Dynamic crosslinking moisture absorption hydrogel and preparation method thereof

Through the reversible crosslinking network of dynamic cross-linking hygroscopic gel, the problem of salt solution leakage during hygroscopic absorption is solved, efficient hygroscopic absorption and stability are achieved, and it is suitable for a variety of applications.

CN119039725AActive Publication Date: 2024-11-29INST OF URBAN ENVIRONMENT CHINESE ACAD OF SCI

Patent Information

Application Number
CN202411379732.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-29
Estimated Expiration
2044-09-30

AI Technical Summary

Technical Problem

The existing hygroscopic hydrogels have a salt solution leakage problem during the hygroscopic process, resulting in a degradation of hygroscopic performance. The existing solutions are complex and cannot completely solve the phase separation problem between the salt solution and the polymer.

Method used

Using dynamic crosslinked hygroscopic gel, the dynamic crosslinking network dissociates with the increase of water content through the reversible reaction of borate ester bonds, prevents the leakage of salt solution and improves hygroscopic kinetics.

Benefits of technology

It realizes that there is no leakage of salt solution during the hygroscopic absorption process, which improves moisture absorption and stability. The hygroscopic/desorption kinetics of dynamic crosslinked hydrogels are faster than those of covalent crosslinked hydrogels, and the preparation process is simple and applicable In applications such as solar air water collection and dehumidification in confined spaces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039725A_ABST
    Figure CN119039725A_ABST
Patent Text Reader

Abstract

The invention relates to a dynamic crosslinking moisture absorption hydrogel and a preparation method thereof. The raw materials comprise a hydroxyl-containing water-soluble polymer material, a boric acid cross-linking agent and a moisture absorption salt material. The preparation method comprises the steps of preparation of a gel precursor solution, preparation of a cross-linking agent solution, a cross-linking reaction process and a process of putting into a mold for gelatinization. The crosslinking sites of boric acid ester bonds in the hydrogel can be subjected to reversible hydrolysis reaction, and the crosslinking density of the dynamic hydrogel is determined by the water content in the hydrogel. Compared with the conventional covalent bond cross-linked moisture absorption hydrogel, the dynamic cross-linked moisture absorption hydrogel with the characteristics has the characteristics of higher moisture absorption salt loading capacity and moisture absorption capacity, faster moisture absorption / desorption dynamic performance, easiness in recovery and regeneration and easiness in large-scale production. The invention further discloses specific application of the dynamic crosslinking moisture absorption hydrogel. The specific application comprises air water collection based on solar energy, drying and dehumidification in a closed space, evaporation and heat dissipation and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hygroscopic gel, and in particular to a dynamic cross-linked hygroscopic hydrogel and a preparation method and application thereof. Background Art

[0002] Water vapor in the air is an important resource in nature. Many technologies have emerged, such as air water collection technology, evaporative heat dissipation technology, and moisture power generation technology, to effectively develop and utilize water vapor in the air. In order to realize the utilization of water vapor in the air, hygroscopic hydrogel has become one of the core materials in the technology of utilizing air water vapor due to its advantages such as large moisture absorption capacity and fast moisture absorption rate (Advanced Materials, 2022,34, 2110079.). Most of the hygroscopic hydrogels that have been reported use hydrophilic polymer networks as carriers, and hygroscopic salts are the main hygroscopic components dispersed in the polymer network. Invention patent CN 108059783 B discloses a hygroscopic hydrogel with sodium acrylate as a polymer carrier and magnesium chloride as the main active component for hygroscopicity. Invention patent CN 111363284 B discloses a composite hygroscopic gel material with a core-shell structure doped with hygroscopic salts. However, the above materials all have the problem of leakage of hygroscopic salt solutions during the hygroscopic process. This is because the polymer substrate used in most existing hygroscopic hydrogels is an irreversibly covalently cross-linked hydrogel material. This type of hygroscopic salt-based hydrogel has the risk of salt solution leakage during the hygroscopic process, that is, the rapid deliquescence of the salt causes the salt solution to separate from the hydrogel material, which reduces the performance of the hygroscopic material.

[0003] In order to prevent the leakage of salt solution, a porous structure is usually used to confine the salt solution inside the hygroscopic material, but due to the blockage of the hygroscopic solution, the hygroscopic dynamics decreases. The invention patent with application publication number CN 116693928 A discloses a method for preparing macroporous hygroscopic hydrogels using an ice template method, which accelerates the kinetics of porous structure hygroscopic hydrogels to a certain extent. In some other research works, the leakage of salt solution is prevented by wrapping the surface of porous structure hygroscopic materials with a breathable hydrophobic layer (Cell Reports Physical Science 2021, 2 (12), 100664.). However, the preparation process of the above method is relatively complicated, which increases the resistance to diffusion during the hygroscopic process, and does not solve the problem of phase separation between the salt solution and the polymer.

[0004] In view of the above prior art, in order to ensure that the hygroscopic gel has sufficient hygroscopic capacity and stability in application, it is necessary to fundamentally solve the problem of salt leakage of the hygroscopic gel material. Therefore, it is necessary to find a technical solution to ensure the hygroscopic performance of the material while effectively preventing the leakage of the salt solution during use of the hygroscopic gel. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the present invention provides a method for preparing a dynamic hydrogel. Based on the reversible reaction between the cross-linking sites of the dynamic cross-linked hygroscopic gel and water, the degree of cross-linking of the dynamic cross-linked hygroscopic gel is related to its water content. When the internal water content of the dynamic cross-linked hygroscopic gel is large, the cross-linking sites are correspondingly reduced, and the dynamic network changes from dense to sparse, which can swell more water. Therefore, the dynamic cross-linked hydrogel disclosed in the present invention can fundamentally solve the problem of salt leakage of the hygroscopic hydrogel. Secondly, due to the variability of the cross-linked network, as the water content of the dynamic cross-linked network increases, the diffusion of water in the dynamic cross-linked network is enhanced. Therefore, compared with other patents disclosing covalently cross-linked hygroscopic hydrogels, the dynamic cross-linked hydrogel disclosed in the present invention has faster moisture absorption dynamics.

[0006] A method for preparing a dynamically cross-linked hygroscopic gel, characterized in that it comprises the following steps:

[0007] (1) A hydroxyl-containing water-soluble polymer material is heated and dissolved in water. After cooling to room temperature, a hygroscopic salt is added and stirred to dissolve to obtain a precursor solution of a gel.

[0008] (2) Dissolve a boric acid cross-linking agent in water at room temperature to obtain a cross-linking agent solution.

[0009] (3) The precursor solution of the gel obtained in step (1) is heated to a high temperature, and a crosslinking agent solution is slowly added dropwise to the precursor solution of the gel under rapid stirring to carry out a crosslinking reaction process, thereby obtaining a low crosslinking degree gel that maintains a certain fluidity.

[0010] (4) Drying and dehydrating the low cross-linking degree gel obtained in step (3) to increase the cross-linking degree of the material and obtain a dynamically cross-linked hygroscopic hydrogel.

[0011] The present invention utilizes borate ester bonds as dynamic crosslinking sites, which can undergo a reversible reaction with water at room temperature and dissociate into boric acid and alcohol. When the salt rapidly deliquesces, the dynamic crosslinking network rapidly dissociates, allowing the salt solution to quickly diffuse into the interior of the gel and maintain the uniformity of the gel. As the water content increases, the dynamic crosslinked hydrogel disclosed in the present invention will not have the problem of salt solution leakage caused by the moisture absorption exceeding the maximum swelling capacity of the crosslinked network. Therefore, the dynamic crosslinked hydrogel disclosed in the present invention can achieve a salt loading that exceeds the polymer mass by several times, and ensure high stability during the moisture absorption-desorption cycle.

[0012] Preferably, in step (1), the hydroxyl-containing water-soluble polymer material is one of polyvinyl alcohol, poly(2,3-dihydroxypropyl acrylate), and poly(2-methyl-2-acrylate-2,3-dihydroxypropyl ester).

[0013] Preferably, in step (1), the hygroscopic salt is one of lithium chloride, calcium chloride, sodium sulfate, sodium chloride and magnesium chloride.

[0014] Preferably, in step (1), the concentration of the hydroxyl-containing water-soluble polymer material in the precursor solution is 2-15 wt.%.

[0015] Preferably, in step (1), the mass ratio of the polymer to the hygroscopic salt is 1 / 1 to 1 / 10.

[0016] Preferably, in step (2), the boric acid cross-linking agent is one of sodium borate decahydrate or boric acid.

[0017] Preferably, in step (2), the concentration of the cross-linking agent solution is 0.1-5.0 wt.%.

[0018] Since borate bonds tend to decompose into boric acid and alcohol at high temperatures, the degree of crosslinking of the dynamically crosslinked hydrogel decreases with increasing temperature under the same water content. In order to ensure that the crosslinking points are evenly distributed in the dynamically crosslinked hygroscopic hydrogel, it is necessary to maintain a suitable temperature during the crosslinking reaction.

[0019] Preferably, in step (3), the temperature of the cross-linking process is 60-100°C, the stirring speed is 500-1000 rpm, and the reaction time is 2-10 h.

[0020] Preferably, in step (4), the drying temperature is 80-100°C and the drying time is 12-20 h.

[0021] The present invention also provides a photothermal dynamic hygroscopic hydrogel prepared by the above method, which is used for solar air water collection. By adding a photothermal material to the dynamic cross-linked hygroscopic hydrogel, water in the dynamic hygroscopic hydrogel can be removed by solar energy. In order to ensure that the photothermal material is evenly dispersed in the dynamic cross-linked hydrogel, it is necessary to mix after the prepared hydrogel contains a certain amount of water.

[0022] Preferably, the photothermal material used to prepare the photothermal dynamic hydrogel is one of carbon powder, carbon nanotubes and graphite powder.

[0023] Preferably, when the photothermal material is mixed into the dynamically cross-linked hygroscopic hydrogel, the water content of the dynamically cross-linked hygroscopic hydrogel is 50-70 wt%.

[0024] Preferably, the amount of photothermal material mixed into the dynamically cross-linked hygroscopic hydrogel is 0.5-5 wt%.

[0025] The photothermal dynamic cross-linked hygroscopic hydrogel of the present invention can achieve photothermal conversion under the intensity of 1 sun, and achieve rapid desorption and water production. Due to its excellent kinetic properties, the photothermal dynamic hydrogel of the present invention can achieve multiple adsorption and desorption cycles within a day, and the whole process does not require any other form of energy input.

[0026] The dynamic cross-linked hygroscopic hydrogel of the present invention can also be used in the fields of dehumidification and evaporative heat dissipation in closed spaces.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The borate dynamic cross-linking structure used in the present invention gives the dynamic cross-linked hydrogel the property of changing the degree of cross-linking according to the amount of moisture absorption, so that the dynamic cross-linked hygroscopic hydrogel can swell in time during the moisture absorption process, effectively eliminating the salt solution leakage problem that is common in hygroscopic hydrogels.

[0029] (2) The dynamically cross-linked hygroscopic hydrogel prepared by the present invention can automatically change the polymer network from dense to sparse during the continuous moisture absorption process, thereby improving the diffusion rate of water in the dynamically cross-linked hygroscopic hydrogel, making the moisture absorption / desorption kinetics of the dynamically cross-linked hygroscopic hydrogel faster than that of the covalently cross-linked hygroscopic hydrogel.

[0030] (3) The preparation process of the dynamic cross-linked hygroscopic hydrogel designed by the present invention is simple, the raw materials are widely available, and the preparation process does not involve expensive experimental equipment, which has good prospects for large-scale preparation.

[0031] (4) The dynamically cross-linked hydrogel prepared by the present invention can easily separate hygroscopic salts and polymers due to its reversible cross-linking sites. When the material completes its application life cycle, the raw materials can be easily recycled and reused, which is conducive to sustainable development.

[0032] (5) The dynamically cross-linked hydrogel prepared by the present invention has good plasticity and can be coated on various material substrates. It can be widely used in applications such as solar air water collection, dehumidification of enclosed spaces, and evaporative heat dissipation. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic diagram of the principle of the dynamically cross-linked hygroscopic hydrogel of the present invention.

[0034] Figure 2 The figures are the performance diagrams of the dynamic cross-linked hygroscopic hydrogel prepared in Example 1 in preventing salt leakage; wherein, (1) is a photograph of the dynamic cross-linked hygroscopic hydrogel after saturation with moisture, and (2) is a photograph of the conventional covalently cross-linked hygroscopic hydrogel after saturation with moisture.

[0035] Figure 3This is the moisture absorption kinetic curve of the dynamically cross-linked hygroscopic hydrogel prepared in Example 1 at 90% RH and 25°C; wherein 1 is the moisture absorption curve of the dynamically cross-linked hygroscopic hydrogel, and 2 is the moisture absorption curve of the conventional covalently cross-linked hygroscopic hydrogel.

[0036] Figure 4 It is the moisture absorption of the dynamically cross-linked hygroscopic hydrogel prepared in Example 1 at various humidity levels at 25°C.

[0037] Figure 5 This is the moisture absorption-solar desorption curve of the dynamically cross-linked hygroscopic hydrogel doped with carbon nanotube powder prepared in Example 4 (70% RH, 25°C, 1 sun intensity). DETAILED DESCRIPTION

[0038] The following further explains the technical solution of the present invention in combination with several embodiments and drawings, but the experimental conditions and setting parameters therein should not be regarded as limiting the basic technical solution of the present invention. And the protection scope of the present invention is not limited to the following embodiments.

[0039] The embodiment of the present invention realizes the preparation of the dynamic cross-linked hygroscopic hydrogel by adjusting the concentration of the polymer solution, the amount of the cross-linking agent added, the type of the hygroscopic salt, the ratio of the polymer to the hygroscopic salt, the amount of the photothermal conversion material added, etc.

[0040] Example 1

[0041] The steps for preparing the dynamically cross-linked hygroscopic hydrogel of this embodiment are as follows:

[0042] (1) To prepare a 4 wt % polyvinyl alcohol aqueous solution, polyvinyl alcohol was heated at 90° C. and dissolved in water. After cooling to room temperature, 16 wt % lithium chloride was added and stirred to dissolve, thereby obtaining a precursor solution of a gel.

[0043] (2) Sodium borate decahydrate crosslinking agent was dissolved in water at room temperature to prepare a 0.8 wt % crosslinking agent solution.

[0044] (3) The precursor solution of the gel was heated to 70°C, and the crosslinking agent solution was slowly added to the precursor solution of the gel under rapid stirring to carry out the crosslinking reaction process, thereby obtaining a low crosslinking degree gel that maintained a certain fluidity. The amount of crosslinking agent added was 2 wt% of the polymer mass.

[0045] (4) The obtained low cross-linked gel is poured into a mold and dried and dehydrated at 90°C for 12 h to increase the cross-linking degree of the material and obtain a dynamically cross-linked hygroscopic hydrogel.

[0046] The salt solution leakage resistance, moisture absorption kinetic curve, moisture absorption amount and other properties of this embodiment are characterized.

[0047] Figure 2 The following are photos of the dynamic cross-linked hygroscopic hydrogel prepared in this embodiment case after absorbing moisture to saturation at 90% RH and 25°C. It can be seen that in Figure (1), the dynamic cross-linked hygroscopic hydrogel presents a complete gel state after saturation and no salt solution leaks out. Figure (2) is a photo of the covalently cross-linked hygroscopic hydrogel cross-linked with glutaraldehyde. After the two hydrogels are saturated with moisture, the dynamic cross-linked hygroscopic hydrogel film maintains a complete gel state, while the bottom gel film of the covalently cross-linked hygroscopic hydrogel remains intact, and obvious salt solution precipitation occurs on the gel surface and gathers at the bottom of the culture dish.

[0048] Figure 3 The moisture absorption kinetic curve of the dynamically cross-linked hygroscopic hydrogel prepared for this embodiment at 90% RH and 25°C, Curve 1 is the curve of the dynamically cross-linked hygroscopic hydrogel, and Curve 2 is the kinetic curve of the covalently cross-linked hygroscopic hydrogel. By comparing the two, it can be clearly seen that in the middle and later stages of the moisture absorption process, the moisture absorption rate of the dynamically cross-linked hygroscopic hydrogel is significantly higher than that of the covalently cross-linked hygroscopic hydrogel.

[0049] Figure 4 The saturated moisture absorption of the dynamically cross-linked hygroscopic hydrogel prepared in this embodiment at different humidity conditions is 25°C. At relative humidity of 30%, 40%, 50%, 60%, 70%, 80%, and 90%, the moisture absorption capacity can reach 1.02, 1.51, 1.73, 2.04, 2.43, 2.89, and 4.10 g / g, respectively.

[0050] Example 2

[0051] The steps for preparing the dynamically cross-linked hygroscopic hydrogel of this embodiment are as follows:

[0052] (1) To prepare a 4 wt% polyvinyl alcohol aqueous solution, polyvinyl alcohol was heated at 90°C and dissolved in water. After cooling to room temperature, 16 wt% calcium chloride was added and stirred to dissolve, thereby obtaining a gel precursor solution.

[0053] Sodium borate decahydrate crosslinking agent was dissolved in water at room temperature to prepare a 0.8 wt % crosslinking agent solution.

[0054] The precursor solution of the gel was heated to 80 °C, and the crosslinking agent solution was slowly added to the precursor solution of the gel under rapid stirring to carry out the crosslinking reaction process, thereby obtaining a low crosslinking degree gel with a certain fluidity. The amount of crosslinking agent added was 2 wt% of the polymer mass.

[0055] The obtained low cross-linked gel was poured into a mold and dried and dehydrated at 90 °C for 12 h to increase the cross-linking degree of the material and obtain a dynamically cross-linked hygroscopic hydrogel.

[0056] Example 3

[0057] The steps for preparing the dynamically cross-linked hygroscopic hydrogel of this embodiment are as follows:

[0058] (1) To prepare a 4 wt% polyvinyl alcohol aqueous solution, polyvinyl alcohol was heated at 90°C and dissolved in water. After cooling to room temperature, 8 wt% lithium chloride was added and stirred to dissolve, thereby obtaining a precursor solution of a gel.

[0059] (2) Dissolve the boric acid crosslinker in water at room temperature to prepare a 0.8 wt % crosslinker solution.

[0060] (3) The precursor solution of the gel was heated to 80 °C, and the crosslinking agent solution was slowly added to the precursor solution of the gel under rapid stirring to carry out the crosslinking reaction process, thereby obtaining a low crosslinking gel that maintained a certain fluidity. The amount of crosslinking agent added was 4 wt% of the polymer mass.

[0061] (4) The obtained low cross-linked gel was poured into a mold and dried and dehydrated at 90 °C for 12 h to increase the cross-linking degree of the material and obtain a dynamically cross-linked hygroscopic hydrogel.

[0062] Example 4

[0063] In order to realize desorption of the dynamically cross-linked hygroscopic hydrogel under sunlight irradiation, it is necessary to mix the photothermal material into the dynamically cross-linked hygroscopic hydrogel. The preparation steps of the dynamically cross-linked hygroscopic hydrogel in this embodiment are as follows:

[0064] (1) To prepare a 4 wt% polyvinyl alcohol aqueous solution, polyvinyl alcohol was heated at 90°C and dissolved in water. After cooling to room temperature, 16 wt% lithium chloride was added and stirred to dissolve, thereby obtaining a precursor solution of a gel.

[0065] (2) Sodium borate decahydrate crosslinking agent was dissolved in water at room temperature to prepare a 0.8 wt % crosslinking agent solution.

[0066] (3) The precursor solution of the gel was heated to 70 °C, and the crosslinking agent solution was slowly added to the precursor solution of the gel under rapid stirring to carry out the crosslinking reaction process, thereby obtaining a low crosslinking gel that maintained a certain fluidity. The amount of crosslinking agent added was 2 wt% of the polymer mass.

[0067] (4) The obtained low cross-linked gel was poured into a mold and dried and dehydrated at 90 °C for 12 h to increase the cross-linking degree of the material and obtain a dynamically cross-linked hygroscopic hydrogel.

[0068] (5) The dried hygroscopic hydrogel can be rehydrated to a water content of 2 g / g at 70% RH and 25°C.

[0069] (6) 1 wt% of carbon nanotube powder is mixed into the hygroscopic hydrogel so that the carbon nanotube powder is dispersed in the hygroscopic hydrogel.

[0070] (7) The obtained carbon nanotube-doped dynamically cross-linked hygroscopic hydrogel was heated to 260 g / m 2 The surface density is coated on a metal substrate to form a dynamic cross-linked hygroscopic hydrogel adsorption bed.

[0071] The adsorption and desorption characterization of the carbon nanotube-doped dynamically cross-linked hygroscopic hydrogel prepared in this case was carried out.

[0072] Figure 5 The moisture absorption-solar desorption curve of the carbon nanotube-doped dynamically cross-linked hygroscopic hydrogel adsorption bed prepared in this case at 25°C, 70%RH and 25°C, 50%RH, 1 sun. It can complete an adsorption-desorption cycle within 4 hours and achieve 450g / m 2 of water collection.

[0073] Comparative Case 1

[0074] The preparation steps of the covalently cross-linked hygroscopic hydrogel in this comparative case are as follows:

[0075] (1) To prepare a 4 wt% polyvinyl alcohol aqueous solution, polyvinyl alcohol was heated at 90°C and dissolved in water. After cooling to room temperature, 16 wt% lithium chloride was added and stirred to dissolve, thereby obtaining a precursor solution of a gel.

[0076] (2) Dissolve glutaraldehyde crosslinker in water at room temperature to prepare a 2.5 wt% crosslinker solution.

[0077] (3) The precursor solution of the gel was heated to 70°C, and 1 wt% acetic acid was first added as a catalyst to the precursor solution of the gel under rapid stirring, and then the crosslinking agent solution was slowly added to carry out the crosslinking reaction process. To ensure that the molar amount of the crosslinking agent was consistent with that of the dynamically crosslinked hydrogel, the amount of the crosslinking agent added was 3.33 wt% of the polymer mass, thereby obtaining an incompletely reacted covalently crosslinked hydrogel.

[0078] (4) The unreacted covalently cross-linked hydrogel was poured into a mold and dried at 90 °C for 12 h to increase the degree of cross-linking of the material and obtain a covalently cross-linked hygroscopic hydrogel.

Claims

1. A dynamically cross-linked hygroscopic gel, characterized in that: The dynamic hydrogel is composed of a polymer network dynamically cross-linked by borate bonds and hygroscopic salts. The cross-linking points of the dynamic network can undergo a reversible hydrolysis reaction at room temperature, thereby achieving automatic adjustment of the degree of cross-linking during the moisture absorption process. When the water content inside the dynamic cross-linked hygroscopic gel is high, the cross-linking sites are reduced accordingly, and the dynamic network becomes sparse from dense, thereby being able to swell with more water.

2. A method for preparing a dynamically cross-linked hygroscopic hydrogel, characterized in that: Its preparation comprises the following steps: (1) The hydroxyl-containing water-soluble polymer material is heated and dissolved in water, and after cooling to room temperature, a hygroscopic salt is added and stirred to dissolve to obtain a precursor solution of a gel; (2) dissolving sodium borate decahydrate crosslinking agent in water at room temperature to obtain a crosslinking agent solution; (3) heating the precursor solution of the gel obtained in step (1) and slowly adding a crosslinking agent solution to the precursor solution of the gel under rapid stirring to carry out a crosslinking reaction process to obtain a low crosslinking degree gel that maintains a certain fluidity; (4) Drying and dehydrating the low cross-linking degree gel obtained in step (3) to increase the cross-linking degree of the material and obtain a dynamically cross-linked hygroscopic hydrogel.

3. The preparation method according to claim 2, characterized in that: In step (1), the hydroxyl-containing water-soluble polymer material is polyvinyl alcohol, and the hygroscopic salt is a hygroscopic salt such as lithium chloride, magnesium chloride, sodium chloride, calcium chloride, sodium sulfate, etc., preferably lithium chloride.

4. The preparation method according to claim 2, characterized in that: In step (1), the concentration of the hydroxyl-containing water-soluble polymer material in the precursor solution is 2-15 wt.%, and the mass ratio of the polymer to the hygroscopic salt is 1 / 1-1 / 5.

5. The preparation method according to claim 2, characterized in that: In step (2), the boric acid cross-linking agent is sodium borate decahydrate or boric acid; the concentration of the cross-linking agent solution is 0.1-5.0 wt.%.

6. The preparation method according to claim 2, characterized in that: In step (3), heating is used to promote the exchange of borate cross-linking sites so that the cross-linking sites are evenly dispersed in the hydrogel. The temperature of the cross-linking process should be 60-100°C, the stirring speed should be 500-1000 rpm, and the reaction time should be 2-10 h.

7. The preparation method according to claim 2, characterized in that: In step (4), the drying temperature is 80-100°C and the drying time is 12-20 h.

8. When the dynamically cross-linked hygroscopic hydrogel prepared according to claims 2 to 6 is used for solar air water collection, a photothermal material can be mixed into the hydrogel, and the photothermal material is carbon nanotubes.

9. The dynamically cross-linked hygroscopic hydrogel prepared according to claims 2 to 6 can also be used in the field of dehumidification and evaporative heat dissipation in closed spaces.

Citation Information

Patent Citations

  • Photo-thermal moisture absorption polymer gel as well as preparation method and application thereof

    CN116693928A

  • Preparation method of novel polyvinyl alcohol conductive elastic aerogel

    CN116948242A

  • Highly water-absorptive resin composition

    JP1989033149A

Cited By

  • Anti-seepage active mineral drying agent and preparation method thereof

    CN122141423A

  • A water-vapor-resistant active mineral desiccant and a preparation method thereof

    CN122141423B