Selenide sodium ion negative electrode material and preparation method and application thereof

By using the nano-hollow cubic structure and interface effect of antimony, bismuth, and indium selenide materials in sodium-ion batteries, the problems of low conductivity and volume expansion of metal selenide are solved, the storage capacity and rate performance of sodium ions are improved, and a better Stable battery performance.

CN118867232APending Publication Date: 2024-10-29SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410855880.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The conductivity of metal selenide sodium ion battery anode materials is low, resulting in large volume expansion, capacity fading and poor rate performance, which limits its practical application.

Method used

Using antimony, bismuth and indium selenide materials, it reduces mechanical stress and provides more active sites by forming a stable nano hollow cube structure, and produces a unique interface effect through the coupling of antimony, bismuth and indium selenide to improve the stability of sodium ions. Diffusion rate and conductivity.

Benefits of technology

It improves the storage capacity and rate performance of sodium ions, and enhances the cycle stability and capacity retention rate of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118867232A_ABST
    Figure CN118867232A_ABST
Patent Text Reader

Abstract

The invention provides a selenide sodium ion negative electrode material and a preparation method and application thereof. The selenide sodium ion negative electrode material comprises an antimony bismuth indium selenide material, and the morphology of the antimony bismuth indium selenide material is of a hollow cubic structure. According to the selenide sodium ion negative electrode material provided by the invention, through element matching of multi-metal selenide of antimony, bismuth and indium, the selenide sodium ion negative electrode material has a stable nano hollow cubic structure, so that mechanical stress during electrochemical reaction can be reduced, self expansion can be relieved, structural stability can be ensured, more active sites can be provided, and Na storage can be improved; a unique interface effect can be generated, the surface reaction kinetics can be further improved, the diffusion rate of sodium ions in a solid is increased, and the rate capability is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sodium ion batteries and relates to a selenide sodium ion negative electrode material and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries have the advantages of flexible application and long service life, but the shortage of Li resources has greatly limited the long-term development and application of lithium-ion batteries. Compared with lithium-ion batteries, sodium-ion batteries have similar energy storage mechanisms, but the relative abundance of sodium in the earth's crust is much greater than that of lithium (2.75% vs 0.0065%). Therefore, sodium-ion batteries, as the best alternative to lithium-ion batteries, have attracted the attention of researchers around the world.

[0003] At present, the most studied negative electrode materials for sodium-ion batteries are hard carbon materials, alloy materials, non-metallic elements and metal compounds. Among them, metal compound materials based on multi-electron conversion mechanism reactions have attracted much attention due to their high theoretical specific capacity.

[0004] Metal selenide is one of the most promising negative electrode materials for sodium ion batteries. + The conversion reaction has attracted widespread attention due to its advantages such as low cost, environmental friendliness and high specific capacity, such as cobalt selenide, zinc selenide, iron selenide, etc.

[0005] CN105789584A discloses a cobalt selenide / carbon sodium ion battery composite negative electrode material and a preparation method and application thereof. The cobalt selenide / carbon composite material is synthesized in one step by a hydrothermal reaction method. The morphology of the cobalt selenide in the composite material is uniformly rod-shaped, and the size and length are controllable.

[0006] CN105390674A discloses a sodium ion battery iron diselenide / sulfur-doped graphene negative electrode composite material and a preparation method thereof. The preparation method is to dissolve a sulfur source, a selenium-containing inorganic substance, an iron-containing inorganic salt, and citric acid or sodium citrate in a graphene oxide solution, add hydrazine hydrate dropwise to form a light black solution, add the solution into a hydrothermal reactor for reaction, cool the solution naturally after the reaction is completed, and repeatedly wash the reaction precipitate with distilled water and anhydrous ethanol, filter it by suction, and dry it to obtain an iron diselenide / sulfur-doped graphene composite material.

[0007] However, the conductivity of metal selenides is low, compared with Na + The conversion reaction leads to large volume expansion, resulting in capacity decay and poor rate performance, which seriously restricts its practical application. How to formulate some strategies to improve the electronic conductivity and cycle stability of selenide materials is the key to the research of selenide sodium ion battery negative electrode materials. Summary of the invention

[0008] In view of the shortcomings of the prior art, the object of the present invention is to provide a sodium selenide negative electrode material and a preparation method and application thereof. The sodium selenide negative electrode material provided by the present invention has a stable nano hollow cubic structure through the element combination of multi-metal selenides of antimony, bismuth and indium, which can not only reduce the mechanical stress during electrochemical reaction, relieve self-expansion, ensure structural stability, but also provide more active sites and improve Na storage; it can also produce a unique interface effect, which can further improve the surface reaction kinetics, promote the diffusion rate of sodium ions in the solid, and improve the rate performance.

[0009] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a sodium selenide negative electrode material, wherein the sodium selenide negative electrode material comprises an antimony bismuth indium selenide material, and the morphology of the antimony bismuth indium selenide material is a hollow cubic structure.

[0011] The selenide sodium ion negative electrode material provided by the present invention is composed of antimony, bismuth and indium selenide materials and has a stable nano hollow cubic structure, in which the metal elements and the morphology cooperate with each other, wherein the hollow structure can not only reduce the mechanical stress during the electrochemical reaction, alleviate its own expansion, and ensure the structural stability, but also provide more active sites and improve the Na storage; in addition, the selenides of antimony, bismuth and indium produce a unique interface effect by coupling nanomaterials with different band gaps, which can further improve the surface reaction kinetics, promote the diffusion rate of sodium ions in the solid, and improve the intrinsic conductivity, capacity and rate performance.

[0012] In the present invention, if the antimony bismuth indium selenide material does not have the morphology of a hollow cubic structure, the huge volume expansion of the material during the electrochemical reaction cannot be alleviated, resulting in too rapid decay of the battery capacity; and if the metal element combination in the selenide lacks any one of the elements in antimony bismuth indium, a higher rate performance cannot be achieved.

[0013] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0014] Preferably, the antimony bismuth indium selenide comprises a heterojunction structure composed of antimony selenide, bismuth selenide and indium selenide, and the heterojunction structure is a hollow cubic structure.

[0015] In the present invention, a heterojunction structure composed of antimony bismuth indium selenide material consisting of antimony selenide (Sb2Se3), bismuth selenide (Bi2Se3) and indium selenide (In2Se3) is obtained by coupling nanomaterials with different band gaps to produce a unique interface effect, which can further improve the surface reaction kinetics, promote the diffusion rate of sodium ions in the solid, and improve the rate performance.

[0016] Preferably, the chemical formula of the antimony bismuth indium selenide material is (Sb x Bi y In 2-x-y )Se3, where 0<x+y<2.

[0017] For example, the x can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8 or 1.9, etc.; the y can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8 or 1.9, etc., but are not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0018] The present invention further regulates the numerical range of the stoichiometric ratio of antimony, bismuth and indium in the antimony bismuth indium selenide material, thereby ensuring that the hollow cubic structure has a more excellent stability and making the interface effect after coupling more excellent; thereby obtaining more excellent cycle performance, capacity and rate performance.

[0019] Preferably, the specific surface area of ​​the antimony bismuth indium selenide material is 50 m 2 / g~300m 2 / g, for example 50m 2 / g, 75m 2 / g、100m 2 / g, 125m 2 / g, 150m 2 / g, 175m 2 / g, 200m 2 / g, 225m 2 / g, 250m 2 / g, 275m 2 / g or 300m 2 / g, etc., but are not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] Preferably, in the hollow cube structure, the side length of the cube is 200nm~1μm, for example 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm or 1μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] In the present invention, the side length of the cube in the hollow cubic structure is regulated to be 200 nm to 1 μm, which is more conducive to the stability of the structure and can better inhibit the self-expansion of the metal selenide material, while also ensuring more active sites.

[0022] Preferably, the surface of the antimony bismuth indium selenide material further includes a carbon coating layer.

[0023] In the present invention, the surface of the antimony bismuth indium selenide material is further treated with carbon coating, which further suppresses the volume expansion of the material and improves the electrode stability.

[0024] In a second aspect, the present invention provides a method for preparing the sodium selenide negative electrode material as described in the first aspect, the preparation method comprising the following steps:

[0025] The sacrificial template, antimony salt, bismuth salt, etchant, precipitant and first solvent are mixed at one time, and a first precipitation reaction is performed to obtain an antimony-bismuth hollow cubic structure;

[0026] The surface of the hollow cubic structure of antimony bismuth is coated with an indium compound, and sintered to obtain an antimony bismuth indium oxide with a hollow three-dimensional structure;

[0027] The antimony bismuth indium oxide is subjected to a selenization reaction with a selenium source to obtain the selenide sodium ion negative electrode material.

[0028] The preparation method provided by the present invention uses a template with a cubic structure as a sacrificial template, antimony bismuth precipitates are condensed on the surface of the cubic structure, and the sacrificial template is etched away by an etchant, thereby obtaining an antimony bismuth hollow cubic structure; further, by coating an indium-containing compound and performing a selenization reaction, a stable nano hollow cubic structure composed of antimony bismuth indium selenide materials is obtained.

[0029] In the present invention, if the antimony source, bismuth source, indium source and selenium source are directly mixed and sintered to obtain a product structure without a specific morphology, electrode stability and high reversible capacity cannot be achieved; at the same time, during the preparation process, an antimony-bismuth hollow cubic structure is preferably prepared, which is more conducive to exerting the heterogeneous structure effect and improving the rate performance.

[0030] Preferably, the sacrificial template comprises a Cu2O nanocube template.

[0031] It should be noted that, in addition to the Cu2O nanocube template, other cubic structure templates are also applicable to the present invention without affecting the structure of the final product.

[0032] Preferably, the method for preparing the Cu2O nanocube template comprises:

[0033] The copper salt, alkaline solution and reducing agent solution are mixed and reacted to obtain the Cu2O nanocube template.

[0034] Preferably, the mixing reaction method comprises: stirring the copper salt solution and the alkaline solution at one time, and then adding the reducing agent solution to carry out an aging reaction.

[0035] Preferably, the molar ratio of the copper in the copper salt, the alkaline substance in the alkaline solution and the reducing agent is (0.001-0.005):(0.02-0.1):(0.006-0.03), for example, 0.001:0.02:0.006, 0.001:0.05:0.006, 0.001:0.1:0.006, 0.001:0.02:0.015, 0.001:0.02:0.03, 0.003:0.02:0.006, 0.003:0.02:0.006, 0.005:0.02:0.006, 0.003:0.1:0.006, 0.005:0.1:0.006, 0.005:0.1:0.03.

[0036] Preferably, the stirring time is 0.5 to 3 h, such as 0.5 h, 1 h, 1.5 h, 2 h, 2.5 h or 3 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0037] Preferably, the temperature of the aging reaction is 25°C to 50°C, for example, 25°C, 30°C, 35°C, 40°C, 45°C or 50°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] Preferably, the aging reaction time is 2 to 6 hours, for example 2 hours, 3 hours, 4 hours, 5 hours or 6 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0039] In the present invention, the size of the obtained cubic structure can be adjusted by adjusting the preparation parameters of the Cu2O nanocube template.

[0040] Preferably, the raw materials mixed once further include a surfactant.

[0041] Preferably, the concentration of the sacrificial template in the solution after one mixing is 0.01mol / L to 2mol / L, for example, 0.01mol / L, 0.1mol / L, 0.3mol / L, 0.5mol / L, 0.8mol / L, 1mol / L, 1.3mol / L, 1.5mol / L, 1.8mol / L or 2mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] Preferably, the concentration of the antimony salt in the solution after the first mixing is 0.01mol / L to 1mol / L, for example, 0.01mol / L, 0.05mol / L, 0.1mol / L, 0.2mol / L, 0.3mol / L, 0.4mol / L, 0.5mol / L, 0.6mol / L, 0.7mol / L, 0.8mol / L, 0.9mol / L or 1mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] Preferably, the concentration of the bismuth salt in the solution after one mixing is 0.01mol / L to 1mol / L, for example, 0.01mol / L, 0.05mol / L, 0.1mol / L, 0.2mol / L, 0.3mol / L, 0.4mol / L, 0.5mol / L, 0.6mol / L, 0.7mol / L, 0.8mol / L, 0.9mol / L or 1mol / L, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] Preferably, the concentration of the etchant in the solution after one mixing is 0.5mol / L to 3mol / L, for example, 0.5mol / L, 0.8mol / L, 1mol / L, 1.3mol / L, 1.5mol / L, 1.8mol / L, 2mol / L, 2.3mol / L, 2.5mol / L, 2.8mol / L or 3mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] Preferably, the concentration of the precipitant in the solution after one mixing is 0.5 mol / L to 4 mol / L, for example 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L or 4 mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0046] Preferably, the etchant comprises thiosulfate.

[0047] The etching agent of the present invention contains S2O3 2- When S2O3 2- Solidification around the sacrificial template, coupled with the etching of Cu2O, followed by S2O3 2- OH produced by hydrolysis - This causes Sb and Bi ions to precipitate and form antimony-bismuth nanocubes, that is, the thiosulfide etchant not only plays the role of etching the sacrificial template, but also plays the role of forming an antimony-bismuth cubic structure; and the types of thiosulfate substances include but are not limited to sodium thiosulfate, sodium potassium thiosulfate or thiosulfuric acid.

[0048] Preferably, the temperature of the first precipitation reaction is 25°C to 50°C, for example, 25°C, 30°C, 35°C, 40°C, 45°C or 50°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0049] Preferably, the time of the first precipitation reaction is 10 to 180 min, for example, 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min or 180 min, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0050] Preferably, the coating method of the indium-containing compound comprises:

[0051] The antimony bismuth hollow cubic structure, indium salt, complex precipitant and second solvent are mixed for a second time, and a second precipitation reaction is performed to obtain an antimony bismuth indium precursor material.

[0052] Preferably, the secondary mixed raw materials further include a surfactant.

[0053] Preferably, the concentration of the antimony-bismuth hollow cubic structure in the solution after secondary mixing is 0.01 mol / L to 0.5 mol / L, for example, 0.01 mol / L, 0.05 mol / L, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L or 0.5 mol / L, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0054] Preferably, the concentration of the indium salt in the solution after the secondary mixing is 0.01mol / L to 1mol / L, for example, 0.01mol / L, 0.05mol / L, 0.1mol / L, 0.2mol / L, 0.3mol / L, 0.4mol / L, 0.5mol / L, 0.6mol / L, 0.7mol / L, 0.8mol / L, 0.9mol / L or 1mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0055] Preferably, the concentration of the complexing precipitant in the solution after the secondary mixing is 0.01 mol / L to 4 mol / L, for example, 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L or 4 mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0056] Preferably, the reaction temperature of the second precipitant is 25°C to 50°C, for example, 25°C, 30°C, 35°C, 40°C, 45°C or 50°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0057] Preferably, the time of the second precipitation reaction is 10 to 180 min, for example, 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min or 180 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0058] Preferably, the sintering heating rate is 1 to 10°C / min, for example, 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0059] Preferably, the sintering temperature is 400-600°C, such as 400°C, 450°C, 500°C, 550°C or 600°C, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0060] Preferably, the sintering time is 1 to 5 hours, such as 1 hour, 2 hours, 3 hours, 4 hours or 5 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0061] Preferably, the molar ratio of the antimony bismuth indium oxide to the selenium source is 1:(1-10), for example 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0062] Preferably, the selenization reaction comprises:

[0063] Antimony bismuth indium oxide, a selenium source, a second reducing agent and a third solvent are mixed and subjected to a solvothermal reaction to obtain a solvothermal reaction product.

[0064] Preferably, the molar ratio of the second reducing agent to the selenium source is (0.01-0.5):1, for example 0.01:1, 0.05:1, 0.11:, 0.2:1, 0.3:1, 0.4:1 or 0.5:1, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0065] Preferably, the temperature of the solvothermal reaction is 50-200°C, for example 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C or 200°C, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0066] Preferably, the solvent thermal reaction time is 1 to 24 h, for example 1 h, 5 h, 10 h, 12 h, 15 h, 18 h, 20 h or 24 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0067] Preferably, the product of the solvothermal reaction is subjected to carbon coating treatment.

[0068] Preferably, the mass ratio of the product of the solvothermal reaction to the carbon source is 1:(0.01-0.5), for example 1:0.01, 1:0.05, 1:0.1, 1:0.2, 1:0.3, 1:0.4 or 1:0.5, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0069] As a preferred technical solution, the preparation method comprises the following steps:

[0070] The copper salt solution and the alkaline solution are stirred for 0.5 to 3 hours at a time, and then the first reducing agent solution is added for aging reaction for 2 to 6 hours, and the molar ratio of copper in the copper salt, the alkaline substance in the alkaline solution and the reducing agent is (0.001 to 0.005): (0.02 to 0.1): (0.006 to 0.03) to obtain a Cu2O nanocube template;

[0071] A Cu2O nanocube template, an antimony salt, a bismuth salt, an etchant, a precipitant, a surfactant and a first solvent are mixed once, wherein the concentration of the Cu2O nanocube template in the mixed solution is 0.01 mol / L to 2 mol / L, the concentration of the antimony salt in the mixed solution is 0.01 mol / L to 1 mol / L, the concentration of the bismuth salt in the mixed solution is 0.01 mol / L to 1 mol / L, the concentration of the etchant in the mixed solution is 0.5 mol / L to 3 mol / L, the concentration of the precipitant in the mixed solution is 0.5 mol / L to 4 mol / L, and the first precipitation reaction is performed for 10 to 180 min to obtain an antimony-bismuth hollow cubic structure;

[0072] The antimony bismuth hollow cubic structure, indium salt, complex precipitant, surfactant and second solvent are mixed twice, wherein the concentration of the antimony bismuth hollow cubic structure in the solution after the second mixing is 0.01mol / L to 0.5mol / L, the concentration of the indium salt in the solution after the second mixing is 0.01mol / L to 1mol / L, and the concentration of the complex precipitant in the solution after the second mixing is 0.01mol / L to 4mol / L, the second precipitation reaction is 10 to 180min to obtain an antimony bismuth indium precursor material, and the temperature is increased to 400 to 600°C at a heating rate of 1 to 10°C / min and sintered for 1 to 5h to obtain an antimony bismuth indium oxide with a hollow three-dimensional structure;

[0073] Mixing antimony bismuth indium oxide, a selenium source, a second reducing agent and a third solvent, wherein the molar ratio of antimony bismuth indium oxide to the selenium source is 1:(1-10), and the molar ratio of the second reducing agent to the selenium source is (0.01-0.5):1, and performing a hydrothermal reaction at 50-200° C. for 1-24 hours to obtain a hydrothermal reaction product;

[0074] The product of the hydrothermal reaction is subjected to carbon coating treatment to obtain the selenide sodium ion negative electrode material.

[0075] It is to be understood that the concentration of the raw materials after the primary mixing and the secondary mixing in the present invention refers to the original concentration after mixing without reaction.

[0076] It should also be noted that the specific types of materials for the preparation of raw materials provided in the present invention, except for the above-mentioned limitations, are all selected by conventional technology, and those skilled in the art can adaptably select and adjust according to actual needs;

[0077] Optionally, the alkaline solution includes, but is not limited to, potassium hydroxide, sodium hydroxide or ammonia water, one or a mixture of any proportions thereof;

[0078] Optionally, the copper salt includes but is not limited to copper chloride, copper nitrate, copper sulfate or copper acetate, one or a mixture of any proportions thereof;

[0079] Optionally, the first reducing agent includes but is not limited to ascorbic acid;

[0080] Optionally, the surfactant (all surfactants involved in the above preparation method) includes but is not limited to polyvinyl pyrrolidone, polyethylene glycol, glycerol, sorbitol or diethanolamine, one or a mixture of any proportions thereof;

[0081] Optionally, the antimony salt includes but is not limited to antimony chloride, antimony nitrate, antimony acetate, antimony carbonate, antimony sulfate or antimony trioxide, or a mixture of any proportion of the above;

[0082] Optionally, the bismuth salt includes but is not limited to a mixture of one or more of bismuth chloride, bismuth nitrate, bismuth sulfate, bismuth acetate or bismuth carbonate in any proportion;

[0083] Optionally, the first solvent and the second solvent each independently include but are not limited to water;

[0084] Optionally, the precipitant includes but is not limited to potassium hydroxide, sodium hydroxide or ammonia water, one or a mixture of any proportions thereof;

[0085] Optionally, the indium salt includes but is not limited to indium acetate, indium nitrate, indium chloride, indium sulfate or indium carbonate, or a mixture of any proportion thereof;

[0086] Optionally, the complexing precipitant includes but is not limited to a precipitant or a complexing agent, the complexing agent includes but is not limited to a mixture of one or more of citric acid, carboxylic acid, ethylenediaminetetraacetic acid, oxalic acid or tartaric acid in any proportion, and the precipitant is a mixture of one or more of potassium hydroxide, sodium hydroxide, ammonia water in any proportion;

[0087] Optionally, the selenium source includes but is not limited to one or a mixture of any proportion of selenium dioxide, sodium selenide, sodium selenide, sodium selenite, selenous acid, sodium selenate or selenium powder;

[0088] Optionally, the third solvent includes but is not limited to one or a mixture of any proportion of dimethylformamide, N-methylpyrrolidone, dimethylacetamide, acetone, dichloromethane, chloroform or acetonitrile;

[0089] Optionally, the second reducing agent includes but is not limited to hydrazine hydrate or hydroxylamine, one or a mixture of any proportions thereof.

[0090] In a third aspect, the present invention further provides a sodium ion battery, comprising the selenide sodium ion negative electrode material as described in the first aspect or the selenide sodium ion negative electrode material prepared by the preparation method as described in the second aspect.

[0091] Compared with the prior art, the present invention has the following beneficial effects:

[0092] (1) The selenide sodium ion negative electrode material provided by the present invention is composed of antimony, bismuth and indium selenide materials and has a stable nano hollow cubic structure. The metal elements and morphology cooperate with each other. The hollow structure can not only reduce the mechanical stress during the electrochemical reaction, alleviate its own expansion, and ensure the structural stability, but also provide more active sites to improve Na storage. In addition, the selenides of antimony, bismuth and indium produce a unique interface effect by coupling nanomaterials with different band gaps, which can further improve the surface reaction kinetics, promote the diffusion rate of sodium ions in the solid, and improve the intrinsic conductivity, capacity and rate performance.

[0093] (2) The preparation method provided by the present invention uses a template with a cubic structure as a sacrificial template, antimony bismuth precipitates are condensed on the surface of the cubic structure, and the sacrificial template is etched away by an etchant, thereby obtaining an antimony bismuth hollow cubic structure; further, by coating with an indium-containing compound and undergoing a selenization reaction, a stable nano hollow cubic structure composed of antimony bismuth indium selenide materials is obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0094] Figure 1 This is a scanning electron microscope image of the antimony bismuth indium oxide material prepared in Example 1 of the present invention.

[0095] Figure 2 This is a scanning electron microscope image of the sodium selenide negative electrode material prepared in Example 1 of the present invention.

[0096] Figure 3 This is a transmission electron micrograph of the selenide sodium ion negative electrode material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0097] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0098] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in this application are intended to cover non-exclusive inclusions.

[0099] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.

[0100] Example 1

[0101] This embodiment provides a sodium selenide negative electrode material, wherein the sodium selenide negative electrode material comprises an antimony bismuth indium selenide material, wherein the antimony bismuth indium selenide comprises a heterojunction structure composed of antimony selenide, bismuth selenide and indium selenide, wherein the heterojunction structure is a hollow cube structure, and the side length of the hollow cube is 500 nm;

[0102] The chemical formula of the antimony bismuth indium selenide material is (Sb 0.8 Bi 0.6 In 0.6 )Se3; The surface of the antimony bismuth indium selenide material also includes a carbon coating layer.

[0103] The preparation method of the selenide sodium ion negative electrode material is as follows:

[0104] (1) A copper salt solution (CuCl2·2H2O) and an alkaline solution (sodium hydroxide) were stirred for 1.5 h, and then a first reducing agent solution (ascorbic acid) was added for aging reaction at 30°C for 4 h, wherein the molar ratio of copper in the copper salt, the alkaline substance in the alkaline solution, and the reducing agent was 0.003:0.06:0.01, to obtain a Cu2O nanocube template (sacrificial template);

[0105] (2) mixing a sacrificial template, an antimony salt (SbCl3), a bismuth salt (BiCl3), an etchant (Na2S2O3), a precipitant (sodium hydroxide), a surfactant (polyvinyl pyrrolidone) and deionized water at one time, wherein the concentration of the sacrificial template is 0.1 mol / L, the concentration of the antimony salt is 0.08 mol / L, the concentration of the bismuth salt is 0.06 mol / L, the concentration of the etchant is 1 mol / L, and the concentration of the precipitant is 0.42 mol / L, and subjecting the mixed solution to a first precipitation reaction at 25° C. for 60 min to obtain a hollow cubic structure of antimony bismuth hydroxide;

[0106] (3) secondary mixing of antimony bismuth hydroxide hollow cubic structure, indium salt (InCl3), complex precipitant (citric acid), surfactant (polyvinyl pyrrolidone) and deionized water, wherein the concentration of antimony bismuth hollow cubic structure, the concentration of indium salt and the concentration of complex precipitant are 1 mol / L, 0.06 mol / L and 0.18 mol / L, and the secondary mixed solution is subjected to a second precipitation reaction at 25°C for 60 min to obtain antimony bismuth indium precursor material, and the temperature is increased to 500°C at a heating rate of 2°C / min and sintered for 2 h to obtain antimony bismuth indium oxide with a hollow three-dimensional structure;

[0107] (4) mixing antimony bismuth indium oxide, a selenium source (sodium selenide), a second reducing agent (hydrazine hydrate) and N,N-dimethylformamide, wherein the molar ratio of antimony bismuth indium oxide to the selenium source is 1:1.5, and the molar ratio of the second reducing agent to the selenium source is 0.03:1, and performing a hydrothermal reaction at 150° C. for 6 hours to obtain a hydrothermal reaction product;

[0108] (5) The hydrothermal reaction product and glucose were dispersed in deionized water at a mass ratio of 1:0.1, transferred to a hydrothermal kettle, and subjected to hydrothermal reaction at 200° C. for 12 hours. After the reaction was completed, the precipitate was filtered and washed to obtain the selenide sodium ion negative electrode material.

[0109] Figure 1 The scanning electron microscope image of the antimony bismuth indium oxide material prepared in Example 1 of the present invention is shown; Figure 2 The scanning electron microscope image of the sodium selenide negative electrode material prepared in Example 1 of the present invention is shown; Figure 3 The transmission electron microscope image of the selenide sodium ion negative electrode material prepared in Example 1 of the present invention is shown.

[0110] from Figure 1-3 It can be concluded that in the selenide sodium ion negative electrode material provided by the present invention, the antimony bismuth indium selenide has the morphology of a hollow cubic structure, and the particle size is uniform and the dispersibility is good.

[0111] Example 2

[0112] This embodiment provides a sodium selenide negative electrode material, wherein the sodium selenide negative electrode material comprises an antimony bismuth indium selenide material, wherein the antimony bismuth indium selenide comprises a heterojunction structure composed of antimony selenide, bismuth selenide and indium selenide, wherein the heterojunction structure is a hollow cube structure, and the side length of the hollow cube is 200 nm;

[0113] The chemical formula of the antimony bismuth indium selenide material is (Sb 0.67 Bi 0.67 In 0.67 )Se3; The surface of the antimony bismuth indium selenide material also includes a carbon coating layer.

[0114] The preparation method of the selenide sodium ion negative electrode material is as follows:

[0115] (1) A copper salt solution (CuCl2·2H2O) and an alkaline solution (sodium hydroxide) were stirred for 0.5 h, and then a first reducing agent solution (ascorbic acid) was added to perform an aging reaction at 50°C for 2 h, wherein the molar ratio of copper in the copper salt, the alkaline substance in the alkaline solution, and the reducing agent was 0.004:0.09:0.02, to obtain a Cu2O nanocube template (sacrificial template);

[0116] (2) Mixing a sacrificial template, antimony salt (Sb(NO3)3), bismuth salt (Bi(NO3)3), etchant (Na2S2O3), precipitant (sodium hydroxide), surfactant (polyethylene glycol) and deionized water at one time, wherein the concentration of the sacrificial template is 0.15 mol / L, the concentration of the antimony salt is 0.1 mol / L, the concentration of the bismuth salt is 0.1 mol / L, the concentration of the etchant is 1.5 mol / L, and the concentration of the precipitant is 0.6 mol / L, and the mixed solution is subjected to a first precipitation reaction at 45°C for 30 minutes to obtain a hollow cubic structure of antimony bismuth hydroxide.

[0117] (3) secondary mixing of antimony bismuth hydroxide hollow cubic structure, indium salt (In(NO3)3), complex precipitant (oxalic acid), surfactant (polyethylene glycol) and deionized water, wherein the concentration of antimony bismuth hollow cubic structure, the concentration of indium salt and the concentration of complex precipitant are 1 mol / L, 0.1 mol / L and 0.3 mol / L, and the secondary mixed solution is subjected to a second precipitation reaction at 45°C for 30 min to obtain antimony bismuth indium precursor material, and the temperature is increased to 400°C at a heating rate of 1°C / min and sintered for 5 h to obtain antimony bismuth indium oxide with a hollow three-dimensional structure;

[0118] (4) mixing antimony bismuth indium oxide, a selenium source (sodium selenide), a second reducing agent (hydrazine hydrate) and N,N-dimethylformamide, wherein the molar ratio of antimony bismuth indium oxide to the selenium source is 1:3, and the molar ratio of the second reducing agent to the selenium source is 0.05:1, and performing a hydrothermal reaction at 200° C. for 12 hours to obtain a hydrothermal reaction product;

[0119] (5) The hydrothermal reaction product and glucose were dispersed in deionized water at a mass ratio of 1:0.5, transferred to a hydrothermal kettle, and subjected to hydrothermal reaction at 200° C. for 12 hours. After the reaction was completed, the precipitate was filtered and washed to obtain the selenide sodium ion negative electrode material.

[0120] Example 3

[0121] This embodiment provides a sodium selenide negative electrode material, wherein the sodium selenide negative electrode material comprises an antimony bismuth indium selenide material, wherein the antimony bismuth indium selenide comprises a heterojunction structure composed of antimony selenide, bismuth selenide and indium selenide, wherein the heterojunction structure is a hollow cube structure, and the side length of the hollow cube is 1000 nm;

[0122] The chemical formula of the antimony bismuth indium selenide material is (Sb 0.4 Bi 0.8 In 0.8 )Se3; The surface of the antimony bismuth indium selenide material also includes a carbon coating layer.

[0123] The preparation method of the selenide sodium ion negative electrode material is as follows:

[0124] (1) A copper salt solution (CuCl2·2H2O) and an alkaline solution (sodium hydroxide) were stirred for 3 h, and then a first reducing agent solution (ascorbic acid) was added to carry out an aging reaction at 30°C for 6 h, wherein the molar ratio of copper in the copper salt, the alkaline substance in the alkaline solution and the reducing agent was 0.003:0.09:0.025, to obtain a Cu2O nanocube template (sacrificial template);

[0125] (2) Mixing a sacrificial template, an antimony salt (SbCl3), a bismuth salt (BiCl3), an etchant (K2S2O3), a precipitant (sodium hydroxide), a surfactant (sorbitol) and deionized water at one time, wherein the concentration of the sacrificial template is 0.2 mol / L, the concentration of the antimony salt is 0.2 mol / L, the concentration of the bismuth salt is 0.4 mol / L, the concentration of the etchant is 2 mol / L, and the concentration of the precipitant is 1.6 mol / L, and the mixed solution is subjected to a first precipitation reaction at 25° C. for 120 min to obtain a hollow cubic structure of antimony bismuth hydroxide.

[0126] (3) secondary mixing of antimony bismuth hydroxide hollow cubic structure, indium salt (InCl3), complex precipitant (citric acid), surfactant (sorbitol) and deionized water, wherein the concentration of antimony bismuth hollow cubic structure, the concentration of indium salt and the concentration of complex precipitant are 1 mol / L, 0.4 mol / L and 1.2 mol / L, and the secondary mixed solution is subjected to a second precipitation reaction at 25°C for 60 min to obtain antimony bismuth indium precursor material, and the temperature is increased to 600°C at a heating rate of 10°C / min and sintered for 1 h to obtain antimony bismuth indium oxide with a hollow three-dimensional structure;

[0127] (4) mixing antimony bismuth indium oxide, a selenium source (sodium selenite), a second reducing agent (hydrazine hydrate) and chloroform, wherein the molar ratio of antimony bismuth indium oxide to the selenium source is 1:5, and the molar ratio of the second reducing agent to the selenium source is 0.1:1, and performing a hydrothermal reaction at 100° C. for 24 hours to obtain a hydrothermal reaction product;

[0128] (5) The hydrothermal reaction product and glucose are dispersed in deionized water at a mass ratio of 1:0.1, dried, and carbonized at 800° C. in a nitrogen atmosphere to obtain the selenide sodium ion negative electrode material.

[0129] Example 4

[0130] This embodiment provides a sodium selenide negative electrode material, wherein the sodium selenide negative electrode material comprises an antimony bismuth indium selenide material, wherein the antimony bismuth indium selenide comprises a heterojunction structure composed of antimony selenide, bismuth selenide and indium selenide, wherein the heterojunction structure is a hollow cube structure, and the side length of the hollow cube is 600 nm;

[0131] The chemical formula of the antimony bismuth indium selenide material is (Sb 1.2 Bi 0.4 In 0.4 )Se3; The surface of the antimony bismuth indium selenide material also includes a carbon coating layer.

[0132] The preparation method of the selenide sodium ion negative electrode material is as follows:

[0133] (1) A copper salt solution (CuCl2·2H2O) and an alkaline solution (sodium hydroxide) were stirred for 2 h, and then a first reducing agent solution (ascorbic acid) was added for aging reaction at 30°C for 4 h, wherein the molar ratio of copper in the copper salt, the alkaline substance in the alkaline solution and the reducing agent was 0.003:0.06:0.01, to obtain a Cu2O nanocube template (sacrificial template);

[0134] (2) Mixing a sacrificial template, antimony salt (SbCl3), bismuth salt (BiCl3), etchant (Na2S2O3), precipitant (sodium hydroxide), surfactant (polyvinyl pyrrolidone) and deionized water at one time, wherein the concentration of the sacrificial template is 0.1 mol / L, the concentration of the antimony salt is 0.3 mol / L, the concentration of the bismuth salt is 0.1 mol / L, the concentration of the etchant is 1 mol / L, and the concentration of the precipitant is 1.5 mol / L, and the mixed solution is subjected to a first precipitation reaction at 25°C for 180 min to obtain a hollow cubic structure of antimony bismuth hydroxide.

[0135] (3) secondary mixing of antimony bismuth hydroxide hollow cubic structure, indium salt (InCl3), complex precipitant (citric acid), surfactant (polyvinyl pyrrolidone) and deionized water, wherein the concentration of antimony bismuth hollow cubic structure, the concentration of indium salt and the concentration of complex precipitant are 1 mol / L, 0.1 mol / L and 0.3 mol / L, and the secondary mixed solution is subjected to a second precipitation reaction at 25°C for 180 min to obtain antimony bismuth indium precursor material, and the temperature is increased to 550°C at a heating rate of 5°C / min and sintered for 3 h to obtain antimony bismuth indium oxide with a hollow three-dimensional structure;

[0136] (4) mixing antimony bismuth indium oxide, a selenium source (sodium selenide), a second reducing agent (hydrazine hydrate) and N,N-dimethylformamide, wherein the molar ratio of antimony bismuth indium oxide to the selenium source is 1:10, and the molar ratio of the second reducing agent to the selenium source is 0.5:1, and performing a hydrothermal reaction at 180° C. for 8 hours to obtain a hydrothermal reaction product;

[0137] (5) The hydrothermal reaction product and glucose were dispersed in deionized water at a mass ratio of 1:0.1, transferred to a hydrothermal kettle, and subjected to hydrothermal reaction at 200° C. for 12 hours. After the reaction was completed, the precipitate was filtered and washed to obtain the selenide sodium ion negative electrode material.

[0138] Example 5

[0139] The difference between this embodiment and embodiment 1 is that the side length of the hollow cube in this embodiment is 100 nm.

[0140] In the preparation method, the stirring time of the copper salt solution (CuCl2·2H2O) and the alkaline solution (sodium hydroxide) is regulated to be 10 minutes, and then the first reducing agent solution (ascorbic acid) is added to carry out an aging reaction at 30°C for 1.5 hours, and the molar ratio of copper in the copper salt, the alkaline substance in the alkaline solution and the reducing agent is 0.001:0.015:0.005 to obtain a Cu2O nanocube template (sacrificial template).

[0141] The rest of the preparation methods and parameters were the same as those in Example 1.

[0142] Example 6

[0143] The difference between this embodiment and embodiment 1 is that the side length of the hollow cube in this embodiment is 1.2 μm.

[0144] In the preparation method, the stirring time of the copper salt solution (CuCl2·2H2O) and the alkaline solution (sodium hydroxide) is regulated to be 4 hours, and then the first reducing agent solution (ascorbic acid) is added to carry out aging reaction at 30°C for 8 hours, and the molar ratio of copper in the copper salt, the alkaline substance in the alkaline solution and the reducing agent is 0.006:0.12:0.04, to obtain a Cu2O nanocube template (sacrificial template).

[0145] The rest of the preparation methods and parameters were the same as those in Example 1.

[0146] Example 7

[0147] The difference between this embodiment and embodiment 1 is that the surface of the antimony bismuth indium selenide material in this embodiment does not contain a carbon coating layer.

[0148] The carbon coating process of step (5) is not performed in the preparation method.

[0149] The rest of the preparation methods and parameters were the same as those in Example 1.

[0150] Comparative Example 1

[0151] The difference between this comparative example and Example 1 is that the selenide in this comparative example is antimony bismuth selenide, and the chemical formula is (Sb 1.1 Bi 0.9 )Se3.

[0152] In the preparation method, the coating process of the indium-containing compound in step (3) is not performed, and the hollow cubic structure of the antimony bismuth hydroxide is directly heated to 500° C. at a heating rate of 2° C. / min and sintered for 2 hours to obtain an antimony bismuth oxide with a hollow three-dimensional structure.

[0153] The rest of the preparation methods and parameters were the same as those in Example 1.

[0154] Comparative Example 2

[0155] The difference between this comparative example and Example 1 is that the selenide in this comparative example is antimony indium selenide, and the chemical formula is (Sb 1.1 In 0.9 )Se3.

[0156] In the preparation method, no bismuth salt is added in step (2).

[0157] The rest of the preparation methods and parameters were the same as those in Example 1.

[0158] Comparative Example 3

[0159] The difference between this comparative example and Example 1 is that the selenide in this comparative example is bismuth indium selenide, and the general chemical formula is (BiIn)Se3.

[0160] In the preparation method, no antimony salt is added in step (2).

[0161] The rest of the preparation methods and parameters were the same as those in Example 1.

[0162] Comparative Example 4

[0163] This comparative example provides a sodium selenide negative electrode material, wherein the sodium selenide negative electrode material comprises an antimony bismuth indium selenide material, and the surface of the antimony bismuth indium selenide material further comprises a carbon coating layer.

[0164] The preparation method is as follows:

[0165] (1) Antimony salt (SbCl3), bismuth salt (BiCl3), indium salt (InCl3), precipitant (sodium hydroxide), surfactant (polyvinyl pyrrolidone) and deionized water are mixed, wherein the concentration of antimony salt is 0.08 mol / L, the concentration of bismuth salt is 0.06 mol / L, the concentration of indium salt is 0.06 mol / L, and the concentration of precipitant is 1 mol / L, and the mixed solution is subjected to precipitation reaction at 25°C for 60 minutes to obtain an antimony indium hydroxide precursor material;

[0166] (2) heating the mixture to 500° C. at a heating rate of 2° C. / min and sintering for 2 h to obtain antimony bismuth indium oxide;

[0167] (3) Antimony bismuth indium oxide, a selenium source (sodium selenide), a second reducing agent (hydrazine hydrate) and N,N-dimethylformamide are mixed, the molar ratio of antimony bismuth indium oxide to the selenium source is 1:1.5, the molar ratio of the second reducing agent to the selenium source is 0.03:1, and a hydrothermal reaction is carried out at 150° C. for 6 hours to obtain a hydrothermal reaction product

[0168] (4) The hydrothermal reaction product and glucose were dispersed in deionized water at a mass ratio of 1:0.1, transferred to a hydrothermal kettle, and subjected to hydrothermal reaction at 200° C. for 12 hours. After the reaction was completed, the precipitate was filtered and washed to obtain the selenide sodium ion negative electrode material.

[0169] The selenide negative electrode materials provided in Examples 1-7 and Comparative Examples 1-4 are respectively used as negative electrode active materials, polyacrylic acid is used as a binder, acetylene black is used as a conductive agent, and N-methylpyrrolidone is used as a solvent, and the mass ratio of the negative electrode active material, the binder, and the conductive agent is 80:5:15; the binder is added to N-methylpyrrolidone, stirred for 1 hour, and then the negative electrode active material and the conductive agent are added, stirred for 1 hour to obtain a negative electrode slurry, which is coated on a copper foil, dried at 65° C. for 8 hours, and sliced ​​to obtain a negative electrode sheet;

[0170] A CR2025 button-type sodium-ion battery was assembled using a sodium sheet as the counter electrode and a sodium hexafluorophosphate solution as the electrolyte.

[0171] The sodium ion batteries provided in Examples 1-7 and Comparative Examples 1-4 were subjected to performance tests under the following test conditions:

[0172] At 200mA·g -1The charge and discharge test was carried out at a current density of , and the capacity and cycle capacity retention rate obtained at the 1st cycle and 500th cycle were obtained. The test results are shown in Table 1.

[0173] Table 1

[0174]

[0175]

[0176] The sodium ion batteries provided by Examples 1-7 and Comparative Examples 1-4 were subjected to rate performance tests: charge and discharge tests were performed at different current densities to obtain capacity retention rates, and the test conditions and results are shown in Table 2.

[0177] Table 2

[0178]

[0179]

[0180] From Table 1 and Table 2, we can get:

[0181] From the data results of Examples 1-4, it can be seen that the antimony bismuth indium selenide with a specific hollow cubic structure provided by the present invention as a negative electrode material for a sodium ion battery not only has a high energy density and excellent cycle stability, but also has excellent rate performance.

[0182] From the data results of Example 1, Example 5 and Example 6, it can be seen that if the side length of the hollow cube structure is too short, it will cause particle agglomeration and affect battery performance, while if it is too long, the structure will be too large, which may easily lead to structural collapse during electrochemical reactions. By adjusting the side length to 200nm~1μm, a sodium ion selenide negative electrode material with better performance and more stable structure is obtained.

[0183] From the data results of Example 1 and Example 7, it can be seen that in the sodium ion selenide negative electrode material provided by the present invention, further carbon coating of antimony bismuth indium selenide can better achieve a higher capacity retention rate under high rate charge and discharge.

[0184] From the data results of Example 1 and Comparative Examples 1-4, it can be seen that in the present invention, the synergistic combination of antimony, bismuth and indium elements and the special morphology of the specific heterojunction structure must exist at the same time to solve the problems of poor rate performance of selenide and rapid capacity decay due to large structural expansion.

[0185] In summary, the selenide sodium ion negative electrode material provided by the present invention is composed of antimony, bismuth, and indium selenide materials and has a stable nano hollow cubic structure, in which the metal elements and morphology cooperate with each other, wherein the hollow structure can not only reduce the mechanical stress during the electrochemical reaction, alleviate its own expansion, and ensure the structural stability, but also provide more active sites to improve Na storage; in addition, the selenides of antimony, bismuth, and indium produce a unique interface effect by coupling nanomaterials with different band gaps, which can further improve the surface reaction kinetics, promote the diffusion rate of sodium ions in the solid, and improve the intrinsic conductivity, capacity, and rate performance.

[0186] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A sodium selenide negative electrode material, characterized in that: The selenide sodium ion negative electrode material includes antimony bismuth indium selenide material, and the morphology of the antimony bismuth indium selenide material is a hollow cubic structure.

2. The sodium selenide negative electrode material according to claim 1, characterized in that: The antimony bismuth indium selenide comprises a heterojunction structure composed of antimony selenide, bismuth selenide and indium selenide, and the heterojunction structure is a hollow cubic structure; Preferably, the chemical formula of the antimony bismuth indium selenide material is (Sb x Bi y In 2-x-y )Se3, where 0<x+y<2; Preferably, the specific surface area of ​​the antimony bismuth indium selenide material is 50 m 2 / g~300m 2 / g; Preferably, in the hollow cubic structure, the side length of the cube is 200 nm to 1 μm; Preferably, the surface of the antimony bismuth indium selenide material further includes a carbon coating layer.

3. A method for preparing the sodium selenide negative electrode material according to claim 1 or 2, characterized in that: The preparation method comprises the following steps: The sacrificial template, antimony salt, bismuth salt, etchant, precipitant and first solvent are mixed at one time, and a first precipitation reaction is performed to obtain an antimony-bismuth hollow cubic structure; The surface of the hollow cubic structure of antimony bismuth is coated with an indium compound, and sintered to obtain an antimony bismuth indium oxide with a hollow three-dimensional structure; The antimony bismuth indium oxide is subjected to a selenization reaction with a selenium source to obtain the selenide sodium ion negative electrode material.

4. The preparation method according to claim 3, characterized in that: The sacrificial template includes a Cu2O nanocube template; Preferably, the method for preparing the Cu2O nanocube template comprises: Mixing and reacting the copper salt, the alkaline solution and the first reducing agent solution to obtain the Cu2O nanocube template; Preferably, the mixing reaction method comprises: stirring the copper salt solution and the alkaline solution at one time, and then adding the reducing agent solution to carry out an aging reaction; Preferably, the molar ratio of the copper in the copper salt, the alkaline substance in the alkaline solution and the reducing agent is (0.001-0.005):(0.02-0.1):(0.006-0.03); Preferably, the stirring time is 0.5 to 3 hours; Preferably, the temperature of the aging reaction is 25° C. to 50° C., and the time of the aging reaction is 2 to 6 hours.

5. The preparation method according to claim 3 or 4, characterized in that: The raw materials mixed once also include a surfactant; Preferably, the concentration of the sacrificial template in the solution after the first mixing is 0.01 mol / L to 2 mol / L; Preferably, the concentration of the antimony salt in the solution after the first mixing is 0.01 mol / L to 1 mol / L; Preferably, the concentration of the bismuth salt in the solution after the first mixing is 0.01 mol / L to 1 mol / L; Preferably, the concentration of the etchant in the solution after the first mixing is 0.5 mol / L to 3 mol / L; Preferably, the concentration of the precipitant in the solution after the first mixing is 0.5 mol / L to 4 mol / L; Preferably, the etchant comprises thiosulfate; Preferably, the temperature of the first precipitation reaction is 25°C to 50°C, and the time of the first precipitation reaction is 10 to 180 minutes.

6. The preparation method according to any one of claims 3 to 5, characterized in that: The coating method of the indium-containing compound comprises: The antimony-bismuth hollow cubic structure, indium salt, complex precipitant and second solvent are mixed for a second time, and a second precipitation reaction is performed to obtain an antimony-bismuth-indium precursor material; Preferably, the secondary mixed raw materials further include a surfactant; Preferably, the concentration of the antimony-bismuth hollow cubic structure in the secondary mixed solution is 0.01 mol / L to 0.5 mol / L; Preferably, the concentration of the indium salt in the solution after secondary mixing is 0.01 mol / L to 1 mol / L; Preferably, the concentration of the complexing precipitant in the solution after secondary mixing is 0.01 mol / L to 4 mol / L; Preferably, the temperature of the second precipitation agent reaction is 25°C to 50°C, and the time of the second precipitation reaction is 10 to 180 minutes; Preferably, the heating rate of the sintering is 1 to 10°C / min; Preferably, the sintering temperature is 400-600° C., and the sintering time is 1-5 hours.

7. The preparation method according to any one of claims 3 to 6, characterized in that: The molar ratio of the antimony bismuth indium oxide to the selenium source is 1:(1-10); Preferably, the selenization reaction comprises: The antimony bismuth indium oxide, the selenium source, the second reducing agent and the third solvent are mixed and subjected to a solvothermal reaction to obtain a solvothermal reaction product; Preferably, the molar ratio of the second reducing agent to the selenium source is (0.01-0.5):1; Preferably, the temperature of the solvent thermal reaction is 50 to 200° C., and the time of the solvent thermal reaction is 1 to 24 hours.

8. The preparation method according to any one of claims 3 to 7, characterized in that: Carrying out carbon coating treatment on the product of the solvothermal reaction; Preferably, the mass ratio of the product of the solvothermal reaction to the carbon source is 1:(0.01-0.5).

9. The preparation method according to any one of claims 3 to 8, characterized in that: The preparation method comprises the following steps: The copper salt solution and the alkaline solution are stirred for 0.5 to 3 hours at a time, and then the first reducing agent solution is added for aging reaction for 2 to 6 hours, and the molar ratio of copper in the copper salt, the alkaline substance in the alkaline solution and the reducing agent is (0.001 to 0.005): (0.02 to 0.1): (0.006 to 0.03) to obtain a Cu2O nanocube template; A Cu2O nanocube template, an antimony salt, a bismuth salt, an etchant, a precipitant, a surfactant and a first solvent are mixed once, wherein the concentration of the Cu2O nanocube template in the mixed solution is 0.01 mol / L to 2 mol / L, the concentration of the antimony salt in the mixed solution is 0.01 mol / L to 1 mol / L, the concentration of the bismuth salt in the mixed solution is 0.01 mol / L to 1 mol / L, the concentration of the etchant in the mixed solution is 0.5 mol / L to 3 mol / L, the concentration of the precipitant in the mixed solution is 0.5 mol / L to 4 mol / L, and the first precipitation reaction is performed for 10 to 180 min to obtain an antimony-bismuth hollow cubic structure; The antimony bismuth hollow cubic structure, indium salt, complex precipitant, surfactant and second solvent are mixed twice, wherein the concentration of the antimony bismuth hollow cubic structure in the solution after the second mixing is 0.01mol / L to 0.5mol / L, the concentration of the indium salt in the solution after the second mixing is 0.01mol / L to 1mol / L, and the concentration of the complex precipitant in the solution after the second mixing is 0.01mol / L to 4mol / L, the second precipitation reaction is 10 to 180min to obtain an antimony bismuth indium precursor material, and the temperature is increased to 400 to 600°C at a heating rate of 1 to 10°C / min and sintered for 1 to 5h to obtain an antimony bismuth indium oxide with a hollow three-dimensional structure; Mixing antimony bismuth indium oxide, a selenium source, a second reducing agent and a third solvent, wherein the molar ratio of antimony bismuth indium oxide to the selenium source is 1:(1-10), and the molar ratio of the second reducing agent to the selenium source is (0.01-0.5):1, and performing a hydrothermal reaction at 50-200° C. for 1-24 hours to obtain a hydrothermal reaction product; The product of the hydrothermal reaction is subjected to carbon coating treatment to obtain the selenide sodium ion negative electrode material.

10. A sodium ion battery, characterized in that: The sodium ion battery comprises the selenide sodium ion negative electrode material as described in claim 1 or 2 or the selenide sodium ion negative electrode material prepared by the preparation method as described in any one of claims 3-9.