Trans-perovskite solar cell constructed by resonant pyridine derivative NPP and preparation method thereof
By using resonant pyridine derivatives NPP and carbon quantum dots to passivate grain boundaries in perovskite solar cells, and introducing diethylenetriamine to repair interface defects, the problem of high grain boundary defect density in perovskite solar cells is solved. , improving the photoelectric performance of the device and the quality of crystal film formation.
Patent Information
- Application Number
- CN202410858198.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-29
AI Technical Summary
The high density of grain boundary defects in perovskite solar cells affects device performance. How to reduce the density of grain boundary defects and achieve grain boundary passivation is a difficulty.
A trans perovskite solar cell method constructed using resonant pyridine derivative NPP uses carbon quantum dots as additives to passivate the perovskite grain boundaries, and introduces diethylenetriamine between the hole transport layer and the perovskite layer. As an interface in-situ induction layer, a chemical bridge is formed to repair buried interface defects.
It effectively reduces the defect concentration in the perovskite film, improves the photoelectric performance of the device, enhances the quality of crystal film formation, reduces non-radiative recombination, and improves the open circuit voltage and photoelectric efficiency.
Smart Images

Figure CN118870932A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of perovskite solar cells, and in particular relates to an inverse perovskite solar cell constructed with a resonance pyridine derivative NPP and a preparation method thereof. Background Art
[0002] Perovskite solar cells (PSCs) can be divided into formal structure (nip) devices and trans structure (pin) devices according to the different positions of the transport layer and the light absorption layer. Compared with formal PSCs, the density of perovskite interface trap states in trans PSCs is lower, which is conducive to carrier transport. Perovskite, as the active layer in perovskite solar cells, has a large number of grain boundaries (GBs) due to its polycrystalline characteristics. Generally, defects (dangling bonds) at the grain boundaries will cause non-radiative recombination of carriers and affect the performance of solar cell devices. Therefore, how to reduce the density of grain boundary defects and achieve grain boundary passivation is a difficult problem in the research of perovskite solar cells. Summary of the invention
[0003] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing an inverse perovskite solar cell constructed by a resonant pyridine derivative NPP, comprising the following steps:
[0004] Step 1, preparation of carbon quantum dots, adding a certain amount of sodium hydroxide to acetone, stirring and standing at room temperature for a period of time, then adding diluted hydrochloric acid dropwise, adjusting the pH to 7, and drying to obtain a mixture of carbon quantum dots and sodium chloride; purifying the mixture with ethanol and drying to obtain a powder of carbon quantum dots; dissolving the carbon quantum dot powder with N,N-dimethylformamide to prepare a carbon quantum dot solution and sealing it for later use;
[0005] Step 2, preparation of the precursor solution, weighing a certain amount of ammine iodide, methyl ammonium bromide, PbBr2, PbI2, dissolving them in a mixed solution of N,N-dimethylformamide and dimethyl sulfoxide, and then adding a certain amount of the carbon quantum dot solution prepared in step 1, stirring; adding a certain amount of CsI dimethyl sulfoxide solution, stirring to obtain a mixed cation perovskite precursor solution with carbon quantum dots; weighing a certain amount of polytriarylamine and dissolving it in toluene to obtain a polytriarylamine-toluene solution; weighing a certain amount of N-(2-pyridyl)-trimethylacetamide and dissolving it in isopropanol, stirring to obtain N-(2-pyridyl)-trimethylacetamide-isopropanol solution; weighing a certain amount of [6,6]phenyl-C61 butyric acid methyl ester and dissolving it in ultra-dry chlorobenzene, stirring to obtain [6,6]phenyl-C61 butyric acid methyl ester-anhydrous chlorobenzene solution;
[0006] Step 3: Cleaning of ITO glass substrate;
[0007] Step 4: Preparation of a hole transport layer: drop a certain amount of polytriarylamine-toluene solution on an ITO glass substrate, spin-coat, and then heat and anneal to form a hole transport layer on the ITO glass substrate;
[0008] Step 5, preparation of the buried bottom interface in-situ induction layer, dissolving a certain amount of diethylenetriamine in dimethyl sulfoxide to obtain a diethylenetriamine-dimethyl sulfoxide solution; taking a certain amount of diethylenetriamine-dimethyl sulfoxide solution and N-(2-pyridyl)-trimethylacetamide-isopropanol solution, mixing them, heating and stirring to form a mixed solution, taking a certain amount of the mixed solution and dropping it on the hole transport layer on the ITO glass substrate, spin coating, and then heating and annealing to form a buried bottom interface in-situ induction layer on the hole transport layer;
[0009] Step 6, preparation of mixed cation perovskite film, taking a certain amount of dimethyl sulfoxide and spin coating it on the buried bottom interface in-situ induction layer to wet the buried bottom interface in-situ induction layer; taking a certain amount of mixed cation perovskite precursor solution with carbon quantum dots and uniformly dropping it on the wetted buried bottom interface in-situ induction layer, spin coating, and uniformly dropping a certain amount of ethyl acetate (EA) during the spin coating process, and immediately heating and annealing after the spin coating is completed to form a mixed cation perovskite film on the buried bottom interface in-situ induction layer;
[0010] Step 7: Preparation of electron transport layer: taking a certain amount of [6,6]phenyl-C61butyric acid methyl ester-anhydrous chlorobenzene solution, adding it evenly onto the mixed cation perovskite film after stirring, and spin coating to form an electron transport layer on the mixed cation perovskite film;
[0011] Step eight, preparation of the cathode metal layer, vacuum evaporation forms a C60 film on the electron transport layer, and then vacuum evaporation forms a Cu film on the C60 film to obtain a cathode metal layer.
[0012] As a preferred embodiment of the above technical scheme, the concentration of the carbon quantum dot solution in step one is 0.15 mg / mL, the concentration of the mixed cation perovskite precursor solution with carbon quantum dots in step two is 1.38 mol / L, the concentration of the polytriarylamine-toluene solution is 4 mg / mL; the concentration of N-(2-pyridyl)-trimethylacetamide-isopropanol solution is 15 mg / mL; the concentration of [6,6]phenyl-C61butyric acid methyl ester-anhydrous chlorobenzene solution is 20 mg / mL, and the concentration of the diethylenetriamine-dimethyl sulfoxide solution in step five is 4 mg / mL.
[0013] As a preferred embodiment of the above technical solution, in step 1, 8 g of sodium hydroxide is added to 50 mL of acetone, stirred and allowed to stand for a period of time at room temperature, and then diluted hydrochloric acid is added dropwise to adjust the pH to 7, and dried at 80°C to obtain a mixture of carbon quantum dots and sodium chloride; the mixture is purified with ethanol and dried, and the carbon quantum dot powder is obtained after repeated multiple times.
[0014] As a preferred embodiment of the above technical scheme, in the step 2, 228.07 mg of ammonium iodide, 26.21 mg of methyl ammonium bromide, 92.48 mg of PbBr2, and 648.07 mg of PbI2 are weighed in a glass bottle, dissolved in a mixed solution of 960 μL of N,N-dimethylformamide and 240 μL of dimethyl sulfoxide, and then a certain amount of the carbon quantum dot solution prepared in step 1 is added, and stirred on a magnetic stirrer at 60°C for 2.5 hours; 0.3897 g of CsI is dissolved in 1000 μL of dimethyl sulfoxide, and stirred at room temperature to obtain a dimethyl sulfoxide solution of CsI; 54.72 μL of CsI in dimethyl sulfoxide is dissolved in 1000 μL of dimethyl sulfoxide. The liquid was added into a glass bottle, and a mixed cation perovskite precursor solution with carbon quantum dots was obtained after magnetic stirring at 60°C; 4.8 mg of polytriarylamine was weighed and dissolved in 1200 μL of toluene, and stirred at room temperature for 12 hours to obtain a polytriarylamine-toluene solution; 30 mg of N-(2-pyridyl)-trimethylacetamide was weighed and dissolved in 2 mL of isopropanol, and N-(2-pyridyl)-trimethylacetamide-isopropanol solution was obtained after uniform stirring at room temperature; 12 mg of [6,6]phenyl-C61butyric acid methyl ester was weighed and dissolved in 600 μL of ultra-dry chlorobenzene, and stirred at room temperature for 12 hours to obtain a [6,6]phenyl-C61butyric acid methyl ester-anhydrous chlorobenzene solution.
[0015] As a preferred embodiment of the above technical solution, in the step three, the ITO glass substrate is scrubbed with a detergent, and then ultrasonically cleaned twice with deionized water, acetone, and ethanol in sequence, each time for 15 minutes, and then the ITO glass substrate after ultrasonic cleaning is placed in a ventilated oven at a temperature of 100°C for drying for 15 minutes, and the dried ITO glass substrate is treated with ultraviolet ozone for 15 minutes using an ozone-ultraviolet surface cleaner.
[0016] As a preferred embodiment of the above technical solution, 60 μL of the polytriarylamine-toluene solution in step 4 is dropped on the ITO glass substrate, and a coating machine is used to spin the solution at a speed of 4000 rpm and an acceleration of 1000 rpm / s for 30 seconds, and the solution is annealed on a heating table at a temperature of 100° C. for 10 minutes to form a hole transport layer on the ITO glass substrate.
[0017] As a preferred embodiment of the above technical solution, in the step five, 60 μl of diethylenetriamine-dimethyl sulfoxide solution and 60 μl of NPP-IPA solution are taken, heated and stirred to form a mixed solution, 60 μL of the mixed solution is drawn with a pipette and dropped on the hole transport layer on the ITO glass substrate, and a coating machine is used to spin coat at a spin coating speed of 4000 rpm and an acceleration of 2000 rpm / s for 30 seconds, and annealed on a heating table at a temperature of 100°C for 15 minutes to form a buried interface in-situ induced layer on the hole transport layer.
[0018] As a preferred embodiment of the above technical solution, in step 6, 60 μL of dimethyl sulfoxide is spin-coated on the buried interface in-situ induction layer to wet the buried interface in-situ induction layer; 70 μL of a mixed cation perovskite precursor solution with carbon quantum dots is evenly dripped on the wetted buried interface in-situ induction layer, and the mixture is spin-coated at a speed of 10000 rpm and an acceleration of 1000 rpm / s for 55 s. At the 40th second of the spin-coating process, 150 μL of ethyl acetate (EA) is uniformly dripped, and the mixture is immediately annealed at 100°C for 10 min after the spin-coating is completed to form a mixed cation perovskite film on the buried interface in-situ induction layer; in step 7, 50 μL of [6,6]phenyl-C61butyric acid methyl ester-anhydrous chlorobenzene solution is evenly dripped on the mixed cation perovskite film, and the mixture is spin-coated at a speed of 2000 rpm and an acceleration of 1000 rpm / s for 30 s; the pressure during vacuum evaporation of C60 in step 8 is 5×10 -4 Pa, temperature is 420℃, evaporation rate is The thickness of the C60 film is 10nm; when vacuum evaporating the Cu film, the evaporation rate is
[0019] The trans-perovskite solar cell constructed by the resonance pyridine derivative NPP is prepared by the above preparation method.
[0020] The beneficial effects of the present invention are: 1. Carbon quantum dots can be used as additives to passivate perovskite grain boundaries to obtain high-performance inverse PSCs. For the unpaired lead ion defects at the perovskite grain boundaries, carbon quantum dots (CQDs) rich in hydroxyl and carbonyl groups on the surface are used as additives to passivate such defects. The CQDs additive slows down the crystallization rate of perovskite, forms a larger perovskite unit cell, and improves the absorbance of the perovskite layer. CQDs play a role in passivating the grain boundaries of the perovskite film and reducing the defect concentration in the perovskite film. This grain boundary passivation effect is caused by the interaction between the uncoordinated lead ions and the hydroxyl and carbonyl functional groups on the carbon quantum dots, which effectively reduces the non-radiative recombination in the perovskite layer;
[0021] 2. Diethylenetriamine (DETA) is used as an interface layer between the hole transport material (HTM) and the perovskite layer to reduce the energy loss between the transport layer and the perovskite layer. Alkyl ammonium can also passivate the uncoordinated defects of the bottom perovskite and inhibit non-radiative energy loss. DETA not only acts as a passivation layer, but also solves the problem of poor spreadability of the spin-coated precursor solution on the hole transport layer. It also effectively guides the growth process of the perovskite film and improves the crystallization quality of the perovskite crystal. It effectively improves the problem of poor spreadability of the precursor solution due to the excessive hydrophobicity of the hole transport layer, is beneficial to the migration of hole carriers, reduces the energy loss of the device, and increases the open circuit voltage of the device. It greatly reduces the pinholes and cracks on the surface of the perovskite film, improves the quality of crystal film formation, reduces the defect state density, and improves the photoelectric performance of the device;
[0022] 3. By modifying the buried interface of the trans-PSC to form a chemical bridge, the buried interface defects of the perovskite are repaired in situ, and a perovskite film with preferentially oriented crystals is obtained, and finally a high-quality perovskite crystal film with preferential orientation, low defect state density, flatness, density, and low roughness is prepared. The new resonant pyridine derivative N-(2-pyridyl)-trimethylacetamide (NPP) is introduced into the PTAA / PVK interface as a multifunctional chemical bridge, and the interface properties are improved through the coordination bonds between NPP / PTAA and NPP / PVK. The insertion of NPP improves the interface properties. The pyridine group in the NPP molecule forms a π-π stack with the benzene ring group in PTAA to improve the hole transport capacity; the NC=O resonance group as a Lewis base can effectively repair the buried interface defects (such as undercoordinated Pb 2+ ions), which improves the interfacial properties of PTAA / perovskite. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of the structure of the present invention;
[0024] Figure 2 This is the SEM image of the in-situ induced layer at the buried interface;
[0025] Figure 3 is the SEM image of the mixed cation perovskite film;
[0026] Figure 4 It is a schematic diagram comparing the electrical performance of the solar cell in Example 1 and the solar cell in Example 2. DETAILED DESCRIPTION
[0027] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] Add 8g of sodium hydroxide to 50mL of acetone, stir and let stand for a while at room temperature, then add diluted hydrochloric acid drop by drop, adjust the pH to 7, and dry at 80℃ to obtain a mixture of carbon quantum dots and sodium chloride; purify the mixture with ethanol and dry it, repeat several times to obtain a powder of carbon quantum dots. Dissolve the carbon quantum dot powder with N,N-dimethylformamide to prepare a carbon quantum dot solution with a concentration of 0.15mg / mL, seal and set aside.
[0030] Weigh 228.07 mg of ammonium iodide, 26.21 mg of methyl ammonium bromide, 92.48 mg of PbBr2, and 648.07 mg of PbI2 in a glass bottle, dissolve in a mixed solution of 960 μL of N,N-dimethylformamide and 240 μL of dimethyl sulfoxide, then add a certain amount of the prepared carbon quantum dot solution, and stir on a magnetic stirrer at 60°C for 2.5 h; take 0.3897 g of CsI and dissolve it in 1000 μL of dimethyl sulfoxide, stir at room temperature to obtain a dimethyl sulfoxide solution of CsI; add 54.72 μL of the dimethyl sulfoxide solution of CsI into a glass bottle, and after magnetic stirring at 60°C, obtain a carbon quantum dot solution with a concentration of 1.38 mol / L. Quantum dot mixed cation perovskite precursor solution; weigh 4.8 mg of polytriarylamine and dissolve it in 1200 μL of toluene, stir it at a constant speed for 12 hours at room temperature to obtain a polytriarylamine-toluene solution with a concentration of 4 mg / mL; weigh 30 mg of N-(2-pyridyl)-trimethylacetamide (NPP) and dissolve it in 2 mL of isopropanol, stir it at a constant speed at room temperature to obtain a N-(2-pyridyl)-trimethylacetamide-isopropanol solution with a concentration of 15 mg / mL; weigh 12 mg of [6,6]phenyl-C61butyric acid methyl ester and dissolve it in 600 μL of ultra-dry chlorobenzene, stir it at room temperature for 12 hours to obtain a [6,6]phenyl-C61butyric acid methyl ester-anhydrous chlorobenzene solution with a concentration of 20 mg / mL.
[0031] The ITO glass substrate was scrubbed with detergent, and then ultrasonically cleaned twice with deionized water, acetone, and ethanol in sequence, each time for 15 minutes, and then the ITO glass substrate after ultrasonic cleaning was placed in a ventilated oven at a temperature of 100°C for 15 minutes. The dried ITO glass substrate was treated with ultraviolet ozone for 15 minutes using an ozone-ultraviolet surface cleaner.
[0032] 60 μL of polytriarylamine-toluene solution was dropped on the ITO glass substrate, and a coating machine was used to spin coat the solution at a speed of 4000 rpm and an acceleration of 1000 rpm / s for 30 s. The solution was annealed on a heating table at 100° C. for 10 min to form a hole transport layer on the ITO glass substrate.
[0033] Take 60 μL of diethylenetriamine-dimethyl sulfoxide solution and 60 μL of NPP-IPA solution, heat and stir to form a mixed solution, use a pipette to draw 60 μL of the mixed solution and drop it on the hole transport layer on the ITO glass substrate, use a coater to spin coat at a speed of 4000 rpm and an acceleration of 2000 rpm / s for 30 seconds, anneal on a heating table at 100°C for 15 minutes, and form a buried interface in-situ induced layer on the hole transport layer.
[0034] Take 60 μL of dimethyl sulfoxide and spin coat it on the buried interface in-situ induction layer to wet the buried interface in-situ induction layer; take 70 μL of the mixed cation perovskite precursor solution with carbon quantum dots and evenly drip it on the wetted buried interface in-situ induction layer, spin coat it at a speed of 10000 rpm and an acceleration of 1000 rpm / s for 55 seconds, and uniformly drip 150 μL of EA at the 40th second of the spin coating process. After the spin coating, anneal at 100°C for 10 minutes to form a mixed cation perovskite film on the buried interface in-situ induction layer; in the step 7, take 50 μL of [6,6]phenyl-C61butyric acid methyl ester-anhydrous chlorobenzene solution and evenly drip it on the mixed cation perovskite film, spin coat it at a speed of 2000 rpm and an acceleration of 1000 rpm / s for 30 seconds; the pressure during vacuum evaporation of C60 in the step 8 is 5×10 -4 Pa, temperature is 420℃, evaporation rate is The thickness of the C60 film is 10nm; when vacuum evaporating the Cu film, the evaporation rate is Finally, the structure of the trans-perovskite solar cell constructed by the resonant pyridine derivative NPP is obtained as follows Figure 1 shown.
[0035] Example 2
[0036] The other steps were the same as in Example 1, except that NPP was not added.
[0037] Example 3
[0038] The other steps were the same as in Example 1, except that the concentration of the NPP solution was changed to 4 mg*mL -1 .
[0039] Example 4
[0040] The other steps were the same as in Example 1, except that the concentration of the NPP solution was changed to 10 mg*mL -1 .
[0041] Example 5
[0042] The other steps were the same as in Example 1, except that the concentration of the NPP solution was changed to 20 mg*mL -1 .
[0043] Example 6
[0044] The other steps were the same as in Example 1, except that the concentration of the NPP solution was changed to 30 mg*mL -1 .
[0045] Using AM 1.5G standard (100mW / cm 2 ) solar simulator to evaluate the photoelectric properties of the solar cells in Examples 1-7. In the experiment, the battery was continuously tested under simulated sunlight to monitor its performance under continuous lighting conditions. Through multiple cycle tests, the changes in battery performance over time were observed to evaluate the stability and reliability of the battery in long-term use. The photoelectric property test process uses conventional technology for testing photoelectric properties of solar cells. The test results are as follows:
[0046]
[0047] The Jsc of the prepared device shows a trend of first increasing and then decreasing with the increase of concentration, which can be attributed to the excessively high concentration of NPP deposition producing a large steric hindrance at the interface, which limits the carrier transport. The FF increases continuously to a stable value with the increase of concentration, which is mainly attributed to the induction effect of NPP on the preferential orientation crystallization of perovskite crystals, thereby improving the crystal growth quality while repairing the bottom defects.
[0048] By adding an interface in-situ induced layer to construct a chemical bridge in the trans-PSC, the substrate interface defects are repaired and the perovskite crystal orientation is optimized. The pyridine-based resonant small molecule is introduced to form a π-π stacked rigid structure with the HTL through the pyridine group to improve the carrier extraction and transmission capacity. At the same time, the tautomeric structure (N+=CO - ) Dynamically repair the uncoordinated defects of the buried perovskite interface to reduce the non-radiative recombination of the interface, slow down the lattice distortion, and prepare high-quality perovskite films. The device based on this has achieved 82% FF and 19.78% PCE. NPP molecules are low in cost and good in effect. It is an excellent in-situ induced material for the buried perovskite interface. Preferential orientation induced crystallization by constructing a chemical bridge is a successful synergistic modification strategy for the upper and lower interfaces.
[0049] It is worth mentioning that the technical features such as the vacuum evaporation equipment involved in the patent application of this invention should be regarded as the prior art. The specific structure, working principle and possible control method and spatial layout method of these technical features can be selected by conventional methods in the field, and should not be regarded as the inventive point of the patent of this invention. The patent of this invention will not be further elaborated.
[0050] The preferred specific embodiments of the present invention are described in detail above. It should be understood that ordinary technicians in this field can make many modifications and changes based on the concept of the present invention without creative work. Therefore, all technical solutions that can be obtained by technicians in this technical field through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the existing technology should be within the scope of protection determined by the claims.
Claims
1. A method for preparing an inverse perovskite solar cell constructed by a resonant pyridine derivative NPP, characterized in that: The following steps are included: Step 1, preparation of carbon quantum dots, adding a certain amount of sodium hydroxide to acetone, stirring and standing at room temperature for a period of time, then adding diluted hydrochloric acid dropwise, adjusting the pH to 7, and drying to obtain a mixture of carbon quantum dots and sodium chloride; purifying the mixture with ethanol and drying to obtain a powder of carbon quantum dots; dissolving the carbon quantum dot powder with N,N-dimethylformamide to prepare a carbon quantum dot solution and sealing it for later use; Step 2, preparation of the precursor solution, weighing a certain amount of ammine iodide, methyl ammonium bromide, PbBr2, PbI2, dissolving them in a mixed solution of N,N-dimethylformamide and dimethyl sulfoxide, and then adding a certain amount of the carbon quantum dot solution prepared in step 1, stirring; adding a certain amount of CsI dimethyl sulfoxide solution, stirring to obtain a mixed cation perovskite precursor solution with carbon quantum dots; weighing a certain amount of polytriarylamine and dissolving it in toluene to obtain a polytriarylamine-toluene solution; weighing a certain amount of N-(2-pyridyl)-trimethylacetamide and dissolving it in isopropanol, stirring to obtain N-(2-pyridyl)-trimethylacetamide-isopropanol solution; weighing a certain amount of [6,6]phenyl-C61 butyric acid methyl ester and dissolving it in ultra-dry chlorobenzene, stirring to obtain [6,6]phenyl-C61 butyric acid methyl ester-anhydrous chlorobenzene solution; Step 3: Cleaning of ITO glass substrate; Step 4: Preparation of a hole transport layer: drop a certain amount of polytriarylamine-toluene solution on an ITO glass substrate, spin-coat, and then heat and anneal to form a hole transport layer on the ITO glass substrate; Step 5, preparation of the buried bottom interface in-situ induction layer, dissolving a certain amount of diethylenetriamine in dimethyl sulfoxide to obtain a diethylenetriamine-dimethyl sulfoxide solution; taking a certain amount of diethylenetriamine-dimethyl sulfoxide solution and N-(2-pyridyl)-trimethylacetamide-isopropanol solution, mixing them, heating and stirring to form a mixed solution, taking a certain amount of the mixed solution and dropping it on the hole transport layer on the ITO glass substrate, spin coating, and then heating and annealing to form a buried bottom interface in-situ induction layer on the hole transport layer; Step 6, preparation of mixed cation perovskite film, taking a certain amount of dimethyl sulfoxide and spin coating it on the buried bottom interface in-situ induction layer to wet the buried bottom interface in-situ induction layer; taking a certain amount of mixed cation perovskite precursor solution with carbon quantum dots and uniformly dropping it on the wetted buried bottom interface in-situ induction layer, spin coating, and uniformly dropping a certain amount of ethyl acetate during the spin coating process, and immediately heating and annealing after the spin coating is completed to form a mixed cation perovskite film on the buried bottom interface in-situ induction layer; Step 7: Preparation of electron transport layer: taking a certain amount of [6,6]phenyl-C61butyric acid methyl ester-anhydrous chlorobenzene solution, adding it evenly onto the mixed cation perovskite film after stirring, and spin coating to form an electron transport layer on the mixed cation perovskite film; Step eight, preparation of the cathode metal layer, vacuum evaporation forms a C60 film on the electron transport layer, and then vacuum evaporation forms a Cu film on the C60 film to obtain a cathode metal layer.
2. The method for preparing a trans-perovskite solar cell constructed by a resonant pyridine derivative NPP according to claim 1, characterized in that: The concentration of the carbon quantum dot solution in step one is 0.15 mg / mL, the concentration of the mixed cation perovskite precursor solution with carbon quantum dots in step two is 1.38 mol / L, the concentration of the polytriarylamine-toluene solution is 4 mg / mL; the concentration of the N-(2-pyridyl)-trimethylacetamide-isopropanol solution is 15 mg / mL; the concentration of the [6,6]phenyl-C61butyric acid methyl ester-anhydrous chlorobenzene solution is 20 mg / mL, and the concentration of the diethylenetriamine-dimethyl sulfoxide solution in step five is 4 mg / mL.
3. The method for preparing a trans-perovskite solar cell constructed by a resonant pyridine derivative NPP as claimed in claim 2, characterized in that: In the step 1, 8 g of sodium hydroxide is added to 50 mL of acetone, stirred and allowed to stand for a period of time in a room temperature environment, and then diluted hydrochloric acid is added dropwise to adjust the pH to 7, and dried at 80° C. to obtain a mixture of carbon quantum dots and sodium chloride; the mixture is purified with ethanol and dried, and the mixture is repeated multiple times to obtain a powder of carbon quantum dots.
4. The method for preparing a trans-perovskite solar cell constructed by a resonant pyridine derivative NPP as claimed in claim 2, characterized in that: In the step 2, 228.07 mg of ammonium iodide, 26.21 mg of methyl ammonium bromide, 92.48 mg of PbBr2, and 648.07 mg of PbI2 were weighed into a glass bottle, dissolved in a mixed solution of 960 μL of N,N-dimethylformamide and 240 μL of dimethyl sulfoxide, and then a certain amount of the carbon quantum dot solution prepared in step 1 was added, and stirred on a magnetic stirrer at 60° C. for 2.5 h; 0.3897 g of CsI was dissolved in 1000 μL of dimethyl sulfoxide, and stirred at room temperature to obtain a dimethyl sulfoxide solution of CsI; 54.72 μL of the dimethyl sulfoxide solution of CsI was added to the glass bottle; The mixture was stirred at 60 °C in a bottle under magnetic stirring to obtain a mixed cation perovskite precursor solution with carbon quantum dots; 4.8 mg of polytriarylamine was dissolved in 1200 μL of toluene and stirred at room temperature for 12 hours to obtain a polytriarylamine-toluene solution; 30 mg of N-(2-pyridyl)-trimethylacetamide was dissolved in 2 mL of isopropanol and stirred at room temperature to obtain a N-(2-pyridyl)-trimethylacetamide-isopropanol solution; 12 mg of [6,6]phenyl-C61butyric acid methyl ester was dissolved in 600 μL of ultra-dry chlorobenzene and stirred at room temperature for 12 hours to obtain a [6,6]phenyl-C61butyric acid methyl ester-anhydrous chlorobenzene solution.
5. The method for preparing a trans-perovskite solar cell constructed by a resonant pyridine derivative NPP as claimed in claim 2, characterized in that: In the step three, the ITO glass substrate is scrubbed with a detergent, and then ultrasonically cleaned twice with deionized water, acetone, and ethanol in sequence, each time for 15 minutes, and then the ITO glass substrate after ultrasonic cleaning is placed in a ventilated oven at a temperature of 100° C. for drying for 15 minutes, and the dried ITO glass substrate is treated with ultraviolet ozone for 15 minutes using an ozone-ultraviolet surface cleaner.
6. The method for preparing a trans-perovskite solar cell constructed by a resonant pyridine derivative NPP as claimed in claim 2, characterized in that: In the step 4, 60 μL of the polytriarylamine-toluene solution was dropped onto the ITO glass substrate, and the coating was performed using a coating machine at a spin coating speed of 4000 rpm and an acceleration of 1000 rpm / s for 30 seconds, and annealed on a heating table at a temperature of 100° C. for 10 minutes to form a hole transport layer on the ITO glass substrate.
7. The method for preparing a trans-perovskite solar cell constructed by a resonant pyridine derivative NPP as claimed in claim 2, characterized in that: In the step five, 60 μL of diethylenetriamine-dimethyl sulfoxide solution and 60 μL of NPP-IPA solution are taken, heated and stirred to form a mixed solution, 60 μL of the mixed solution is drawn with a pipette and dropped on the hole transport layer on the ITO glass substrate, and a coating machine is used to spin coat at a spin coating speed of 4000 rpm and an acceleration of 2000 rpm / s for 30 seconds, and annealed on a heating table at a temperature of 100° C. for 15 minutes to form a buried interface in-situ induction layer on the hole transport layer.
8. The method for preparing a trans-perovskite solar cell constructed by a resonant pyridine derivative NPP as claimed in claim 2, characterized in that: In the step 6, 60 μL of dimethyl sulfoxide is spin-coated on the buried interface in-situ induction layer to wet the buried interface in-situ induction layer; 70 μL of a mixed cation perovskite precursor solution with carbon quantum dots is evenly dripped on the wetted buried interface in-situ induction layer, and the mixture is spin-coated at a speed of 10000 rpm and an acceleration of 1000 rpm / s for 55 seconds. At the 40th second of the spin-coating process, 150 μL of ethyl acetate is uniformly dripped, and the mixture is immediately annealed at 100° C. for 10 minutes after the spin-coating is completed to form a mixed cation perovskite film on the buried interface in-situ induction layer; in the step 7, 50 μL of [6,6]phenyl-C61butyric acid methyl ester-anhydrous chlorobenzene solution is evenly dripped on the mixed cation perovskite film, and the mixture is spin-coated at a speed of 2000 rpm and an acceleration of 1000 rpm / s for 30 seconds; the pressure during vacuum evaporation of C60 in the step 8 is 5×10 -4 Pa, temperature is 420℃, evaporation rate is The thickness of the C60 film is 10nm; when vacuum evaporating the Cu film, the evaporation rate is 9. An inverse perovskite solar cell constructed with a resonant pyridine derivative NPP, characterized in that it is prepared by the preparation method according to any one of claims 1 to 8.