Acceleration test data driven initial value calculation method for double-index nested model
The initial value calculation method of the double-exponential nested model driven by accelerated test data solves the problem of difficulty in determining the initial value of the double-exponential aging kinetic model in the aging performance evaluation of polymer materials, achieves efficient and accurate aging performance prediction, and reduces The technical threshold has been reached.
Patent Information
- Application Number
- CN202410980679.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-22
AI Technical Summary
In the evaluation of the aging performance of polymer materials, existing nonlinear regression analysis methods are difficult to accurately determine the initial value of the double-exponential aging kinetic model, resulting in low prediction accuracy and easily causing the fitting process to iteratively oscillate or converge to local extreme values.
The initial value calculation method of the double exponential nested model driven by accelerated test data is used to simplify the aging kinetic function by specifying the size relationship of the power exponent and the linear regression method, calculate the initial values of macro parameters and micro parameters, and use linear regression fitting to Quickly determine the initial value of the model.
It improves the accuracy and efficiency of polymer material aging performance assessment, avoids non-linear regression non-convergence problems caused by inappropriate initial values, lowers the technical threshold and simplifies the data processing process.
Smart Images

Figure SMS_1 
Figure SMS_18 
Figure SMS_20
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of accelerated degradation test material performance evaluation, and in particular to an accelerated test data-driven double exponential nested model initial value calculation method. Background Art
[0002] With the rapid development of modern industry, polymer materials are increasingly used in the industrial field, but the aging problem of polymer materials has become the biggest limitation in their application. During the storage and use of polymer materials, due to the influence of various factors, such as light, oxygen, ozone, moisture, oil and other working media and temperature, stress, strain, etc., the internal molecular structure of the material undergoes chemical changes such as cross-linking and degradation, and various performance indicators gradually degrade, and the service life is gradually exhausted. In order to ensure the stability of polymer material storage and the reliability of long-term use, the accurate evaluation of the aging performance and service life of polymer materials has become an important research topic. For example, a variety of prediction methods have been formed for the life evaluation of rubber materials, and standards such as HG3087, GB / T20028, and GB / T27800 have also been formulated. The existing polymer material performance prediction algorithms are mostly based on linear regression analysis, and the prediction effect is poor; the nonlinear regression analysis prediction algorithm relies heavily on the initial value of the parameter. Inappropriate initial values are likely to cause iterative oscillations in the fitting process, which is difficult to converge, or converge to local extreme values, and the prediction accuracy is low. Zhu Minren's "Circular Search Method for Determining the Initial Values of Double Exponential Curve Parameters" in "Mathematics in Practice and Understanding" 2003-12.Vol.33.No.12 proposed a circular search method for determining the initial values of parameters by making full use of observed values when fitting double exponential curves with the Gauss-Newton method in the sense of least squares. Although this method can predict the initial values of the regression parameters of the double exponential function, there is no relevant research on the calculation method of the initial values of nonlinear regression fitting parameters for nested functions containing other parameters in the undetermined parameters. Summary of the invention
[0003] The technical problem solved by the present invention is to provide an initial value calculation method for a double exponential nested model driven by accelerated test data, so as to solve the problem that in the process of accelerating degradation test to evaluate material performance, the initial value of the double exponential aging kinetic model with micro-parameters embedded in the regression parameters is difficult to determine in the nonlinear regression analysis.
[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions: according to the accelerated thermal aging test data, the double exponential nested model is used as a function to describe the aging characteristics of the material, and its fitting parameters include macro parameters and micro parameters, and the micro parameters are embedded in the thermal aging kinetic function as the implementation form of the macro parameters. The size relationship between the two power exponents is specified, and according to the characteristics of the double exponential function, the material thermal aging kinetic function is simplified according to the aging time; the accelerated test data is pre-split, and the material performance data is formally split according to the residual value of the material performance; the two simplified aging kinetic functions are linearized, and the initial values of the macro parameters and micro parameters are calculated using the linear regression method, so as to achieve the purpose of the present invention.
[0005] The present invention relates to a method for calculating initial values of a double exponential nested model driven by accelerated test data, which is characterized by the following steps: 1) For polymer materials whose thermal aging reaction kinetics satisfy the Arrhenius equation, based on the thermal properties of the materials, select no less than three test temperatures within the range below the glass transition temperature of the materials to conduct accelerated thermal aging tests on the materials; group the test data according to the accelerated test temperature to obtain no less than three groups of test data ( t i , P i ), the number of groups is consistent with the number of test temperatures; 2) Take the natural logarithm of each set of material performance test value data, perform linear regression fitting, and obtain the slope of the fitting equation of the material performance logarithm value to the aging time at all accelerated test temperatures. Take the average value of the slope to obtain k0; if k0 < 0, then let the material performance characterization value y i = P i ; If k0>0, let the material performance characterization value y i =1- P i ; 3) According to the following formula, the accelerated thermal aging test temperature T i Perform conversion and calculate the conversion temperature value suitable for the accelerated thermal aging kinetic function;
[0006] 4) According to the thermal aging reaction mechanism of the material, the double exponential nested model shown below is used as a function to describe the thermal aging kinetic characteristics of the material; y i =(1-e)×exp(-b i × t i )+e×exp(-di × t i ) Where e and b i d i is the regression macro parameter; the e value is the weight coefficient of the two reactions before and after, 0<e<1; 5) Nested parameter b in thermal aging kinetic function i d i The following formula is used to describe: b i =b0×[exp(-bE1×X i )] d i =d0×[exp(-dE1×X i )] Where b0, bE1, d0, dE1 are the material activation energy micro parameters; b i >0,d i >0; 6) Let 0<b i <d i , the critical test is determined based on the number of tests; when the aging time is greater than or equal to the aging time corresponding to the critical test, the material thermal aging kinetic function is approximately: y i =(1-e)×exp(-b i × t i ); When the aging time is less than the corresponding aging time of the critical test, the material thermal aging kinetic function is approximately y i =(1-e)+e×exp(-d i × t i ); 7) Based on the determined critical test, the material performance characterization data at each accelerated test temperature is pre-split, and only the corresponding data points of the critical test and after are taken to obtain the material aging performance data at each accelerated test temperature after the split ( th i , yh i ); 8) Taking the material aging performance data after splitting, the material thermal aging kinetic function is simplified to y i =(1-e)×exp(-b i × t i ); Taking the natural logarithm of both sides of the function model equation, we get the following linear model; ln( y i)=ln(1-e)-b i × t i Material aging performance data ( th i , yh i ) is substituted into the above formula, and the model is fitted with linear regression to obtain the slope, intercept and goodness of fit of the regression line; 9) Based on the intercept of the regression line, calculate the estimated value e0 of the parameter e i ; Calculate the residual value y i -(1-e0 i ), y i -(1-e0 i )>0 is divided into data ( td i , yd i ), the remaining data points are divided into data ( tb i , yb i ) to complete the formal splitting of material aging performance data at each test temperature; 10) Obtain material aging performance data at each accelerated test temperature ( tb i , yb i ), and substitute it into ln( y i )=ln(1-e)-b i × t i , perform linear regression fitting on the model, obtain the slope, intercept and goodness of fit of the regression line, and calculate the estimated value of parameter e at the test temperature of the i-th group , parameter b i Estimated value of ; 11) Obtain material aging performance data at each accelerated test temperature ( td i , yd i ), substituting the estimated value of parameter e at each set of test temperatures , the material thermal aging kinetic function is simplified to y i -(1- )= ×exp(-d i × t i); Taking the natural logarithm of both sides of the function model equation, we get the following linear model; ln( y i -(1- ))=ln( )-d i × t i Material aging performance data ( td i , yd i ) is substituted into the above formula, and the model is fitted with linear regression to obtain the slope, intercept and goodness of fit of the regression line, and the parameter d at the test temperature of the i-th group is calculated. i Estimated value of ; 12) Estimated values of parameter e Take the arithmetic mean to get the initial value of parameter e ; b i =b0×[exp(-bE1×X i )], converted into a linear equation ln(b0)-X i ×bE1=ln(b i ),Will , X i Substitute the value into the linear equation system and solve it to get the initial value of the parameter b , ; D i =d0×[exp(-dE1×X i )], converted into a linear equation ln(d0)-X i ×dE1=ln(d i ),Will , X i Substitute the value into the linear equation system and solve it to get the initial value of the parameter d , ; So far, the initial values of all regression parameters of the double exponential nested model of thermal aging kinetics have been quickly calculated.
[0007] Preferably, in the step 2), the linear fitting of the material property test logarithm to the aging time only distinguishes the increasing and decreasing relationship between the material property test value and the aging time, and uniformly sets the material property characterization value to decrease with the aging time.
[0008] Preferably, in step 6), the test corresponding to half of the test number at each accelerated test temperature is taken as the critical test. If half of the test number is a decimal, it is rounded up to be the critical test.
[0009] Preferably, in step 6), the order of the two reactions is not distinguished in the thermal aging kinetic function fitting, b i d i Can be interchanged.
[0010] Preferably, in the step 7), in the accelerated thermal aging test of materials, at each test temperature, the number of test time test points should not be less than 10, and the number of data points selected by data pre-splitting should not be less than 6.
[0011] Preferably, in step 9), when the aging time t i When the aging time is less than the critical test corresponding aging time, the material thermal aging kinetic function is approximately: y i =(1-e)+e×exp(-d i × t i ), e×exp(-d i × t i ) is always a positive number, that is y i -(1-e) is always a positive number, so take y i The time interval in which -(1-e)>0 holds is approximately t i The parameter d is calculated in the time interval less than the aging time corresponding to the critical test. i The solution.
[0012] Preferably, in steps 8), 10) and 11), when performing linear regression fitting, the goodness of fit value needs to be greater than 0.8.
[0013] Preferably, in step 12), solving b i d i The linear equations of micro-parameters are overdetermined, and the solution is the least squares solution of the equations.
[0014] The invention relates to an accelerated test data-driven double exponential nested model initial value calculation method. According to the accelerated thermal aging test data, the double exponential nested model is used as a function to describe the material aging characteristics. The fitting parameters include macro parameters and micro parameters. The micro parameters are nested into the thermal aging kinetic function as the implementation form of the macro parameters. The size relationship of the two power exponents is specified. According to the characteristics of the double exponential function, the material thermal aging kinetic function is simplified according to the size of the aging time; the accelerated test data is pre-split, and the material performance data is formally split according to the residual value of the material performance; the simplified two aging kinetic functions are linearized, and the initial values of the macro parameters and micro parameters are calculated using a linear regression method. The initial values of the regression parameters are input into the fitting software of the nonlinear regression analysis method, and the precise values of the thermal aging kinetic model parameters can be obtained quickly and accurately. The method can help non-statistical researchers quickly select the initial values of the regression parameters of the double exponential nested model, avoid problems such as nonlinear regression non-convergence and deviation from the true value caused by inappropriate initial values of the parameters, reduce the technical threshold value of accelerated degradation test evaluation of material performance, and improve the efficiency of scientific research work. The method of the invention has clear logic, simple calculation steps, strong versatility, and is easy to implement with programming software, and does not make special requirements on the data processing software used. DETAILED DESCRIPTION
[0015] In order to make the implementation purpose, technical methods and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be described in more detail below in combination with the embodiments of the present invention. The described embodiments are part of the embodiments of the present invention, rather than all the embodiments. The embodiments described below by reference are exemplary and are intended to be used to explain the present invention, and should not be understood as limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. The embodiments of the present invention are described in detail below.
[0016] In the following examples, the subscript i represents any accelerated test temperature.
[0017] Example 1 In this embodiment, accelerated thermal aging tests are performed on ethylene propylene rubber EPDM at accelerated test temperatures of 90°C, 80°C and 70°C, respectively. The test data are grouped according to the accelerated test temperatures, and the data in each group are arranged in ascending order according to the test time. The thermal aging performance test data of the EPDM rubber material are obtained as shown in Table 1 below.
[0018] Table 1 Test data of thermal aging performance of EPDM ethylene propylene rubber at different accelerated test temperatures
[0019] The natural logarithm of each set of material performance test value data is taken as the dependent variable, and the corresponding aging time is taken as the independent variable. Linear regression fitting is performed to obtain the slope of the fitting equation of the material performance test logarithm value at all temperatures to the aging time. The average of all slopes is taken to obtain k0=5.9072E-04, the material performance characterization value y i =1- P i .
[0020] The accelerated thermal aging test temperature T i Substituting into the following formula (1), we can obtain the conversion temperature value X suitable for the accelerated thermal aging kinetic function: i Through the above conversion, the rubber material performance characterization data is obtained as shown in Table 2 below.
[0021]
[0022] Table 2 Characterization data of thermal aging performance of EPDM ethylene propylene rubber at different accelerated test temperatures
[0023] According to the thermal aging reaction mechanism of rubber materials, the double exponential nested model shown in formula (2) is used as a function to describe the aging kinetic characteristics of the material.
[0024]
[0025] In formula (2), e and b i d i is the regression macro parameter. The value of e is the weight coefficient of the two reactions before and after, 0<e<1; Nested parameter b in the thermal aging kinetic function i d i It is described by formula (3).
[0026]
[0027] In formula (3), b0, bE1, d0, and dE1 are the material activation energy micro parameters; b i >0,d i >0.
[0028] Let 0<b i <d i , take the test corresponding to half of the test times at each accelerated test temperature as the critical test. If half of the test times is a decimal, round it up to the integer as the critical test; when the aging time is greater than or equal to the aging time corresponding to the critical test, the material thermal aging kinetic function is approximately:
[0029] When the aging time is less than the aging time corresponding to the critical test, the material thermal aging kinetic function is approximately:
[0030] The order of the two reactions is not distinguished in the thermal aging kinetic function fitting. i d i They can be interchanged. Let 0<b i <d i , calculate the parameter b i When the initial value is used, the thermal aging kinetic function omits e×exp(-d i × t i ), parameter b i The solution is too small; calculate the parameter d i When the initial value is reached, the thermal aging kinetic function will be exp(-b i × t i ) is approximately 1, and the parameter d i The solution is too large, so when calculating 0<b i <d i Always remain established.
[0031] Based on the determined critical tests, the material performance characterization values at each accelerated test temperature y i Perform pre-splitting and only take the data points corresponding to the critical test and after it to obtain the split data ( th i , yh i ), as shown in Table 3 below.
[0032] Table 3 Pre-split data of thermal aging performance characterization of EPDM ethylene propylene rubber at different accelerated test temperatures
[0033] Taking the natural logarithm of both sides of the function model (4) equation, we obtain the following linear model, as shown in formula (6).
[0034]
[0035] The data ( th i , yh i ) is substituted into formula (6), and the model is fitted with linear regression to obtain the slope of the regression line kh i , intercept wh i And goodness of fit Rh i .
[0036] wh i=ln(1-e), and the parameter estimation value e0 at the i-th group test temperature is calculated using formula (6): i ; Substitute e0 i , calculate the residual value y i -(1-e0 i ). By calculation, the linear regression line intercept wh 90 =-0.3178,wh 80 =-0.2523,wh 70 =-0.3104; goodness of fit Rh 90 =0.9423, Rh 80 =0.9487, Rh 70 =0.9637, the goodness of fit values are all greater than 0.8; the parameter estimate value e0 90 =0.2723,e0 80 =0.2230,e0 70 =0.2668, and the performance characterization residual data at each test temperature are shown in Table 4 below.
[0037] Table 4 Residual data of thermal aging performance characterization of EPDM ethylene propylene rubber at different test temperatures
[0038] When the aging time t i When it is less than the critical value, the material thermal aging kinetic function is approximately as follows: y i =(1-e)+e×exp(-d i × t i ), e×exp(-d i × t i ) is always a positive number, that is y i -(1-e) is always a positive number, so take y i The time interval in which -(1-e)>0 holds is approximately t i The parameter d is smaller than the interval of aging time corresponding to the critical test. i The solution.
[0039] The material aging performance data at each accelerated test temperature is formally split according to the residual value. y i -(1-e0 i )>0 is divided into data ( td i , yd i ), the remaining data points are divided into data ( tb i , yb i ), the performance characterization data of the first part at each accelerated test temperature after splitting ( td i , yd i ) is shown in Table 5 below, and the latter part of the performance characterization data ( tb i , yb i ) is shown in Table 6 below.
[0040] Table 5 Characterization data of thermal aging performance of EPDM ethylene propylene rubber at different accelerated test temperatures
[0041] Table 6 Characterization data of partial thermal aging performance of EPDM ethylene propylene rubber at different accelerated test temperatures
[0042] Take the material aging performance data after splitting at each accelerated test temperature ( tb i , yb i ), substitute it into formula (6), perform linear regression fitting on the model, and obtain the slope of the regression line kb i , intercept wb i and goodness of fit Rb i ; Let wb i =ln(1-e), calculate the estimated value of parameter e at the test temperature of the i-th group , let kb i =-b i , calculate the parameter b at the test temperature of the i-th group i Estimated value of .
[0043] By calculation, the slope of the linear regression line kb 90 =-3.1272E-04, kb 80 =-2.2389E-04, kb 70 =-7.4720E-05; intercept wb 90 =-0.3866, wb 80 =-0.2523,wb 70 =-0.3104; goodness of fit Rb 90 =0.9713, Rb 80 =0.9487, Rb 70=0.9637, the goodness of fit values are all greater than 0.8; the parameter estimates =0.3206, =0.2230, =0.2668; =3.1272E-04, =2.2389E-04, =7.4720E-05.
[0044] Take the material aging performance data after splitting at each accelerated test temperature ( td i , yd i ), substituting the estimated value of parameter e at each set of test temperatures , which is simplified from the material thermal aging kinetic function (5) into formula (7).
[0045]
[0046] Taking the natural logarithm of both sides of the function model equation, we obtain the following linear model, as shown in formula (8).
[0047]
[0048] The data ( td i , yd i ) is substituted into formula (8), and the model is fitted with linear regression to obtain the slope of the regression line kd i , intercept wd i and goodness of fit Rd i ; Let kd i =-d i , calculate the parameter d at the test temperature of the i-th group i Estimated value of .
[0049] By calculation, the slope of the linear regression line kd 90 =-0.0092, kd 80 =-0.0102, kd 70 =-0.0024; goodness of fit Rd 90 =0.9712, Rd 80 =0.9480, Rd 70 =0.9822, the goodness of fit values are all greater than 0.8; the parameter estimates =0.0092, =0.0102, =0.0024.
[0050] The estimated values of parameter e Take the arithmetic mean to get the initial value of parameter e =0.2702; b i =b0×[exp(-bE1×X i )], converted into a linear equation ln(b0)-X i ×bE1=ln(b i ),Will , X i Substitute the values into the equations to obtain an overdetermined linear system, and solve them simultaneously to obtain the initial value of the microparameter b =0.000309, =8.9502; D i =d0×[exp(-dE1×X i )], converted into a linear equation ln(d0)-X i ×dE1=ln(d i ),Will , X i Substitute the values into the equations to obtain an overdetermined linear system, and solve them simultaneously to obtain the initial value of the micro-parameter d =0.01047, =8.3873.
[0051] The initial values of the parameters determined above were input into the mature Russian commercial software Rubber Ageing for nonlinear fitting calculation. After 15 iterations, the fitting converged and the precise values of the regression parameters were obtained: e=0.2646, b0=0.000343, bE1=10.1307, d0=0.01090, dE1=9.1995.
[0052] Set any parameter to an initial value =0.5, =1, =1, =1, =1 is input into the Russian mature commercial software Rubber Ageing for nonlinear fitting calculation. The initial value deviates greatly and the fitting cannot converge. =0.5, =0.001, =1, =0.001, =1 was input into the mature Russian commercial software Rubber Ageing for nonlinear fitting calculation. After 22 iterations, the fitting converged and the precise values of the regression parameters were obtained: e=0.2646, b0=0.000343, bE1=10.1307, d0=0.01090, dE1=9.1995.
[0053] It can be found from this embodiment that when performing the thermal aging characteristics fitting analysis of materials, if any given initial value of the parameter =0.5, =1, =1, =1, =1, the initial value deviates greatly, and nonlinear fitting is prone to fail to converge; if the initial value of the parameter is given =0.5, =0.001, =1, =0.001, =1, the initial value is relatively close, and the fitting converges after 22 iterations; the method of the present invention can give the initial value of the parameter close to the precise value of the parameter, and the fitting converges after 15 iterations to obtain the precise value of the regression parameter in a short time. It can avoid the problems of nonlinear regression nonconvergence and deviation from the true value caused by inappropriate initial parameter values, and improve the efficiency of scientific research work.
[0054] Example 2 In this embodiment, accelerated heat aging tests are performed on natural rubber NR at accelerated test temperatures of 85°C, 75°C and 65°C, respectively. The test data are grouped according to the accelerated test temperatures, and the data in each group are arranged in ascending order according to the test time. The test data of the heat aging performance of the NR rubber material are obtained as shown in Table 7 below.
[0055] Table 7 NR rubber thermal aging performance test data at different accelerated test temperatures
[0056] The natural logarithm of each set of material performance test value data is taken as the dependent variable, and the corresponding aging time is taken as the independent variable. Linear regression fitting is performed to obtain the slope of the fitting equation of the material performance test logarithm value at all temperatures to the aging time. The average value of all slopes is k0=-0.0296, and the material performance characterization value y i = P i .
[0057] The accelerated thermal aging test temperature T i Substituting into formula (1), we can obtain the conversion temperature value X suitable for the accelerated thermal aging kinetic function. iThrough the above conversion, the rubber material performance characterization data is obtained as shown in Table 8 below.
[0058] Table 8 Characterization data of thermal aging performance of NR rubber at different accelerated test temperatures
[0059] According to the thermal aging reaction mechanism of rubber materials, the double exponential nested model shown in formula (2) is used as a function to describe the aging kinetic characteristics of the material.
[0060] Nested parameter b in the thermal aging kinetic function i d i It is described by formula (3).
[0061] Let 0<b i <d i , take the test corresponding to half of the test times at each accelerated test temperature as the critical test. If half of the test times is a decimal, round it up to the integer as the critical test. When the aging time is greater than or equal to the aging time corresponding to the critical test, the material thermal aging kinetic function is approximately as formula (4). When the aging time is less than the aging time corresponding to the critical test, the material thermal aging kinetic function is approximately as formula (5).
[0062] Based on the determined critical tests, the material performance characterization values at each accelerated test temperature y i Perform pre-splitting and only take the data points corresponding to the critical test and after it to obtain the split data ( th i , yh i ), as shown in Table 9 below.
[0063] Table 9 Pre-split data of NR rubber thermal aging performance characterization at different accelerated test temperatures
[0064] The data ( th i , yh i ) into model (6), perform linear regression fitting on the model, and obtain the slope of the regression line kh i , intercept wh i And goodness of fit Rh i .
[0065] wh i =ln(1-e), and the parameter estimation value e0 at the i-th group test temperature is calculated using formula (6): i ; Substitute e0 i , calculate the residual value yi -(1-e0 i ). By calculation, the linear regression line intercept wh 85 =-0.4114,wh 75 =-0.4174,wh 65 =-0.3916; goodness of fit Rh 85 =0.9888, Rh 75 =0.9960, Rh 65 =0.9914, the goodness of fit values are all greater than 0.8; the parameter estimate value e0 85 =0.3373,e0 75 =0.3412, e0 65 =0.3241, and the performance characterization residual data at each test temperature are shown in Table 10 below.
[0066] Table 10 Residual data of NR rubber thermal aging performance characterization at different test temperatures
[0067] The material aging performance data at each accelerated test temperature is formally split according to the residual value. y i -(1-e0 i )>0 is divided into data ( td i , yd i ), the remaining data points are divided into data ( tb i , yb i ), the performance characterization data of the first part at each accelerated test temperature after splitting ( td i , yd i ) is shown in Table 11 below, and the latter part of the performance characterization data ( tb i , yb i ) is shown in Table 12 below.
[0068] Table 11 Characterization data of thermal aging performance of NR rubber front part at different accelerated test temperatures
[0069] Table 12 Characterization data of partial thermal aging performance of NR rubber at different accelerated test temperatures
[0070] Take the material aging performance data after splitting at each accelerated test temperature ( tb i , yb i ), substitute it into formula (6), perform linear regression fitting on the model, and obtain the slope of the regression line kb i , intercept wb i and goodness of fit Rb i ; Let wb i =ln(1-e), calculate the estimated value of parameter e at the test temperature of the i-th group , let kb i =-b i , calculate the parameter b at the test temperature of the i-th group i Estimated value of .
[0071] By calculation, the slope of the linear regression line kb 85 =-0.0513, kb 75 =-0.0208, kb 65 =-0.0084; intercept wb 85 =-0.3816, wb 75 =-0.3945,wb 65 =-0.3778; goodness of fit Rb 85 =0.9943, Rb 75 =0.9951, Rb 65 =0.9900, the goodness of fit values are all greater than 0.8; the parameter estimates =0.3173, =0.3260, =0.3147; =0.0513, =0.0208, =0.0084.
[0072] Take the material aging performance data after splitting at each accelerated test temperature ( td i , yd i ), substituting the estimated value of parameter e at each set of test temperatures , the data ( td i , yd i ) is substituted into formula (8), and the model is fitted with linear regression to obtain the slope of the regression line kd i , intercept wd i and goodness of fit Rd i ; Let kd i =-d i , calculate the parameter d at the test temperature of the i-th group iEstimated value of .
[0073] By calculation, the slope of the linear regression line kd 85 =-1.7483, kd 75 =-0.8510, kd 65 =-0.5248; goodness of fit Rd 85 =0.9882, Rd 75 =0.9947, Rd 65 =0.9921, the goodness of fit values are all greater than 0.8; the parameter estimates =1.7483, =0.8510, =0.5248.
[0074] The estimated values of parameter e Take the arithmetic mean to get the initial value of parameter e =0.3193; b i =b0×[exp(-bE1×X i )], converted into a linear equation ln(b0)-X i ×bE1=ln(b i ),Will , X i Substitute the values into the equations to obtain an overdetermined linear system, and solve them simultaneously to obtain the initial value of the microparameter b =0.065599, =10.921290; D i =d0×[exp(-dE1×X i )], converted into a linear equation ln(d0)-X i ×dE1=ln(d i ),Will , X i Substitute the values into the equations to obtain an overdetermined linear system, and solve them simultaneously to obtain the initial value of the micro-parameter d =1.976761, =7.264393.
[0075] The initial values of the parameters determined above were input into the mature Russian commercial software Rubber Ageing for nonlinear fitting calculation. After 7 iterations, the fitting converged and the precise values of the regression parameters were obtained: e=0.3219, b0=0.0665068, bE1=11.1218, d0=1.08025, dE1=5.54241.
[0076] will be close to the initial value of the parameter =0.5, =1, =1, =1, =1 was input into the mature Russian commercial software Rubber Ageing for nonlinear fitting calculation. After 40 iterations, the fitting converged and the precise values of the regression parameters were obtained: e=0.3219, b0=0.0665068, bE1=11.1218, d0=1.08025, dE1=5.54241.
[0077] It can be found from this embodiment that when performing the thermal aging characteristics fitting analysis of the material, if the initial value of the parameter is given =0.5, =1, =1, =1, =1, the initial value is relatively close, and the fitting converges after 40 iterations; the method of the present invention can give the initial value of the parameter close to the precise value of the parameter, and after 7 iterations of fitting convergence, the precise value of the regression parameter is obtained in a short time, which can avoid the problems of nonlinear regression nonconvergence and deviation from the true value caused by inappropriate initial parameter values, thereby improving the efficiency of scientific research work.
Claims
1. A method for calculating the initial value of a double exponential nested model driven by accelerated test data, characterized in that: Here are the steps: 1) For polymer materials whose thermal aging reaction kinetics satisfy the Arrhenius equation, based on the thermal properties of the materials, select no less than three test temperatures within the range below the glass transition temperature of the materials to conduct accelerated thermal aging tests on the materials; group the test data according to the accelerated test temperature to obtain no less than three groups of test data ( t i , P i ), the number of groups is consistent with the number of test temperatures; 2) Take the natural logarithm of each set of material performance test value data, perform linear regression fitting, and obtain the slope of the fitting equation of the material performance logarithm value to the aging time at all accelerated test temperatures. Take the average value of the slope to obtain k0; if k0 < 0, then let the material performance characterization value y i = P i ; If k0>0, let the material performance characterization value y i =1- P i ; 3) According to the following formula, the accelerated thermal aging test temperature T i Perform conversion and calculate the conversion temperature value suitable for the accelerated thermal aging kinetic function; 4) According to the thermal aging reaction mechanism of the material, the double exponential nested model shown below is used as a function to describe the thermal aging kinetic characteristics of the material; y i =(1-e)×exp(-b i × t i )+e×exp(-d i × t i ) Where e and b i ,d i is the regression macro parameter; the e value is the weight coefficient of the two reactions before and after, 0<e<1; 5) Nested parameter b in thermal aging kinetic function i ,d i The following formula is used to describe: b i =b0×[exp(-bE1×X i )] d i =d0×[exp(-dE1×X i )] Where b0, bE1, d0, dE1 are the material activation energy micro parameters; b i >0,d i >0; 6) Let 0<b i <d i , the critical test is determined based on the number of tests; when the aging time is greater than or equal to the aging time corresponding to the critical test, the material thermal aging kinetic function is approximately: y i =(1-e)×exp(-b i × t i ); When the aging time is less than the corresponding aging time of the critical test, the material thermal aging kinetic function is approximately y i =(1-e)+e×exp(-d i × t i ); 7) Based on the determined critical test, the material performance characterization data at each accelerated test temperature is pre-split, and only the corresponding data points of the critical test and after are taken to obtain the material aging performance data at each accelerated test temperature after the split ( th i , yh i ); 8) Taking the material aging performance data after decomposition, the material thermal aging kinetic function is simplified to y i =(1-e)×exp(-b i × t i ); Taking the natural logarithm of both sides of the function model equation, we get the following linear model; ln( y i )=ln(1-e)-b i x t i Material aging performance data ( th i , yh i ) is substituted into the above formula, and the model is fitted with linear regression to obtain the slope, intercept and goodness of fit of the regression line; 9) Based on the intercept of the regression line, calculate the estimated value e0 of the parameter e i ; Calculate the residual value y i -(1-e0 i ), y i -(1-e0 i )>0 is divided into data ( td i , yd i ), the remaining data points are divided into data ( tb i , yb i ) to complete the formal splitting of material aging performance data at each test temperature; 10) Obtain material aging performance data at each accelerated test temperature ( tb i , yb i ), and substitute it into ln( y i )=ln(1-e)-b i × t i , perform linear regression fitting on the model, obtain the slope, intercept and goodness of fit of the regression line, and calculate the estimated value of parameter e at the test temperature of the i-th group , parameter b i Estimated value of ; 11) Obtain material aging performance data at each accelerated test temperature ( td i , yd i ), substituting the estimated value of parameter e at each set of test temperatures , the material thermal aging kinetic function is simplified to y i -(1- )= ×exp(-d i × t i ); Taking the natural logarithm of both sides of the function model equation, we get the following linear model; ln( y i -(1- ))=ln( )-d i × t i Material aging performance data ( td i , yd i ) is substituted into the above formula, and the model is fitted with linear regression to obtain the slope, intercept and goodness of fit of the regression line, and the parameter d at the test temperature of the i-th group is calculated. i Estimated value of ; 12) Estimated values of parameter e Take the arithmetic mean to get the initial value of parameter e ; b i =b0×[exp(-bE1×X i )], converted into a linear equation ln(b0)-X i ×bE1=ln(b i ),Will , X i Substitute the value into the linear equation system and solve it to get the initial value of the parameter b , ; D i =d0×[exp(-dE1×X i )], converted into a linear equation ln(d0)-X i ×dE1=ln(d i ),Will , X i Substitute the value into the linear equation system and solve it to get the initial value of the parameter d , ; So far, the initial values of all regression parameters of the double exponential nested model of thermal aging kinetics have been quickly calculated.
2. The method for calculating initial values of a double exponential nested model driven by accelerated test data according to claim 1, characterized in that: In the step 2), the linear fitting of the material performance test logarithm to the aging time only distinguishes the increasing and decreasing relationship between the material performance test value and the aging time, and uniformly sets the material performance characterization value to decrease with the aging time.
3. The method for calculating initial values of a double exponential nested model driven by accelerated test data according to claim 1, characterized in that: In step 6), the test corresponding to half of the test number at each accelerated test temperature is taken as the critical test. If half of the test number is a decimal, it is rounded up as the critical test.
4. The method for calculating initial values of a double exponential nested model driven by accelerated test data according to claim 1, characterized in that: In step 6), the order of the two reactions is not distinguished in the thermal aging kinetic function fitting. i ,d i Can be interchanged.
5. The method for calculating initial values of a double exponential nested model driven by accelerated test data according to claim 1, characterized in that: In the step 7), in the accelerated thermal aging test of materials, at each test temperature, the number of test time test points should not be less than 10, and the number of data points selected by data pre-splitting should not be less than 6.
6. The method for calculating initial values of a double exponential nested model driven by accelerated test data according to claim 1, characterized in that: In step 9), when the aging time t i When the aging time is less than the critical test corresponding aging time, the material thermal aging kinetic function is approximately: y i =(1-e)+e×exp(-d i × t i ), e×exp(-d i × t i ) is always a positive number, that is y i -(1-e) is always a positive number, so take y i The time interval in which -(1-e)>0 holds is approximately t i The parameter d is smaller than the interval of aging time corresponding to the critical test. i The solution.
7. The method for calculating initial values of a double exponential nested model driven by accelerated test data according to claim 1, characterized in that: In the steps 8), 10) and 11), when performing linear regression fitting, the goodness of fit value must be greater than 0.
8.
8. The method for calculating initial values of a double exponential nested model driven by accelerated test data according to claim 1, characterized in that: In step 12), solve b i ,d i The linear equations of micro-parameters are overdetermined, and the solution is the least squares solution of the equations.