thereof
CN114379175A
Cited By
Waterborne polyurethane-based flame-retardant microfiber synthetic leather and preparation method thereof
CN119571637A