Preparation method of positive electrode material and energy storage battery

By combining iron-based metal-organic framework materials with lithium iron phosphate particles to form nitrogen-doped carbon nanotubes and a carbon coating layer, the problem of poor conductivity of lithium iron phosphate cathode materials was solved, and the electronic conductivity and lithium-ion diffusion rate were improved, thereby enhancing the overall performance of the battery.

CN119008910APending Publication Date: 2024-11-22ZHEJIANG JINKO ENERGY STORAGE CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411214830.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The poor conductivity of lithium iron phosphate cathode materials limits their further development in lithium-ion batteries.

Method used

By preparing iron-based metal-organic framework materials (Fe-MOF), nitrogen-doped bamboo-like carbon nanotubes are formed using cyanamide-based organic ligands, and a carbon coating layer is formed during high-temperature sintering. Combined with lithium iron phosphate particles and carbon nanotubes, a continuous three-dimensional conductive network is formed, which improves electronic conductivity and lithium-ion diffusion rate.

Benefits of technology

It significantly improves the electronic conductivity and lithium-ion diffusion rate of lithium iron phosphate cathode materials, eliminating the need for additional carbon sources and enhancing the battery's conductivity and energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008910A_ABST
    Figure CN119008910A_ABST
Patent Text Reader

Abstract

The embodiment of the invention relates to the technical field of batteries, and provides a preparation method of a positive electrode material and an energy storage battery, the method comprises the following steps: preparing an iron-based metal organic framework material, the preparation steps comprise: dispersing a first iron source in a solvent, adding a cyanamide organic ligand, and carrying out a reflux reaction to obtain a reaction liquid, cooling, filtering and washing the reaction liquid to obtain the iron-based metal organic framework material; grinding and blending the iron-based metal organic framework material, a second iron source, a lithium source and a phosphorus source to obtain a premix; and sintering the premix in an inert gas atmosphere to obtain the composite lithium iron phosphate positive electrode material, the composite lithium iron phosphate positive electrode material comprises lithium iron phosphate particles and a carbon nanotube, the lithium iron phosphate particles are attached to the surface of the carbon nanotube, and iron is coated in the carbon nanotube. According to the preparation method of the positive electrode material and the energy storage battery provided by the embodiment of the invention, the conductivity of the positive electrode material in the lithium iron phosphate battery is at least improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present application relate to the field of battery technology, and in particular to a method for preparing a positive electrode material and an energy storage battery. Background Art

[0002] With the development of lithium-ion battery research, the requirements for energy density, working voltage and cycle life are getting higher and higher. At present, the positive electrode materials of lithium-ion batteries mainly include lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, ternary materials, etc. Among them, lithium iron phosphate (LiFePO4) is widely used due to its advantages such as high capacity, environmental friendliness, high safety and long cycle life.

[0003] However, the inherent poor conductivity of lithium iron phosphate cathode materials has always been the main reason hindering its further development. Summary of the invention

[0004] The embodiments of the present application provide a method for preparing a positive electrode material and an energy storage battery, which are at least beneficial to improving the conductivity of the positive electrode material in a lithium iron phosphate battery.

[0005] According to some embodiments of the present application, on the one hand, the embodiments of the present application provide a method for preparing a positive electrode material, including: preparing an iron-based metal-organic framework material, the metal of the iron-based metal-organic framework material is iron, and the organic ligand is a cyanamide-type organic ligand, the preparation steps including: dispersing a first iron source in a solvent, adding a cyanamide-type organic ligand, performing a reflux reaction to obtain a reaction liquid, cooling, filtering and washing the reaction liquid to obtain the iron-based metal-organic framework material; grinding and blending the iron-based metal-organic framework material with a second iron source, a lithium source and a phosphorus source to obtain a premix; sintering the premix under an inert gas atmosphere to obtain a composite lithium iron phosphate positive electrode material, the composite lithium iron phosphate positive electrode material includes lithium iron phosphate particles and carbon nanotubes, the lithium iron phosphate particles are attached to the surface of the carbon nanotubes, and the carbon nanotubes are coated with iron.

[0006] In some embodiments, the first iron source and the second iron source are selected from one or more of ferric nitrate, ferric sulfate, ferric acetate, ferric phosphate, ferric chloride, ferrous perchlorate, ferrous phosphate, ferrous citrate, ferrous sulfate, ferrous acetate, ferrous nitrate, ferrous oxalate or ferrous fluoride.

[0007] In some embodiments, the cyanamide organic ligand is selected from one or more of melamine, dicyandiamide or cyanamide.

[0008] In some embodiments, in the step of preparing an iron-based metal organic framework material, the molar ratio of the cyanamide organic ligand to the first iron source is 0.2-1, the reflux reaction temperature is 80°C-180°C, and the reflux reaction time is 2h-24h.

[0009] In some embodiments, the specific surface area of ​​the iron-based metal organic framework material is 150 m 2 / g~1000m 2 / g.

[0010] In some embodiments, the particle shape of the iron-based metal organic framework material is a cuboid, and the length of the cuboid is 50-100 nm.

[0011] In some embodiments, before grinding and blending the iron-based metal-organic framework material with a second iron source, a lithium source, and a phosphorus source to obtain a premix, the process includes: blending the iron-based metal-organic framework material with a binder and water to obtain a mixture, and extruding the mixture into a preset shape; grinding and blending the iron-based metal-organic framework material with a second iron source, a lithium source, and a phosphorus source to obtain a premix includes: blending the mixture of a preset shape with a second iron source, a lithium source, and a phosphorus source to obtain a premix.

[0012] In some embodiments, the sintering temperature of the sintering process is 500° C. to 850° C., the heating rate is 1° C. / min to 10° C. / min, and the sintering time is 10 h to 24 h.

[0013] In some embodiments, the specific surface area of ​​the composite lithium iron phosphate positive electrode material is 5m 2 / g~60m 2 / g, when the cumulative particle size distribution percentage of the composite lithium iron phosphate positive electrode material reaches 50%, the corresponding particle size is 50nm~2000nm.

[0014] According to some embodiments of the present application, on the other hand, embodiments of the present application further provide an energy storage battery, including: a positive electrode sheet and a negative electrode sheet, and the material of the positive electrode sheet is manufactured using any of the preparation methods of the positive electrode material in the above embodiments.

[0015] The technical solution provided by the embodiments of the present application has at least the following advantages:

[0016] In the preparation method of the positive electrode material provided in the embodiment of the present application, the first iron source is reacted with the cyanamide organic ligand to prepare the iron-based metal organic framework material, and then the iron-based metal organic framework material is blended with the second iron source, the lithium source and the phosphorus source and sintered to obtain a composite lithium iron phosphate positive electrode material. The second iron source, the lithium source and the phosphorus source react to generate lithium iron phosphate particles, and the iron-based metal organic framework material is sintered to form carbon nanotubes coated with iron. In the microstructure, the lithium iron phosphate particles are attached to the surface of the carbon nanotubes. Among them, the ligand in the iron-based metal organic framework material is a cyanamide organic ligand, which will form nitrogen-doped bamboo-shaped carbon nanotubes after high-temperature sintering. The active site of iron is wrapped at the front end of the carbon nanotube, and the unique carbon wrapping structure can protect and fix the active site of iron to improve its stability. At the same time, the nitrogen-doped carbon nanotubes can provide efficient electron transmission channels to form a continuous three-dimensional conductive network. This structure can be beneficial to improve the electronic conductivity and lithium ion diffusion rate of the composite lithium iron phosphate positive electrode material. In addition, the carbon volatilized from cyanamide organic ligands during high-temperature sintering can be used as a carbon source to form a carbon coating on the surface of lithium iron phosphate particles without adding additional carbon sources. The carbon-coated lithium iron phosphate particles are beneficial to improving the conductivity of the composite lithium iron phosphate positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] One or more embodiments are exemplarily illustrated by the pictures in the corresponding drawings. These exemplified descriptions do not constitute a limitation on the embodiments. Unless otherwise specified, the pictures in the drawings do not constitute a scale limitation. In order to more clearly illustrate the embodiments of the present application or the technical solutions in the traditional technology, the drawings required for use in the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 A flowchart corresponding to a method for preparing a positive electrode material provided in an embodiment of the present application;

[0019] Figure 2 A scanning electron microscope image of a sintered Fe-MOF provided in an embodiment of the present application;

[0020] Figure 3 Cyclic performance test diagram of two energy storage batteries provided in the embodiments of the present application;

[0021] Figure 4 This is a DC impedance test diagram of two energy storage batteries provided in an embodiment of the present application. DETAILED DESCRIPTION

[0022] As known from the background technology, the conductivity of the positive electrode material in the lithium iron phosphate battery needs to be improved.

[0023] The embodiment of the present application provides a method for preparing a positive electrode material and an energy storage battery. In the method for preparing the positive electrode material, the first iron source is first reacted with a cyanamide organic ligand to prepare an iron-based metal organic framework material, and then the iron-based metal organic framework material is mixed with a second iron source, a lithium source and a phosphorus source and sintered to obtain a composite lithium iron phosphate positive electrode material. The second iron source, the lithium source and the phosphorus source react to generate lithium iron phosphate particles, and the iron-based metal organic framework material is sintered to form carbon nanotubes coated with iron. In terms of microstructure, the lithium iron phosphate particles are attached to the surface of the carbon nanotubes. Among them, the ligand in the iron-based metal organic framework material is a cyanamide organic ligand, which will form nitrogen-doped bamboo-shaped carbon nanotubes after high-temperature sintering. The active site of iron is wrapped at the front end of the carbon nanotube, and the unique carbon wrapping structure can protect and fix the active site of iron to improve its stability. At the same time, the nitrogen-doped carbon nanotubes can provide efficient electron transmission channels to form a continuous three-dimensional conductive network. This structure can be beneficial to improve the electronic conductivity and lithium ion diffusion rate of the composite lithium iron phosphate positive electrode material. In addition, the carbon volatilized from cyanamide organic ligands during high-temperature sintering can be used as a carbon source to form a carbon coating on the surface of lithium iron phosphate particles without adding additional carbon sources. The carbon-coated lithium iron phosphate particles are beneficial to improving the conductivity of the composite lithium iron phosphate positive electrode material.

[0024] In the description of the embodiments of the present application, technical terms such as "first" and "second" are only used to distinguish different objects and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features.

[0025] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0026] In the description of the embodiments of the present application, when a certain component “includes” another component, unless otherwise stated, other components are not excluded and other components may be further included.

[0027] The terms used in the description of the various described embodiments herein are used only to describe specific embodiments and are not intended to be limiting. As used in the description of the various described embodiments and the appended claims, "components" are also intended to include plural forms unless the context clearly indicates otherwise.

[0028] The following will describe the various embodiments of the present application in detail. However, it will be appreciated by those skilled in the art that in the various embodiments of the present application, many technical details are provided in order to enable the reader to better understand the present application. However, even without these technical details and various changes and modifications based on the following embodiments, the technical solution claimed in the present application can be implemented.

[0029] Figure 1 A flow chart corresponding to a method for preparing a positive electrode material provided in an embodiment of the present application.

[0030] refer to Figure 1 According to some embodiments of the present application, the present application provides a method for preparing a positive electrode material, comprising:

[0031] Step 11: prepare an iron-based metal organic framework material (Fe-MOF), wherein the metal of the Fe-MOF is iron, and the organic ligand of the Fe-MOF is a cyanamide organic ligand, and the specific preparation steps include: dispersing the first iron source in a solvent, adding a cyanamide organic ligand, performing a reflux reaction to obtain a reaction solution, and cooling, filtering and washing the reaction solution to obtain Fe-MOF. Among them, Fe-MOF is in the form of a blue powder.

[0032] The first iron source can be selected from one or more of ferric nitrate, ferric sulfate, ferric acetate, ferric phosphate, ferric chloride, ferrous perchlorate, ferrous phosphate, ferrous citrate, ferrous sulfate, ferrous acetate, ferrous nitrate, ferrous oxalate or ferrous fluoride.

[0033] The solvent may be selected from one or more of dimethylformamide (DMF), diethylformamide (DEF), dimethylacetamide (DMA), water, ethanol, methanol, ethanol, propanol or acetone. The selection of the solvent is conducive to the dispersion of the first iron source, so as to facilitate the subsequent reaction of the first iron source with the cyanamide organic ligand to form Fe-MOF.

[0034] The cyanamide organic ligand can be selected from one or more of melamine, dicyandiamide or cyanamide.

[0035] The molar ratio of the cyanamide organic ligand to the first iron source can be 0.2-1, for example, 0.2-0.4, 0.4-0.6, 0.6-0.8 or 0.8-1, specifically 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or 1, etc.

[0036] In some embodiments, a surfactant may be added at the same time as the cyanamide organic ligand. The surfactant may be selected from hexadecyltrimethylammonium bromide, sodium dodecylbenzenesulfonate, polyvinylpyrrolidone, dodecylammonium sulfate, dodecylbenzenesulfonic acid, and the like.

[0037] The molar ratio of the surfactant to the cyanamide organic ligand is 0.1-0.3, for example, 0.1-0.2 or 0.2-0.3, specifically 0.1, 0.13, 0.15, 0.18, 0.2, 0.22, 0.25, 0.28 or 0.3.

[0038] In some embodiments, in the microstructure, the Fe-MOF particles are in the shape of a cuboid, and the length of the cuboid is 50nm to 100nm, such as 50nm to 70nm, 70nm to 90nm or 90nm to 100nm, and specifically can be 50nm, 56nm, 60nm, 64nm, 70nm, 73nm, 80nm, 88nm, 90nm, 95nm or 100nm. It is understood that the particle size of different single Fe-MOF particles may be different, and therefore, the particle size of Fe-MOF fluctuates within a certain range.

[0039] The microstructure can be observed by scanning electron microscopy (SEM), transmission electron microscopy (TEM), atomic force microscopy (AFM) and other detection methods.

[0040] In some embodiments, the specific surface area of ​​Fe-MOF is 150 m 2 / g~1000m 2 / g, for example 150m 2 / g~250m 2 / g, 250m 2 / g~460m 2 / g, 460m 2 / g~750m 2 / g or 750m 2 / g~1000m 2 / g, specifically 150m 2 / g, 190m 2 / g, 250m 2 / g, 340m 2 / g, 460m 2 / g, 570m 2 / g, 640m 2 / g, 750m 2 / g, 880m 2 / g, 940m 2 / g or 1000m 2 / g. Specific surface area refers to the total surface area of ​​particles per unit volume or unit mass. It can be understood that different single Fe-MOF particles have different sizes. Correspondingly, in Fe-MOFs of different unit volumes or different unit masses, the total surface area of ​​Fe-MOF particles fluctuates within a certain range, that is, the specific surface area of ​​Fe-MOF fluctuates within a certain range. The smaller the Fe-MOF particle size, the larger the Fe-MOF specific surface area; the larger the Fe-MOF particle size, the smaller the Fe-MOF specific surface area.

[0041] In the step of preparing Fe-MOF, the temperature of the reflux reaction can be 80°C to 180°C, for example, 80°C to 100°C, 100°C to 158°C or 158°C to 180°C, specifically 80°C, 90°C, 100°C, 115°C, 134°C, 146°C, 158°C, 163°C, 170°C, 175°C or 180°C; the reflux reaction time can be 2h to 24h, for example, 2h to 6h, 6h to 10h, 10h to 15h, 15h to 20h or 20h to 24h, specifically 2h, 4h, 6h, 8h, 11h, 15h, 19h, 20h, 22h or 24h. The temperature and time of the reflux reaction can be adjusted within a certain range. Appropriate temperature and time are conducive to the full progress of the reaction. By controlling parameters such as the temperature and time of the reflux reaction within an appropriate range, the formation of a complex between iron ions and cyanamide organic ligands can be promoted, thereby improving the efficiency of constructing a metal-organic framework.

[0042] Step 12: Grind and blend Fe-MOF with a second iron source, a lithium source, and a phosphorus source to obtain a premix.

[0043] The second iron source can be selected from one or more of ferric nitrate, ferric sulfate, ferric acetate, ferric phosphate, ferric chloride, ferrous perchlorate, ferrous phosphate, ferrous citrate, ferrous sulfate, ferrous acetate, ferrous nitrate, ferrous oxalate or ferrous fluoride.

[0044] The lithium source can be selected from lithium carbonate, lithium hydroxide, lithium nitrate, lithium sulfate, lithium phosphate, lithium permanganate, lithium metaphosphate, lithium fluoride, lithium bromide, lithium oxalate, lithium formate, lithium citrate, lithium salicylate, lithium trifluoroacetate, lithium acetoacetate, lithium difluorophosphate, lithium hexafluorophosphate, lithium benzoate, lithium pyruvate, lithium acetate, etc.

[0045] The phosphorus source may be selected from one or both of diammonium hydrogen phosphate and ammonium dihydrogen phosphate.

[0046] In a specific example, the molar ratio of Fe-MOF, the second iron source, the lithium source and the phosphorus source is 1:1:1:1.

[0047] In some embodiments, the method of grinding and blending Fe-MOF with the second iron source, the lithium source and the phosphorus source is ball milling. The ball-to-material ratio of the ball milling process can be 1:1 to 10:1, for example, 1:1 to 3:1, 3:1 to 6:1 or 6:1 to 10:1, specifically 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1 or 10:1; the speed of the ball milling process can be 100rpm / min to 400rpm / min, for example, 100rpm / min to 180rpm / min, 180rpm / min to 250rpm / min or 250rpm / min to 400rpm / min. min, specifically 100rpm / min, 130rpm / min, 160rpm / min, 180rpm / min, 200rpm / min, 220rpm / min, 250rpm / min, 290rpm / min, 310rpm / min, 360rpm / min or 400rpm / min; the ball milling time can be 0.5h-2h, such as 0.5h-0.9h, 0.9h-1.5h or 1.5h-2h, specifically 0.5h, 0.4h, 0.6h, 0.9h, 1h, 1.3h, 1.5h, 1.6h, 1.8h or 2h. Wherein, the ball-to-material ratio refers to the ratio of the mass of the material in the ball mill to the mass of the grinding body.

[0048] Step 13: Sintering the premix in an inert gas atmosphere to obtain a composite lithium iron phosphate positive electrode material. The composite lithium iron phosphate positive electrode material includes lithium iron phosphate particles and carbon nanotubes. In the microstructure, the lithium iron phosphate particles are attached to the surface of the carbon nanotubes, and the carbon nanotubes are coated with iron.

[0049] The microstructure can be observed by scanning electron microscopy (SEM), transmission electron microscopy (TEM), atomic force microscopy (AFM) and other detection methods.

[0050] In some embodiments, the sintering temperature of the sintering process can be 500°C to 850°C, for example, 500°C to 640°C, 640°C to 780°C, or 780°C to 850°C, and specifically can be 500°C, 530°C, 560°C, 590°C, 610°C, 640°C, 670°C, 700°C, 750°C, 780°C, 800°C, or 850°C; the heating rate can be 1°C / min to 10°C / min, for example, 1°C / min to 5°C / min. min, 5℃ / min~8℃ / min or 8℃ / min~10℃ / min, specifically can be 1℃ / min, 3℃ / min, 5℃ / min, 7℃ / min, 8℃ / min or 10℃ / min, etc.; the sintering time can be 10h~24h, for example 10h~16h, 16h~20h or 20h~24h, specifically can be 10h, 12h, 15h, 16h, 18h, 20h, 21h or 24h, etc.

[0051] In some embodiments, the inert gas may be nitrogen, argon, helium, or the like.

[0052] In some embodiments, before grinding and blending Fe-MOF with a second iron source, a lithium source, and a phosphorus source to obtain a premix, the method further includes: blending Fe-MOF with a binder and water to obtain a mixture, and extruding the mixture into a preset shape; grinding and blending Fe-MOF with a second iron source, a lithium source, and a phosphorus source to obtain a premix includes: blending the mixture of a preset shape with a second iron source, a lithium source, and a phosphorus source to obtain a premix. Usually, positive electrode materials are mostly used in powder or gel form. The powder form is difficult to transport and use, which limits the prospect of industrial application of positive electrode materials; and the gel form will reduce the porosity of the positive electrode material and affect its mechanical properties. Compared with the transportation method of gel and powder form, mixing Fe-MOF with a binder and water and then extruding it into a preset shape can facilitate the transportation of Fe-MOF materials while avoiding the gel affecting the performance of Fe-MOF materials.

[0053] In some embodiments, the preset shape may be a cube, a cylinder, a sphere, or the like.

[0054] The binder can be selected from polyacrylic acid, carboxymethyl cellulose, polymethyl methacrylate, chitosan, carboxyethyl cellulose, polyvinyl alcohol, polyvinyl butyral, polyvinyl pyrrolidone, methyl cellulose or hydroxypropyl cellulose.

[0055] The mass ratio of the binder to the Fe-MOF may be 0.05 to 0.2, such as 0.05 to 0.13, 0.13 to 0.17 or 0.17 to 0.2, specifically 0.05, 0.08, 0.1, 0.13, 0.15, 0.17, 0.19 or 0.2.

[0056] The mass ratio of water to the mass ratio of the mixture is 0.1-0.5, for example, 0.1-0.26, 0.26-0.34, 0.34-0.45 or 0.45-0.5, and specifically can be 0.1, 0.15, 0.2, 0.26, 0.3, 0.34, 0.4, 0.45 or 0.5.

[0057] The extrusion pressure can be 70kgf / cm 2 ~250kgf / cm 2 , for example 70kgf / cm 2 ~100kgf / cm 2 、100kgf / cm 2 ~150kgf / cm 2 、150kgf / cm 2 ~180kgf / cm 2 、180kgf / cm 2 ~230kgf / cm 2 or 230kgf / cm 2 ~250kgf / cm 2 , specifically 70kgf / cm 2 、80kgf / cm 2 、90kgf / cm 2 、100kgf / cm 2 、120kgf / cm 2 、140kgf / cm 2 、150kgf / cm 2 、160kgf / cm 2 、180kgf / cm 2 、200kgf / cm 2 、230kgf / cm 2 Or 250kgf / cm 2 .

[0058] In some embodiments, the specific surface area of ​​the composite lithium iron phosphate positive electrode material is 5m 2 / g~20m 2 / g, for example 5m 2 / g~8m 2 / g, 8m 2 / g~10m 2 / g, 10m 2 / g~15m 2 / g or 15m 2 / g~20m 2 / g, specifically 5m 2 / g, 6.5m 2 / g, 8m 2 / g, 10.2m 2 / g, 15m 2 / g, 18.6m 2 / g, 19m 2 / g or 20m 2 / g. Specific surface area refers to the total surface area of ​​particles per unit volume or unit mass. The particle sizes of different single composite lithium iron phosphate positive electrode materials may be different. Correspondingly, in composite lithium iron phosphate positive electrode materials of different unit volumes or different unit masses, the total surface area of ​​the particles of the composite lithium iron phosphate positive electrode material fluctuates within a certain range, that is, the specific surface area of ​​the composite lithium iron phosphate positive electrode material fluctuates within a certain range. The smaller the particle size of the composite lithium iron phosphate positive electrode material, the larger the specific surface area of ​​the composite lithium iron phosphate positive electrode material; the larger the particle size of the composite lithium iron phosphate positive electrode material, the smaller the specific surface area of ​​the composite lithium iron phosphate positive electrode material.

[0059] In some embodiments, the particle size corresponding to the cumulative particle size distribution percentage of the composite lithium iron phosphate positive electrode material reaches 50% is 50nm to 2000nm, such as 50nm to 300nm, 300nm to 600nm, 600nm to 1230nm, 1230nm to 1654nm or 1654nm to 2000nm, and can be specifically 50nm, 100nm, 300nm, 600nm, 900nm, 1000nm, 1230nm, 1450nm, 1188nm, 1300nm, 1654nm, 1741nm or 2000nm. The average particle size of the composite lithium iron phosphate positive electrode material refers to the particle size corresponding to the cumulative particle size distribution percentage of the composite lithium iron phosphate positive electrode material reaches 50%.

[0060] In some embodiments, the carbon coating content of the composite lithium iron phosphate positive electrode material can be 0.1% to 1.5%, for example 0.1%, 0.25%, 0.3%, 0.5%, 0.8%, 1%, 1.1%, 1.3% or 1.5%. Among them, the carbon coating content is usually expressed by the mass fraction of carbon in the composite lithium iron phosphate material, and the carbon coating content can be measured by an infrared sulfur-carbon analyzer. The carbon coating content affects the electrical properties of the positive electrode material. The carbon coating content within an appropriate range can be beneficial to the composite lithium iron phosphate positive electrode material having good conductivity and the energy density of the lithium iron phosphate battery.

[0061] In the preparation method of the positive electrode material provided in the embodiment of the present application, the first iron source is first reacted with a cyanamide organic ligand to prepare an iron-based metal organic framework material (Fe-MOF), and then the Fe-MOF is mixed with a second iron source, a lithium source and a phosphorus source and sintered to obtain a composite lithium iron phosphate positive electrode material. The second iron source, the lithium source and the phosphorus source react to generate lithium iron phosphate particles, and the Fe-MOF is sintered to form carbon nanotubes coated with iron. In terms of microstructure, the lithium iron phosphate particles are attached to the surface of the carbon nanotubes. Reference Figure 2 , Figure 2 A scanning electron microscope image of a Fe-MOF after sintering provided in an embodiment of the present application, the ligand in the Fe-MOF is a cyanamide organic ligand, which will form nitrogen-doped bamboo-shaped carbon nanotubes after high-temperature sintering, and the active sites of iron are wrapped at the front end of the carbon nanotubes. The unique carbon-wrapped structure can protect and fix the active sites of iron to improve its stability. At the same time, the nitrogen-doped carbon nanotubes can provide efficient electron transmission channels to form a continuous three-dimensional conductive network. This structure can be beneficial to improving the electronic conductivity and lithium ion diffusion rate of the composite lithium iron phosphate positive electrode material. In addition, the carbon volatilized by the cyanamide organic ligand during the high-temperature sintering process can be used as a carbon source to form a carbon coating layer on the surface of the lithium iron phosphate particles without adding an additional carbon source. The carbon-coated lithium iron phosphate particles are beneficial to improving the conductivity of the composite lithium iron phosphate positive electrode material.

[0062] Correspondingly, another embodiment of the present application further provides an energy storage battery, including a positive electrode sheet and a negative electrode sheet, wherein the positive electrode material of the positive electrode sheet is manufactured by any of the preparation methods of the positive electrode materials in the above embodiments. For the parts that are the same or corresponding to the previous embodiment, reference may be made to the corresponding description of the above embodiment, and will not be described in detail below.

[0063] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode material layer, the positive electrode material layer includes a positive electrode material and a positive electrode bonding layer, the positive electrode material is formed using the preparation method of the positive electrode material in the above embodiments, and the positive electrode material is dispersed in the positive electrode bonding layer.

[0064] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode material layer, the negative electrode material layer includes a negative electrode material and a negative electrode bonding layer, and the negative electrode material is dispersed in the negative electrode bonding layer.

[0065] The negative electrode material can be selected from natural graphite, artificial graphite, soft carbon or hard carbon.

[0066] In a specific example, the material of the positive electrode current collector is aluminum foil, and the material of the negative electrode current collector is copper foil.

[0067] The material of the positive electrode adhesive layer and the material of the negative electrode adhesive layer can both be selected from sodium hydroxycellulose, polyvinylidene fluoride or styrene-butadiene rubber.

[0068] The following are specific embodiments of the present application:

[0069] Example 1

[0070] This embodiment prepares a lithium iron phosphate positive electrode material, and the preparation steps are as follows:

[0071] The Fe-MOF was prepared by dispersing 0.4 g of ferric sulfate in 100 g of DMF, adding 0.062 g of melamine (the molar ratio of melamine to ferric sulfate was 0.5), refluxing at 120° C. for 3 h to obtain a reaction solution, cooling, filtering and washing the reaction solution to obtain 0.106 g of Fe-MOF.

[0072] 0.1 g of Fe-MOF was blended with 0.4 g of ferric nitrate, 0.08 g of lithium carbonate and 0.12 g of diammonium hydrogen phosphate (the molar ratio of Fe-MOF, ferric nitrate, lithium carbonate and diammonium hydrogen phosphate was 1:1:1:1) by ball milling to obtain a premix. The ball-to-material ratio of the ball milling was 5:1, the rotation speed was 250 rpm / min, and the time was 1 h.

[0073] The premix was sintered in a nitrogen atmosphere to obtain a composite lithium iron phosphate positive electrode material. The sintering temperature was 700° C., the heating rate was 5° C. / min, and the sintering time was 12 h.

[0074] Example 2

[0075] The preparation methods of Example 2 and Example 1 are basically the same, except that the mass of melamine is different, and the molar ratio of melamine to ferric sulfate is 0.2.

[0076] Example 3

[0077] The preparation methods of Example 3 and Example 1 are basically the same, except that the mass of melamine is different and the molar ratio of melamine to ferric sulfate is 1.

[0078] Comparative Example 1

[0079] Comparative Example 1: A lithium iron phosphate positive electrode material was prepared, and the preparation steps were as follows:

[0080] 0.4 g of ferric nitrate, 0.08 g of lithium carbonate and 0.12 g of diammonium hydrogen phosphate (the molar ratio of ferric nitrate, lithium carbonate and diammonium hydrogen phosphate is 1:1:1) are ball-milled and blended to obtain a premix. The ball-to-material ratio of the ball-milling treatment is 5:1, the rotation speed is 250 rpm / min, and the time is 1 hour.

[0081] The premix was sintered in a nitrogen atmosphere to obtain a composite lithium iron phosphate positive electrode material. The sintering temperature was 700° C., the heating rate was 5° C. / min, and the sintering time was 12 h.

[0082] Comparative Example 2

[0083] The preparation method of Comparative Example 2 is basically the same as that of Example 1, except that the mass of melamine is different, and the molar ratio of melamine to ferric sulfate is 0.1.

[0084] Comparative Example 3

[0085] The preparation method of Comparative Example 3 is basically the same as that of Example 1, except that the mass of melamine is different and the molar ratio of melamine to ferric sulfate is 2.

[0086] The resistivity test was performed on the lithium iron phosphate positive electrode materials of the above-mentioned Examples 1 to 3 and Comparative Examples 1 to 3. The test results are shown in the following table:

[0087]

[0088] According to the resistivity test results of Example 1 and Comparative Example 1, it can be found that compared with conventional lithium iron phosphate positive electrode materials, the composite lithium iron phosphate positive electrode material provided in the embodiment of the present application has better conductivity. According to the resistivity test results of Examples 1 to 3, Comparative Examples 2 and 3, it is found that when the mass of the first iron source is constant, the amount of cyanamide organic ligand added is controlled within a suitable range, which can ensure that the cyanamide organic ligand provides sufficient linking points so that the iron ions react fully with the cyanamide organic ligand, and on the other hand, the composite lithium iron phosphate positive electrode material can have better conductivity.

[0089] Example 4

[0090] The preparation method of Example 4 is basically the same as that of Example 1, except that 0.0359 g of hexadecyltrimethylammonium bromide is added at the same time as melamine (the molar ratio of hexadecyltrimethylammonium bromide to melamine is 0.2).

[0091] Example 5

[0092] The preparation methods of Example 5 and Example 4 are basically the same, except that the mass of cetyltrimethylammonium bromide is different, and the molar ratio of cetyltrimethylammonium bromide to melamine is 0.1.

[0093] Example 6

[0094] The preparation methods of Example 6 and Example 4 are basically the same, except that the mass of cetyltrimethylammonium bromide is different, and the molar ratio of cetyltrimethylammonium bromide to melamine is 0.3.

[0095] Comparative Example 4

[0096] The preparation methods of Comparative Example 4 and Example 4 are basically the same, except that the mass of cetyltrimethylammonium bromide is different, and the molar ratio of cetyltrimethylammonium bromide to melamine is 0.05.

[0097] Comparative Example 5

[0098] The preparation methods of Comparative Example 5 and Example 4 are basically the same, except that the mass of cetyltrimethylammonium bromide is different, and the molar ratio of cetyltrimethylammonium bromide to melamine is 0.6.

[0099] The specific surface area test, carbon coating content test and resistivity test were performed on Example 1, Example 4 to Example 6 and Comparative Example 4 to Comparative Example 5, and the test results are as follows:

[0100]

[0101] By comparing the resistivity of the above-mentioned embodiment and the comparative example, it can be found that the addition of surfactant affects the particle size of Fe-MOF, thereby affecting the specific surface area and carbon coating content of the composite lithium iron phosphate positive electrode material. By adjusting the amount of surfactant, the specific surface area and carbon coating content of the composite lithium iron phosphate positive electrode material can be adjusted, thereby improving the conductivity of the composite lithium iron phosphate positive electrode material. When the amount of surfactant is small, the specific surface area and carbon coating content of the composite lithium iron phosphate positive electrode material are less affected, so the improvement of the conductivity is not obvious; but when the amount of surfactant is too much, the specific surface area of ​​the composite lithium iron phosphate positive electrode material is too large and prone to agglomeration. In addition, the specific surface area of ​​the composite lithium iron phosphate positive electrode material is too large, resulting in a higher carbon coating content, and excessive carbon coating content will reduce the proportion of lithium iron phosphate active materials in the composite lithium iron phosphate positive electrode material and the tap density, thereby affecting the volume energy density of the composite lithium iron phosphate positive electrode material.

[0102] Example 7

[0103] The preparation method of Example 7 is basically the same as that of Example 1, except that the ball-to-material ratio is 1:1.

[0104] Example 8

[0105] The preparation method of Example 8 is basically the same as that of Example 1, except that the ball-to-material ratio is 10:1.

[0106] Comparative Example 6

[0107] The preparation method of Comparative Example 6 is basically the same as that of Example 1, except that the ball-to-material ratio is 0.5:1.

[0108] Comparative Example 7

[0109] The preparation method of Comparative Example 7 is basically the same as that of Example 1, except that the ball-to-material ratio is 12:1.

[0110] The carbon coating content test and resistivity test were performed on Example 1, Example 7, Example 8, Comparative Example 6 and Comparative Example 7, and the test results are as follows:

[0111]

[0112] Example 9

[0113] The preparation method of Example 9 is basically the same as that of Example 1, except that the ball milling time is 0.5 h.

[0114] Example 10

[0115] The preparation method of Example 10 is basically the same as that of Example 1, except that the ball milling time is 2 hours.

[0116] Comparative Example 8

[0117] The preparation method of Comparative Example 8 is basically the same as that of Example 1, except that the ball milling time is 0.2 h.

[0118] Comparative Example 9

[0119] The preparation method of Comparative Example 9 is basically the same as that of Example 1, except that the ball milling time is 3 hours.

[0120] Carbon coating content test and resistivity test were performed on Examples 9 to 10 and Comparative Examples 8 to 9, and the test results are as follows:

[0121]

[0122] Embodiment 11

[0123] The preparation method of Example 11 is basically the same as that of Example 1, except that the sintering temperature is 500°C.

[0124] Example 12

[0125] The preparation method of Example 12 is basically the same as that of Example 1, except that the sintering temperature is 850°C.

[0126] Comparative Example 10

[0127] The preparation method of Comparative Example 10 is basically the same as that of Example 1, except that the sintering temperature is 300°C.

[0128] Comparative Example 11

[0129] The preparation method of Comparative Example 11 is basically the same as that of Example 1, except that the sintering temperature is 1000°C.

[0130] Carbon coating content test and resistivity test were performed on Examples 11 to 12 and Comparative Examples 10 to 11, and the test results are as follows:

[0131]

[0132] According to the carbon coating content test results and resistivity test results of Example 1, Example 7 to Example 12 and Comparative Examples 6 to Comparative Examples 11, it is found that the carbon coating content of the composite lithium iron phosphate positive electrode material can be controlled by controlling the ball-to-material ratio, ball milling time and sintering temperature. The carbon coating content affects the electrical properties of the composite lithium iron phosphate positive electrode material. When the carbon coating content is within an appropriate range, it can be beneficial for the composite lithium iron phosphate positive electrode material to have good conductivity and maintain the lithium iron phosphate battery to have a high energy density.

[0133] Embodiment 13

[0134] The present embodiment is an energy storage battery, which includes a positive electrode sheet and a negative electrode sheet. The positive electrode sheet includes an aluminum foil and a positive electrode material layer covering the surface of the aluminum foil, the positive electrode material layer includes polyvinylidene fluoride and a composite lithium iron phosphate material dispersed in the polyvinylidene fluoride, and the composite lithium iron phosphate material is the composite lithium iron phosphate positive electrode material prepared in the above-mentioned embodiment 1; the negative electrode sheet includes a copper foil and a negative electrode material layer covering the surface of the copper foil, and the negative electrode material layer includes polyvinylidene fluoride and artificial graphite dispersed in the polyvinylidene fluoride.

[0135] Comparative Example 12

[0136] This embodiment is an energy storage battery. The energy storage battery of comparative example 12 is basically the same as the energy storage battery of embodiment 13, except that the positive electrode material layer includes polyvinylidene fluoride and lithium iron phosphate material dispersed in the polyvinylidene fluoride, and the lithium iron phosphate material is the lithium iron phosphate positive electrode material prepared in the above comparative example 1.

[0137] Figure 3 The cycle performance test diagram of the two energy storage batteries provided in the embodiments of the present application. Curve a corresponds to embodiment 13; curve b corresponds to embodiment 12. The cycle performance test conditions are to charge and discharge at a temperature of 45°C and a charge and discharge power of 1P, with a cycle voltage of 2.5V to 3.65V, and the number of cycles is 1200.

[0138] By comparing the cycle performance test results of Example 13 and Comparative Example 12, it is found that compared with conventional lithium iron phosphate batteries, the energy storage battery obtained by preparing a composite lithium iron phosphate positive electrode material using the preparation method of the positive electrode material of this embodiment and then using the composite lithium iron phosphate positive electrode material to make the positive electrode sheet of the battery has a better capacity retention rate, and the capacity retention rate can still reach about 90% after 1200 cycles.

[0139] Figure 4 The DC impedance (DCR) test graph of two energy storage batteries provided in the embodiments of the present application. Curve c corresponds to the test results of two parallel samples in Example 13; curve d corresponds to the test results of two parallel samples in Example 12. The DC impedance test uses the difference between the voltage at the moment before the end of the intermittent discharge of the energy storage battery and the voltage after the discharge ends to calculate the internal resistance of the battery.

[0140] By comparing the DC impedance test results of Example 13 and Comparative Example 12, it is found that, relative to conventional lithium iron phosphate batteries, the energy storage battery obtained by preparing a composite lithium iron phosphate positive electrode material using the preparation method of the positive electrode material of this embodiment, and then using the composite lithium iron phosphate positive electrode material to make the positive electrode sheet of the battery has a lower DC impedance, and the performance of the energy storage battery is improved.

[0141] The preparation method of the positive electrode material and the energy storage battery provided in the embodiment of the present application, in the preparation method of the positive electrode material, the first iron source is reacted with the cyanamide organic ligand to prepare the iron-based metal organic framework material (Fe-MOF), and then the Fe-MOF is blended with the second iron source, the lithium source and the phosphorus source and sintered to obtain a composite lithium iron phosphate positive electrode material. The second iron source, the lithium source and the phosphorus source react to generate lithium iron phosphate particles, and the Fe-MOF forms carbon nanotubes coated with iron after sintering. In the microstructure, the lithium iron phosphate particles are attached to the surface of the carbon nanotubes. Among them, the ligand in the Fe-MOF is a cyanamide organic ligand, which forms nitrogen-doped bamboo-shaped carbon nanotubes after high-temperature sintering, and the active site of iron is wrapped at the front end of the carbon nanotube. The unique carbon wrapping structure can protect and fix the active site of iron, so as to improve its stability. At the same time, the nitrogen-doped carbon nanotubes can provide efficient electron transmission channels to form a continuous three-dimensional conductive network, which can be beneficial to improve the electronic conductivity and diffusion rate of lithium ions of the composite lithium iron phosphate positive electrode material. In addition, the carbon volatilized from cyanamide organic ligands during high-temperature sintering can be used as a carbon source to form a carbon coating on the surface of lithium iron phosphate particles without adding additional carbon sources. The carbon-coated lithium iron phosphate particles are beneficial to improving the conductivity of the composite lithium iron phosphate positive electrode material.

[0142] Those skilled in the art will appreciate that the above-mentioned embodiments are specific examples for implementing the present application, and in practical applications, various changes may be made to the embodiments in form and detail without departing from the spirit and scope of the present application. Any person skilled in the art may make various changes and modifications without departing from the spirit and scope of the present application, and therefore the scope of protection of the present application shall be subject to the scope defined in the claims.

Claims

1. A method for preparing a positive electrode material, It is characterized in that include: An iron-based metal organic framework material is prepared, wherein the metal of the iron-based metal organic framework material is iron, and the organic ligand is a cyanamide organic ligand, and the preparation steps include: dispersing a first iron source in a solvent, adding the cyanamide organic ligand, performing a reflux reaction to obtain a reaction liquid, and cooling, filtering and washing the reaction liquid to obtain the iron-based metal organic framework material; Grinding and blending the iron-based metal organic framework material with a second iron source, a lithium source and a phosphorus source to obtain a premix; The premix is ​​sintered in an inert gas atmosphere to obtain a composite lithium iron phosphate positive electrode material, wherein the composite lithium iron phosphate positive electrode material comprises lithium iron phosphate particles and carbon nanotubes, wherein the lithium iron phosphate particles are attached to the surface of the carbon nanotubes, and the carbon nanotubes are coated with iron.

2. The method for preparing the positive electrode material according to claim 1, It is characterized in that The first iron source and the second iron source are selected from one or more of ferric nitrate, ferric sulfate, ferric acetate, ferric phosphate, ferric chloride, ferrous perchlorate, ferrous phosphate, ferrous citrate, ferrous sulfate, ferrous acetate, ferrous nitrate, ferrous oxalate or ferrous fluoride.

3. The method for preparing the positive electrode material according to claim 1, It is characterized in that The cyanamide organic ligand is selected from one or more of melamine, dicyandiamide or cyanamide.

4. The method for preparing the positive electrode material according to claim 1, It is characterized in that In the step of preparing the iron-based metal organic framework material, the molar ratio of the cyanamide organic ligand to the first iron source is 0.2-1; the temperature of the reflux reaction is 80° C.-180° C.; and the time of the reflux reaction is 2h-24h.

5. The method for preparing the positive electrode material according to claim 1, It is characterized in that The specific surface area of ​​the iron-based metal organic framework material is 150 m 2 / g~1000m 2 / g.

6. The method for preparing the positive electrode material according to claim 1, It is characterized in that The particle shape of the iron-based metal organic framework material is a cuboid, and the length of the cuboid is 50nm to 100nm.

7. The method for preparing the positive electrode material according to claim 1, It is characterized in that Before grinding and blending the iron-based metal organic framework material with the second iron source, the lithium source and the phosphorus source to obtain the premix, the method comprises: The iron-based metal organic framework material is mixed with a binder and water to obtain a mixture, and the mixture is extruded into a preset shape; Grinding and blending the iron-based metal organic framework material with the second iron source, the lithium source and the phosphorus source to obtain the premix comprises: blending the mixture of the preset shape with the second iron source, the lithium source and the phosphorus source to obtain the premix.

8. The method for preparing the positive electrode material according to claim 1, It is characterized in that The sintering temperature of the sintering treatment is 500° C. to 850° C., the heating rate is 1° C. / min to 10° C. / min, and the sintering time is 10 h to 24 h.

9. The method for preparing the positive electrode material according to claim 1, It is characterized in that The specific surface area of ​​the composite lithium iron phosphate positive electrode material is 5m 2 / g~60m 2 / g, when the cumulative particle size distribution percentage of the composite lithium iron phosphate positive electrode material reaches 50%, the corresponding particle size is 50nm-2000nm.

10. An energy storage battery, It is characterized in that include: A positive electrode sheet and a negative electrode sheet, wherein the material of the positive electrode sheet is made by the method for preparing the positive electrode material according to any one of claims 1 to 9.

Citation Information

Cited By

  • Phosphate positive electrode material and preparation method and application thereof

    CN120637426A

  • Phosphate-based positive electrode material, preparation method and application thereof

    CN120637426B