Preparation method for constructing aqueous zinc ion battery negative electrode by metal organic framework coating
Through the metal organic framework coating construction method, the problem of zinc electrode instability is solved, a dense and uniform ZIF-8-M coating is prepared, which significantly improves the cycle stability and protective capabilities of the zinc electrode, and the cycle life is increased to that of traditional 20 times the method.
Patent Information
- Application Number
- CN202410283741.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-10
AI Technical Summary
The instability of the zinc electrode in aqueous zinc-ion batteries is mainly due to the uneven deposition of zinc ions on the electrode. Existing materials are used to limit and guide the diffusion of zinc ions, but the effect is not good, and the formed pores and gaps are uneven in size, affecting zinc ions. transmission.
Using a metal organic framework coating construction method, the ZIF-8 precursor solution is prepared by mixing a methanol solution of dimethylimidazole, a methanol solution of zinc ions and the regulator triethylamine, and then centrifuges and adds organic solvents and binders. A colloid is formed, coated on the zinc negative electrode, and subjected to high-temperature treatment in an inert atmosphere to optimize the coating crystal form and form a dense and uniform ZIF-8-M coating.
The prepared ZIF-8-M coating is more dense and uniform, without stacking holes, which significantly improves the cycle stability of the zinc electrode. The electrode's protective ability is better than that of traditional MOF-based coatings, and the cycle life is significantly improved.
Smart Images

Figure CN118867104A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic synthesis, and in particular to a method for preparing a negative electrode of an aqueous zinc ion battery constructed by using a metal organic framework coating. Background Art
[0002] As a new type of battery, aqueous zinc-ion battery has attracted widespread attention from researchers as soon as it was proposed. Its negative electrode is zinc. Unlike highly active lithium, zinc does not react violently with oxygen in an air atmosphere and is very safe. At the same time, due to the limited activity of zinc, it does not react violently with water. Aqueous electrolyte can be used to avoid the toxicity and harm of organic electrolytes. The positive electrode is usually manganese dioxide, which is also a non-toxic and harmless material. In addition, aqueous zinc-ion batteries have high theoretical capacity (820mAh g-1, 5855mAh cm-3) and low cost. It is precisely because of these advantages of aqueous zinc-ion batteries that they have become a research hotspot as soon as they were proposed. However, there is still a difficult problem in aqueous zinc-ion batteries - the instability of zinc electrodes. The instability of zinc electrodes is mainly caused by the uneven deposition of zinc ions on zinc electrodes. Diffusion, as the first step in zinc ion deposition, plays a vital role in the deposition of zinc ions. Therefore, the deposition of zinc ions can be affected or even controlled by controlling the diffusion of zinc ions.
[0003] To date, a variety of materials have been reported to be used to limit and guide the diffusion of zinc ions. For example, the accumulated pores formed by granular materials and the gaps remaining during the solidification process of organic matter can be used to guide and limit the diffusion of zinc ions, and these modified materials show better cycle stability than bare zinc electrodes. However, these materials have not completely solved this problem. The accumulated pores formed by these materials or the gaps formed during molding can control and limit the transport of zinc ions to a certain extent, but these accumulated pores or gaps are of different sizes and unevenly distributed, which is not conducive to better control of zinc ion transport. Therefore, it is of great significance to develop MOF-based coatings with specific pore structures and infinitely expandable network structures. Summary of the invention
[0004] The purpose of the present invention is to provide a preparation process of high-strength and high-heat-resistant para-aramid nanopaper with simple process, excellent product performance, environmental friendliness and low cost in view of the above-mentioned problems.
[0005] The present invention provides a method for preparing a negative electrode of an aqueous zinc ion battery constructed by a metal organic framework coating, comprising the following steps:
[0006] S1, mixing a methanol solution of dimethylimidazole, a methanol solution of zinc ions and a regulator, triethylamine, to prepare a ZIF-8 precursor solution;
[0007] S2, centrifuging the ZIF-8 precursor solution to obtain a precipitate, adding an organic solvent and a binder solution to the precipitate to mix into a colloid, coating the precipitate on a zinc negative electrode, drying and cooling to form an oligomer;
[0008] S3. Treat the electrode at high temperature in an inert atmosphere to fully polymerize the oligomers and optimize the coating crystal form.
[0009] In some embodiments, the concentration of the methanol solution of zinc ions is 1.2544 mol / L, the concentration of the methanol solution of dimethylimidazole is 0.4571 mol / mL, the volume ratio of the methanol solution of zinc ions to the methanol solution of dimethylimidazole is 1:1, and the molar ratio of the methanol solution of zinc ions to the regulator is 1:4 to 1:0.5.
[0010] In some embodiments, in step S2, the organic solvent is methanol, and the binder solution is a DMF solution of polyvinylidene fluoride.
[0011] In some embodiments, in step S2, the concentration of the DMF solution of polyvinylidene fluoride is 1 mg / mL, and the volume ratio of the methanol, the DMF solution of polyvinylidene fluoride and the ZIF-8 precursor solution is 3:1:10.
[0012] In some embodiments, in step S2, the drying temperature is 60° C. to 80° C., and the drying time is 2 to 3 hours.
[0013] In some embodiments, in step S3, the inert gas is argon or nitrogen, and the processing temperature is 120°C to 200°C.
[0014] Compared with the prior art, the present invention has the following beneficial effects:
[0015] The present invention provides a method for preparing a negative electrode of an aqueous zinc ion battery using a metal organic framework coating. The polymerization induction strategy is simple to operate and easy to control, and the ZIF-8 coating prepared by the method is more dense and uniform, and has no accumulation pores. The coating prepared by the new method has better protection for the zinc electrode than the MOF-based coating prepared by the traditional method, because the ZIF-8-M coating is more uniform, and the product formed after the transformation is also more uniform and dense. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 Characterization of the crystal form (a) and SEM morphology (b) of ZIF-8-M coating;
[0017] Figure 2 is the contact angle of ZIF-8-M / Zn electrode;
[0018] Figure 3SEM images of the cross-section of ZIF-8-M with different thicknesses, (a) ZIF-8-M-30 / Zn, (b) ZIF-8-M / Zn,
[0019] (c) ZIF-8-M-80 / Zn;
[0020] Figure 4 (a) is the XRD characterization of ZIF-8-M / Zn electrodes treated at different temperatures, (b) is the SEM characterization of ZIF-8-M-R120, and (c) is the SEM characterization of ZIF-8-M-R200;
[0021] Figure 5 It is a symmetrical electrode constant current charge and discharge test of ZIF-8-M-R120 / Zn electrode;
[0022] Figure 6 SEM image of MOF-based coating prepared by traditional method;
[0023] Figure 7 Symmetrical electrode constant current charge and discharge tests were performed on bare zinc electrode, ZIF-8-P / Zn electrode, and ZIF-8-M / Zn electrode. DETAILED DESCRIPTION
[0024] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0025] Embodiment 1:
[0026] Preparation of ZIF-8-M / Zn electrode
[0027] Weigh 0.186 g of zinc nitrate and add it to 5 mL of methanol, then dissolve it in 5 mL of methanol, marking it as solution 1. Weigh 0.103 g of dimethylimidazole and dissolve it in 5 mL of methanol, then add 160 μL of triethylamine, ultrasonically dissolve it, and mark it as solution 2. Quickly mix solutions 1 and 2, stir for 30 minutes, and then transfer the mixed solution to a refrigerator for cold storage for later use.
[0028] Take 1mL of ZIF-8 precursor solution, centrifuge (5min, 8000rpm), remove the upper solution, then add 300μL of methanol and 100μL of 1mg / mL polyvinylidene fluoride DMF solution to the lower precipitate, and disperse it by ultrasonic. Take 50μL of the turbid solution obtained in the previous step and apply it to the bare zinc electrode, then transfer it to a sealed petri dish, dry it in an 80℃ oven for 2h, and then cool it naturally for use.
[0029] in, Figure 1 Characterization of the crystal form (a) and SEM morphology (b) of the ZIF-8-M coating. From XRD, it can be basically confirmed that the coating is a ZIF-8-M coating. The coating is composed of a whole piece, not the accumulation of particles, and the surface is smooth and dense without accumulation pores.
[0030] Figure 2 is the contact angle of ZIF-8-M / Zn electrode. Compared with the bare zinc electrode, the contact angle between the electrode and water after ZIF-8 coating is reduced, and both become hydrophilic interfaces, which is conducive to the infiltration of electrolyte into the electrode;
[0031] Figure 3 (b) SEM image of the cross section of the ZIF-8-M / Zn electrode.
[0032] Embodiment 2:
[0033] Preparation of ZIF-8-M-30 / Zn electrode
[0034] Take 1 mL of ZIF-8 precursor solution, centrifuge (5 min, 8000 rpm), remove the upper solution, then add 300 μL of methanol and 100 μL of 1 mg / mL polyvinylidene fluoride DMF solution to the lower precipitate, and disperse by ultrasonic. Take 30 μL of the turbid solution obtained in the previous step and apply it to bare zinc.
[0035] in, Figure 3 (a) SEM image of the cross section of the ZIF-8-M-30 / Zn electrode.
[0036] Embodiment 3:
[0037] Preparation of ZIF-8-M-80 / Zn electrode
[0038] Take 1mL of ZIF-8 precursor solution, centrifuge (5min, 8000rpm), remove the upper solution, then add 300μL of methanol and 100μL of 1mg / mL polyvinylidene fluoride DMF solution to the lower precipitate, and disperse it by ultrasonic. Take 80μL of the turbid solution obtained in the previous step and apply it to the bare zinc electrode, then transfer it to a sealed culture dish, dry it in an oven at 80℃ for 2h, and then cool it naturally for use.
[0039] Embodiment 4:
[0040] Preparation of ZIF-8-M-R120 / Zn electrode
[0041] The ZIF-8-M / Zn electrode was treated at high temperature for 4 h at 120 °C in a nitrogen atmosphere using a tubular furnace.
[0042] in, Figure 4(a) (b) are the XRD and SEM characterizations of the ZIF-8-M / Zn electrode treated at 120°C. Small depressions and rods appear on the surface of the ZIF-8 after heat treatment. This is because during heat treatment, the oligomers tend to be more perfect crystals and migrate.
[0043] Embodiment 5:
[0044] Preparation of ZIF-8-M-R200 / Zn electrode
[0045] The ZIF-8-M / Zn electrode was treated at high temperature for 4 h at 200 °C in a nitrogen atmosphere using a tubular furnace.
[0046] in, Figure 4 (a) (c) are XRD and SEM characterizations of ZIF-8-M / Zn electrode treated at 120°C. After treatment at 200°C, cracks appeared in the ZIF-8 coating, which was caused by the different thermal expansion coefficients between the ZIF-8 coating and the zinc foil during heat treatment.
[0047] in, Figure 5 The symmetrical electrode constant current charge and discharge test of ZIF-8-M-R120 / Zn electrode showed that the cycle life of ZIF-8-M / Zn electrode after heat treatment at 120°C was about 1180h.
[0048] Comparative Example 1:
[0049] Preparation of ZIF-8-P / Zn electrode
[0050] The MOF-based coating was prepared by conventional methods, specifically:
[0051] Weigh the ZIF-8 particles and PVDF in a mass ratio of 8:2, place them in a mortar and grind them to mix evenly, and then transfer them to a weighing bottle. Add 450 μL DMF to every 100 mg of the mixture and stir for 12 hours to obtain a ZIF-8 particle slurry. The obtained ZIF-8 particle slurry is evenly scraped onto a commercial zinc foil using an automatic coating machine, then transferred to an 80°C oven to dry most of the solvent, and then transferred to a 120°C vacuum oven and dried for 12 hours to completely remove the solvent. The zinc foil coated with the ZIF-8 particle coating was cut into small discs with a diameter of 1.4 cm to obtain a zinc negative electrode modified with MOFs particles.
[0052] in, Figure 6 The SEM image of the MOF-based coating prepared by the conventional method shows that the MOF-based coating prepared by the conventional method has a large number of stacked pores, while the ZIF-8 coating prepared by the present invention has Figure 4 It can be seen that it is more dense and uniform, and there are no accumulation holes.
[0053] Figure 7 This is the constant current charge and discharge test of the symmetrical electrode of bare zinc electrode, ZIF-8-P / Zn electrode, and ZIF-8-M / Zn electrode. As can be seen from the figure, at 2 mA cm -2 Under the current density, the cycle life of bare zinc is about 120h, the cycle life of ZIF-8-P / Zn electrode is about 550h, and the cycle life of ZIF-8-M / Zn electrode is as long as 2400h. The comparison of the cycle life of symmetric cells shows that the ZIF-8 coating plays a protective role on the zinc electrode, but the ZIF-8 coating obtained by the polymerization coating method has better protection performance for the zinc electrode, and its cycle life is 20 times that of the bare zinc electrode and 4 times that of ZIF-8-P / Zn under the same conditions.
[0054] Finally, it should be noted that: technicians in this industry should understand that the present invention is not limited to the above-mentioned implementation cases. The above-mentioned embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which shall fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing a negative electrode of an aqueous zinc ion battery constructed with a metal organic framework coating, characterized in that: The following steps are involved: S1, mixing a methanol solution of dimethylimidazole, a methanol solution of zinc ions and a regulator, triethylamine, to prepare a ZIF-8 precursor solution; S2, centrifuging the ZIF-8 precursor solution to obtain a precipitate, adding an organic solvent and a binder solution to the precipitate to mix into a colloid, coating the precipitate on a zinc negative electrode, drying and cooling to form an oligomer; S3. Treat the electrode at high temperature in an inert atmosphere to fully polymerize the oligomers and optimize the coating crystal form.
2. The preparation method according to claim 1, characterized in that: The concentration of the zinc ion methanol solution is 1.2544 mol / L, the concentration of the dimethylimidazole methanol solution is 0.4571 mol / mL, the volume ratio of the zinc ion methanol solution to the dimethylimidazole methanol solution is 1:1, and the molar ratio of the zinc ion methanol solution to the regulator is 1:4 to 1:0.
5.
3. The preparation method according to claim 1, characterized in that: In the step S2, the organic solvent is methanol, and the binder solution is a DMF solution of polyvinylidene fluoride.
4. The preparation method according to claim 3, characterized in that: In the step S2, the concentration of the DMF solution of polyvinylidene fluoride is 1 mg / mL, and the volume ratio of the methanol, the DMF solution of polyvinylidene fluoride and the ZIF-8 precursor solution is 3:1:
10.
5. The preparation method according to claim 1, characterized in that: In the step S2, the drying temperature is 60°C to 80°C, and the drying time is 2 to 3 hours.
6. The preparation method according to claim 1, characterized in that: In step S3, the inert gas is argon or nitrogen, and the processing temperature is 120°C to 200°C.
Citation Information
Patent Citations
Preparation method of zinc ion battery negative electrode composite material and application thereof
CN112072087A
Modification method for interface of metal zinc negative electrode of aqueous zinc ion battery
CN113258070A
ZIF-8 film and spraying preparation method and application thereof
CN114733368A
Preparation method and application of amorphous MOF-derived ZIF
CN118083920A
Raised floor
KR102716729B1
Cited By
Preparation method and application of carbon-coated hydroxyapatite-loaded zinc compound composite material
CN121269652A
Preparation method and application of carbon-coated hydroxyapatite loaded zinc compound composite
CN121269652B