Black light-shielding member
By combining the use of black particles, chain structures and low refractive index nanoparticles in the light-shielding layer, the problem of difficulty in balancing high blackness and low gloss in the existing technology is solved, achieving an effect close to pure black and improving processing sex.
Patent Information
- Application Number
- CN202380027584.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-24
- Filing Date
- 2023-05-23
- Publication Date
- 2024-10-29
AI Technical Summary
While pursuing high blackness, existing light-shielding parts have difficulty balancing low gloss and processability. They often appear bluish, making it difficult to achieve an effect close to pure black.
Add black particles, chain structures and low-refractive index nanoparticles to the light-shielding layer, and adjust their proportions and structure to reduce the reflectivity on the low-wavelength side and form a black color closer to pure black.
A low-gloss, high-black light-shielding component is realized, which has excellent design and is suitable for use in camera units of mobile phones such as smartphones. It also suppresses the bluish cast and improves processability.
Smart Images

Figure CN118871823A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a black light shielding component, and more particularly to a black light shielding component that can be suitably used in optical elements such as camera units of mobile phones including smartphones. Background Art
[0002] Light shielding components are commonly used in camera lens apertures, shutters, and lens spacers.
[0003] As such a light-shielding component, a black film having a predetermined concavo-convex shape formed on the surface of a black polyester substrate or the like containing a black pigment such as carbon black is known. In the above structure, the light is effectively scattered by controlling the fine concavo-convex shape on the surface of the light-shielding layer, and the black pigment absorbs the light to reduce the reflected light, thereby achieving low gloss. As a method for forming the above concavo-convex shape, a method of covering the surface of the substrate with a light-shielding layer containing a matting agent, and a method of roughening the surface of the substrate by means such as sandblasting can be cited.
[0004] Patent Document 1 states that: Using the above method, the arithmetic mean roughness Ra of the surface of the light-shielding component according to JIS B0601:2001 is adjusted to be 0.5 μm or more, and the difference (Rp-Rv) between the maximum peak height Rp and the maximum valley depth Rv is less than 3. Thus, the light-shielding component having such a surface shape exhibits excellent anti-reflection performance even when thinned, has high hardness, and has excellent adhesion between the light-shielding layer and the film substrate, and can therefore maintain excellent low gloss for a long time.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. WO2018 / 052044 Summary of the invention
[0008] Technical problem to be solved by the invention
[0009] In recent years, in order to improve the design, a high blackness and significant blackness of optical elements are sought. However, in the existing shading components, since light is scattered on the surface of the shading layer, it is white and the blackness is not significant, making it difficult to take into account both low gloss and high blackness. Although the blackness can be improved while maintaining low gloss by increasing the amount of black particles, there is a problem that the shading layer coating is easy to fall off and the processability is reduced.
[0010] Therefore, the inventors conducted research and found that in a black light-shielding component having a substrate and a light-shielding layer formed on at least one surface of the substrate, by adding black fine particles and low-refractive-index nanoparticles to the resin component of the light-shielding layer, a light-shielding component with low gloss, high blackness, and excellent processability can be obtained (PCT / JP2021 / 042871, hereinafter referred to as "prior application technology"). It has been confirmed that the L value of the above-mentioned black light-shielding component is less than 10, the blackness is high, and the design is excellent. However, it is known that the black obtained by the prior application technology is sometimes bluish, which is not enough to meet the requirements of black close to pure black.
[0011] Technical solutions adopted to solve technical problems
[0012] In view of the above technical problems, the inventors have found through intensive research that by adding a chain structure to the light-shielding layer of a black light-shielding component, the reflectivity on the low-wavelength side can be reduced, and a black color closer to pure black can be obtained, thereby conceiving of the present invention. That is, the black light-shielding component of the present invention includes a substrate and a light-shielding layer formed on at least one surface of the substrate, characterized in that the light-shielding layer contains black microparticles, a chain structure, and a resin component.
[0013] It is preferred that the chain structure include a chain structure having a low refractive index (hereinafter referred to as a "low-refractive-index chain structure").
[0014] Preferably, the low-refractive index chain structure includes chain silica.
[0015] Furthermore, the light shielding layer may further contain low-refractive index nanoparticles (in addition to the low-refractive index chain structure).
[0016] Preferably, the low refractive index nanoparticles comprise magnesium fluoride particles.
[0017] Preferably, the total content of the black fine particles and the chain structure in the light-shielding layer is 50% to 95% of the volume of the entire light-shielding layer.
[0018] Preferably, the total content of the black fine particles, the chain structure, and the low-refractive-index nanoparticles in the light-shielding layer is 40% to 95% of the volume of the entire light-shielding layer.
[0019] Preferably, the content of the chain structure is 1% to 50% of the total volume of the black fine particles and the chain structure.
[0020] In addition, another black light-shielding component of the present invention includes a substrate and a light-shielding layer formed on at least one surface of the substrate, and is characterized in that the light-shielding layer contains black particles, a chain structure and a resin component, and the spectral reflectivity of the black light-shielding component at a wavelength of 360nm on the surface where the light-shielding layer is formed is less than 0.8%.
[0021] Preferably, the chain structure includes chain silica.
[0022] The black light-shielding member may further contain magnesium fluoride particles.
[0023] Furthermore, the present invention provides a black paint composition comprising black fine particles, a chain structure, and a resin component.
[0024] Preferably, the chain structure includes chain silica.
[0025] The black coating composition may further contain magnesium fluoride particles.
[0026] In the present invention, low-refractive-index nanoparticles refer to particles other than low-refractive-index chain structures.
[0027] Effects of the Invention
[0028] The black shading component of the present invention has low gloss, high blackness and is close to pure black (pure black), so it has excellent design and can be suitable for use as a camera unit of mobile phones such as smart phones. In addition, in the case where a black sheet displays black in the next generation display, there is a problem that the black is bluish, and the black shading component of the present invention is close to pure black (pure black), so it can be particularly suitable for use. Moreover, the black shading layer of the black shading component of the present invention has good adhesion, so the peeling of the shading layer coating can also be suppressed during punching, and it has excellent processability. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic cross-sectional view showing the structure of the black light shielding member of the present invention.
[0030] Figure 2 (A) is a schematic cross-sectional view showing the attenuation behavior of incident light in the black light-shielding component of the present invention, and (B) and (C) are schematic cross-sectional views showing the attenuation behavior of incident light in the black light-shielding component of the prior art.
[0031] Figure 3 This is a graph showing the spectral reflectance of the black light shielding members of Example 1, Comparative Example 1, and Comparative Example 2 in the visible light region.
[0032] Figure 4 This is a graph showing the spectral reflectance of the black light shielding members of Example 2, Comparative Example 3, and Comparative Example 4 in the visible light region.
[0033] Explanation of symbols
[0034] 1 Light shielding parts
[0035] 2. Substrate
[0036] 3 Shading layer
[0037] 31 Resin composition
[0038] 32 Black particles
[0039] 33 Chain structure
[0040] 331 Low refractive index nanoparticles DETAILED DESCRIPTION
[0041] The embodiments of the present invention are described in detail below.
[0042] In addition, in this specification, "to" indicating a numerical range means a range including numerical values recorded as the upper limit and the lower limit, respectively. In addition, when only the upper limit unit is recorded in the numerical range, it means that the lower limit is also in the same unit as the upper limit.
[0043] In the numerical ranges described stepwise in the present specification, the upper limit value or the lower limit value described in a certain numerical range may be replaced with the upper limit value or the lower limit value of the numerical range described stepwise in another range.
[0044] Furthermore, in the numerical range described in the present specification, the upper limit value or the lower limit value described in a certain numerical range may be replaced with the value shown in the Examples.
[0045] In this specification, unless otherwise specified, the content rate or content amount of each component in a composition means, when there are plural types of substances corresponding to each component in the composition, the total content rate or content amount of the plural types of substances present in the composition.
[0046] Figure 1 1 is a schematic cross-sectional view showing the structure of the black light-shielding component 1 of the present invention. The black light-shielding component 1 of the present invention comprises a substrate 2 and a light-shielding layer 3 formed on at least one surface of the substrate 2, wherein the light-shielding layer 3 contains black particles 22, a chain structure 33 and a resin component 31. Figure 1 In FIG. 1 , the chain-like structure 33 is simplified and represented only by black dots.
[0047] Figure 2 (B) and (C) are schematic cross-sectional views showing the attenuation behavior of incident light in the black light shielding component of the prior art. In the prior art, since the (spherical) low refractive index nanoparticles 331 are dispersed in the resin component 31, the refractive index of the light shielding layer 3 is reduced, and the light shielding layer 3 and the air layer (n d =1.00) becomes smaller, and the diffuse reflected light on the surface of the light shielding layer 3 is reduced. In addition, the diffuse reflected light is reflected by the black particles ( Figure 2(B) and (C) are not shown in the figure) and are reflected and absorbed, so the light is significantly attenuated. Therefore, in the black light shielding component of the prior application technology, low gloss and high blackness can be achieved. Figure 2 In (B) and (C), the particle sizes of the added low refractive index nanoparticles 331 are different, but the other structures are the same.
[0048] Thus, in the black light shielding component of the prior art, although a high blackness can be achieved, the obtained black is sometimes bluish, and it is difficult to apply it to applications requiring a black color close to pure black. The reasons are considered to be as follows. Figure 2 As shown in (B) and (C), the particle diameter of the low refractive index nanoparticles in the prior art is smaller than the wavelength of visible light, so most of the visible light is not reflected. However, in the case where the particle size of the low refractive index nanoparticles is large ( Figure 2 (B)) and the case where small-diameter, low-refractive-index nanoparticles are densely packed (agglomerated) ( Figure 2 In (C)), short-wavelength visible light is reflected on the surface of the low-refractive-index nanoparticles, so the reflectivity on the short-wavelength side increases, resulting in a bluish black color.
[0049] On the other hand, in the black light shielding member of the present invention in which the chain structures 33 are dispersed, as shown in FIG. Figure 2 As shown in (A), it is not easy to produce aggregation (dense) in the light shielding layer 3. The particle size of the primary particles constituting the chain structure 33 is smaller than the wavelength of visible light. If it is in an unagglomerated state, it not only includes the long wavelength side ( Figure 2 LW) in the image, and also includes light on the short wavelength side ( Figure 2 The reflection of all visible light (SW) in the light shielding layer 3 is suppressed, so that a black color closer to pure black can be obtained. In addition, it is considered that by adding the chain structure 33, a layer containing air (n d =1.00), and air is also sucked between the particles constituting the chain structure inside the shading layer 3, so that the refractive index of the shading layer 3 is reduced. Therefore, the refractive index difference between the shading layer 3 and the air layer becomes smaller, and the reflection of visible light on the surface of the shading layer 3 is further suppressed, which can achieve a black color with higher blackness (low L value) and closer to pure black.
[0050] As described later, in the present invention, low refractive index nanoparticles can also be dispersed in the resin component 31. As a result, it is considered that the refractive index of the light shielding layer 3 is further reduced, and the light shielding layer 3 and the air layer (n d =1.00) becomes smaller, the diffuse reflected light on the surface of the light shielding layer 3 is further reduced, and low gloss and higher blackness can be achieved.
[0051] Hereinafter, the specific material structure of the black light shielding member of the present invention will be described.
[0052] (1) Base material
[0053] The substrate used in the present invention is not particularly limited and may be transparent or opaque. As the substrate material of the present invention, resin, metal, glass, etc. can be used.
[0054] Examples of materials for the resin substrate include polyolefins such as polyethylene, polypropylene, ethylene-propylene copolymers, copolymers of ethylene and α-olefins having 4 or more carbon atoms, polyesters such as polyethylene terephthalate, polyamides such as nylon, ethylene-vinyl acetate copolymers, polyvinyl chloride, polyvinyl acetate and other general-purpose plastics, or engineering plastics such as polycarbonate and polyimide.
[0055] In addition, the metal substrate may be, for example, a metal substrate using a metal such as gold, silver, copper, aluminum, titanium, zinc, beryllium, nickel, tin, or an alloy substrate using an alloy such as phosphor bronze, copper nickel, copper beryllium, stainless steel, brass, duralumin, or the like.
[0056] The glass substrate is not particularly limited, and for example, ultra-thin plate glass (G-Leaf (registered trademark), manufactured by Nippon Electric Glass Co., Ltd.) etc. can be used.
[0057] Among these materials, biaxially stretched polyethylene terephthalate substrates are relatively strong, economical and versatile, and therefore are preferred. In addition, from the viewpoint of heat resistance, polyimide substrates are preferred, and in the case of requiring higher heat resistance, metal substrates composed of copper are preferably used. In the case of resin substrates, by pre-mixing a black colorant such as carbon black or aniline black and adjusting the optical density to 2 or more, preferably 4 or more, a more excellent light-shielding property can be obtained.
[0058] The thickness of the substrate is not particularly limited. When a resin substrate is used, it is preferably 2 μm to 250 μm, and more preferably 4 μm to 100 μm. By setting the thickness of the substrate to the above range, it can be suitable for small and thin optical parts. In addition, in the case of optical elements such as camera units for mobile phones, it is preferably 4 μm to 20 μm.
[0059] When a metal substrate is used, the thickness of the substrate is preferably 6 μm to 40 μm. When used for an optical element such as a camera unit of a mobile phone, the thickness of the substrate is preferably 10 μm to 20 μm.
[0060] When a glass substrate is used, the thickness of the substrate is preferably 5 to 200 μm, more preferably 10 to 100 μm. When used in an optical element such as a camera unit of a mobile phone, the thickness is preferably 10 to 35 μm.
[0061] Either a flat substrate can be used, or a substrate that has been subjected to matte processing to form concavoconvex (roughened portion) on the surface can be used. Through matte processing, it is possible to control the concavoconvex shape of the surface of the shading component after the shading layer is covered, and it is also possible to improve the close contact between the substrate and the shading layer. The matte processing method is not particularly limited, and known methods can be used. For example, in the case where the substrate is a resin substrate, chemical etching, spraying, embossing, calendering, corona discharge, plasma discharge, chemical matting using resin and roughening forming agent, etc. can be used. In addition, it is also possible to make the substrate directly contain a matte agent to form concavoconvex on the surface of the resin substrate. Among the above-mentioned processing methods, from the viewpoints of simplicity of shape control, economy and operability, it is preferred to use a spraying method, especially a sandblasting method.
[0062] In the sandblasting method, the surface properties can be controlled by the particle size of the abrasive used, the blasting pressure, etc. In the embossing method, the surface properties can be controlled by adjusting the embossing roll shape and pressure.
[0063] When the substrate is a metal substrate film, projections and depressions can be formed on the surface by blackening treatment, blasting treatment, etching treatment, or the like.
[0064] (2) Anchoring layer
[0065] Before the shading layer is provided on at least one surface of the above-mentioned substrate, an anchoring layer can also be provided to improve the adhesion between the substrate and the shading layer. As the anchoring layer, a urea resin layer, a melamine resin layer, a polyurethane resin layer, a polyester resin layer, etc. can be applied. For example, the polyurethane resin layer can be obtained by applying a solution containing active hydrogen compounds such as polyisocyanates, diamines, and diols to the surface of the substrate and solidifying it. In addition, in the case of a urea resin layer and a melamine resin layer, it can be obtained by applying a solution containing a water-soluble urea resin or a water-soluble melamine resin to the surface of the substrate and solidifying it. The polyester resin layer can be obtained by applying a solution dissolved or diluted in an organic solvent (methyl ethyl ketone, toluene, etc.) to the surface of the substrate and drying it.
[0066] (3) Light-shielding layer
[0067] The light-shielding layer of the present invention is characterized by containing a resin component, black fine particles and a chain structure.
[0068] The various components are described below.
[0069] 1) Resin composition
[0070] The resin component is an adhesive for the black particles and the chain structure. The material of the resin component is not particularly limited, and any one of a thermoplastic resin and a thermosetting resin can be used. As specific thermosetting resins, acrylic resins, polyurethane resins, phenolic resins, melamine resins, urea resins, diallyl phthalate resins, unsaturated polyester resins, epoxy resins, alkyd resins, etc. can be cited. In addition, as thermoplastic resins, polyacrylate resins, polyvinyl chloride resins, butyral resins, styrene-butadiene copolymer resins, etc. can be cited.
[0071] From the viewpoint of heat resistance, moisture resistance, solvent resistance and surface hardness, thermosetting resins are preferably used. Among thermosetting resins, acrylic resins are particularly preferred in view of flexibility and toughness of the coating. On the other hand, when toughness of the coating is not required, the heat curing process can be omitted, and therefore, thermoplastic acrylic resins are preferably used.
[0072] By adding a curing agent as a constituent of the light-shielding layer, the bridging of the resin component can be promoted. As the curing agent, urea compounds, melamine compounds, isocyanate compounds, epoxy compounds, aziridine compounds, oxazoline compounds, etc. having functional groups can be used. Among them, isocyanate compounds are particularly preferred. Preferably, the mixing ratio of the curing agent is 10% to 50% by mass relative to 100% by mass of the resin component. By adding a curing agent within the above range, a light-shielding layer with a more suitable hardness can be obtained, and even in the case of sliding with other components, the surface shape of the light-shielding layer can be maintained for a long time, and the low gloss can be maintained.
[0073] When a curing agent is used, a reaction catalyst can also be used simultaneously to promote the reaction. Examples of the reaction catalyst include ammonia and ammonium chloride. Preferably, the proportion of the reaction catalyst is in the range of 0.1% to 10% by mass relative to 100% by mass of the curing agent.
[0074] 2) Black particles
[0075] The black light-shielding member of the present invention contains black fine particles in the light-shielding layer.
[0076] like Figure 1 As shown, a fine concavo-convex shape is formed on the surface of the light shielding layer 3 by the black particles 32. And, by scattering light on the concavo-convex surface, the glossiness can be reduced. Furthermore, the light is absorbed by the black particles 32, and the scattering and absorption are repeated, the reflected light is reduced, and a lower glossiness can be achieved.
[0077] exist Figure 12 shows a structure in which the surface of a flat substrate 2 is covered with a light shielding layer 3 containing black fine particles 32, but as described above, a substrate having a concavo-convex shape formed on the surface by matte processing may also be used.
[0078] In the present invention, the concavo-convex shape of the surface of the light-shielding layer 3 can be controlled according to the existing method to achieve the desired glossiness. The surface shape of the light-shielding layer 3 can be controlled by adjusting the surface shape of the substrate 2, the particle size, particle size distribution, content of the black particles 32, and the film thickness of the light-shielding layer 3. In addition, it can also be controlled by adjusting the type of solvent, solid content concentration, and coating amount to the substrate when making the coating liquid. Moreover, it can also be controlled by the coating method of the coating liquid, the drying temperature, time, and the air volume during drying, etc.
[0079] The average particle size of the black particles of the present invention is not particularly limited as long as a light-shielding layer having a desired surface shape can be obtained, and is preferably 0.1 μm to 50 μm, and more preferably 1 μm to 10 μm. By setting the average particle size of the black particles to the above range, fine concavities and convexities can be formed on the surface of the light-shielding layer, further reducing the glossiness.
[0080] In addition, the content of black particles also depends on the average particle size of the black particles, the particle size distribution, the film thickness of the light-shielding layer, and the surface shape of the substrate. If the light-shielding layer as a whole is set to 100 volume %, the content of black particles is preferably 25 volume % to 93 volume %, and more preferably 50 volume % to 88 volume %.
[0081] By setting the content of the black fine particles in the above range, both better blackness and low glossiness can be achieved.
[0082] The volume content (volume occupancy) of the black fine particles in the light-shielding layer can be obtained by converting a cross-sectional photograph of the light-shielding layer into an area occupancy calculated by image analysis or the like.
[0083] As black microparticles, any one of resin particles and inorganic particles can also be used. As the material of resin particles, for example, melamine resin, benzoguanamine resin, benzoguanamine / melamine / formalin condensate, acrylic resin, polyurethane resin, styrene resin, fluororesin, silicone resin etc. can be cited. On the other hand, as the material of inorganic particles, silicon dioxide, aluminum oxide, calcium carbonate, barium sulfate, titanium oxide (titanium dioxide), carbon etc. can be cited. These can be used alone or in combination of two or more.
[0084] In addition, when a non-black material is used, the fine particles can be colored black with an organic or inorganic colorant to form black fine particles. Specific examples of the colorant include carbon black, aniline black, and carbon nanotubes.
[0085] As such a colored material, composite silica, conductive silica, black silica, black acrylic, etc. may be mentioned.
[0086] As composite silica, for example, carbon black and silica are synthesized and composited at the nano level. As conductive silica, for example, conductive silica particles are coated with conductive particles such as carbon black. As black silica, for example, natural ore containing graphite in silica can be cited. In addition, as black acrylic, acrylic copolymers colored with carbon black can be cited.
[0087] In order to obtain more excellent properties, it is preferred to use inorganic particles as black particles. By using inorganic particles as black particles, a black light-shielding component with lower gloss and high blackness can be obtained. As the inorganic particle material used as the black particles, carbon is preferred. Among carbons, porous carbon particles are particularly preferably used. Compared with the case of using non-porous black particles, the following effects can be obtained by using porous carbon particles. That is, light is repeatedly reflected and absorbed and attenuated on the surface and inside of the particles. In addition, in the case of containing low-refractive index nanoparticles, more low-refractive index nanoparticles can be kept on the surface and inside of the black particles, and therefore, the glossiness can be further reduced.
[0088] The shape of the black fine particles is not particularly limited, but it is preferred to use ideally spherical black fine particles in consideration of the flow characteristics of the coating liquid, coating properties, and the slip properties of the obtained light-shielding layer.
[0089] 3) Chain structure
[0090] The light-shielding member of the present invention is characterized in that the light-shielding layer contains a chain structure.
[0091] like Figure 1 As shown, in the black light shielding member 1 of the present invention, a fine concavo-convex shape is formed on the surface of the light shielding layer 3 by the black particles 32. Here, in the resin component 31 (binder resin) of the light shielding layer 3, the black particles 32 and the chain structure 33 are dispersed, and the surface of the black particles 32 on the air layer side has a structure covered by the resin component 31 in which the chain structure 33 is dispersed. In addition, as shown above, Figure 1 In FIG. 1 , the chain-like structure 33 is simplified and represented by black dots.
[0092] In the black light shielding member of the present invention in which the chain structures 33 are dispersed, as Figure 2 As shown in (A), it is not easy to produce aggregation (dense) in the light shielding layer 3. The particle size of the primary particles constituting the chain structure 33 is smaller than the wavelength of visible light. If it is in an unagglomerated state, it not only includes the long wavelength side ( Figure 2 LW) in the image, and also includes light on the short wavelength side ( Figure 2 The reflection of all visible light (SW) in the light shielding layer 3 is suppressed, so that a black color closer to pure black can be obtained. In addition, it is considered that by adding the chain structure 33, a layer containing air (n d =1.00), and air is also sucked in between the particles constituting the chain structure 33 inside the shading layer 3, so that the refractive index of the shading layer 3 is reduced, and thus the refractive index difference between the shading layer 3 and the air layer becomes smaller, and the reflection of visible light on the surface of the shading layer 3 is suppressed, so that a black color with a higher blackness and closer to pure black can be achieved.
[0093] The chain structure is a structure having a long chain portion and a side chain portion, including not only a chain shape but also a pearl necklace shape, wherein in the long chain portion, nano-sized primary particles are connected into multiple pieces and extend in a constant direction, and the side chain portion branches out from the long chain portion.
[0094] The average particle diameter of the primary particles constituting the chain structure is preferably in the range of 3 to 50 nm, and the number of primary particles constituting one chain structure is preferably 2 to 100. In addition, the average length of the long chain portion of the chain structure is preferably in the range of 6 to 500 nm, and the ratio of the average length to the average particle diameter of the primary particles is preferably in the range of 2 to 50.
[0095] As the chain structure, for example, chain silicon dioxide, chain zirconium oxide, chain antimony oxide, chain aluminum oxide (aluminum oxide) etc. can be cited. The chain structure preferably includes a low-refractive index chain structure, wherein it preferably includes chain silicon dioxide. In addition, here, the low refractive index refers to a refractive index of 1.5 or less.
[0096] The chain structure as described above can be used alone as one chain structure, or can be mixed with two or more chain structures with different components, chain structures with different average particle diameters of primary particles, chain structures with different average lengths of the long chain parts of the chain structures, and chain structures with different ratios of average length to the average particle diameter of the primary particles. As a combination of chain structures with different components, for example, there can be cited: a combination of two or more low-refractive index chain structures and chain structures without low refractive index (hereinafter referred to as "non-low-refractive index chain structures"), a combination of two or more chain structures with different components in low-refractive index chain structures, or a combination of two or more chain structures with different components in non-low-refractive index chain structures.
[0097] The total content of the black particles 32 and the chain structure 33 in the light-shielding layer 3 of the black light-shielding component 1 of the present invention is not particularly limited as long as the desired properties can be obtained, but when the light-shielding layer as a whole is set to 100 volume %, the total content is preferably 50 volume % to 95 volume %, and more preferably 60 volume % to 90 volume %.
[0098] In the above range, while maintaining excellent bonding strength, the blackness is further improved and the reflectivity is reduced, and a black color closer to pure black can be obtained.
[0099] In addition, there is no particular limitation on the mixing ratio of the black particles 32 and the chain structure 33 as long as the desired characteristics can be obtained, but the chain structure 33 is preferably 1% to 50% by volume, and more preferably 2% to 25% by volume, relative to the total amount of the black particles 32 and the chain structure 33. By adjusting the mixing ratio of the black particles 32 and the chain structure 33 to the above range, better low gloss and blackness can be obtained. In addition, within the above range, the interface between the substrate 2 and the light-shielding layer 3 and the interface between the particles and the resin component 31 are fully bonded, so the light-shielding layer 3 will not peel off during processing, and excellent processability can be achieved.
[0100] The volume content (volume occupancy) of the chain structures 33 in the light shielding layer 3 can also be obtained by converting a cross-sectional photograph of the light shielding layer 3 into an area occupancy calculated by image analysis or the like.
[0101] 4) Low refractive index nanoparticles (except low refractive index chain structures)
[0102] The light-shielding component of the present invention can contain low-refractive index nanoparticles in the light-shielding layer. When the aforementioned chain structure is a low-refractive index chain structure, although it also has the function of low-refractive index nanoparticles, different low-refractive index nanoparticles can also be added. In addition, when the chain structure is a non-low-refractive index chain structure, low-refractive index nanoparticles can be added.
[0103] The following, Figure 1 Detailed Description is given of the attenuation behavior of incident light when the chain structures 33 dispersed in the light shielding layer 3 are low-refractive-index chain structures or when low-refractive-index nanoparticles are added in addition to the chain structures 33.
[0104] The incident light reaches the surface of the black particles 32 via the resin component 31 dispersed with a low-refractive index chain structure, or a chain structure and low-refractive index nanoparticles (hereinafter referred to as "low-refractive index nanoparticles, etc."), a part of which is transmitted and absorbed by the black particles, and a part of which becomes reflected light. Here, since the black particles 32 are covered by the resin component 31 dispersed with the low-refractive index nanoparticles, etc., the reflection on the surface of the resin component 31 is suppressed. Therefore, it can be considered that, compared with the light-shielding component in which the black particles 32 are covered with the resin component 31 that does not contain the low-refractive index nanoparticles, etc., more light is transmitted through the resin component 31, and more light is absorbed by the black particles 32, so the reflected light can be effectively reduced.
[0105] In addition, a part of the incident light reaching the surface of the light shielding layer 3, which is the interface between the air layer and the resin component 31 not covered with the black particles 32, is transmitted through, and a part is reflected. In the black light shielding component 1 of the present embodiment, compared with a light shielding component having a resin component that does not contain low-refractive index nanoparticles, etc., since low-refractive index nanoparticles, etc. are dispersed in the resin component 31, the light reflected at the interface between the air layer and the resin component 31 of the light shielding layer 3 is reduced, and the light transmitted through the resin component 31 of the light shielding layer 3 is increased.
[0106] Then, the light transmitted through the resin component 31 of the light shielding layer 3 is reflected at the interface between the substrate 2 and the light shielding layer 3 , that is, at the surface of the substrate 2 , and is absorbed by the black particles 32 in the light shielding layer 3 .
[0107] In the present embodiment, it is considered that due to the synergistic effect of the effect of the chain structure and the effect of the low refractive index nanoparticles, etc., a black color with low gloss and high blackness close to pure black can be further realized.
[0108] Here, low refractive index nanoparticles refer to nanoparticles with a refractive index of less than 1.5 and an average particle size of the primary particles less than 250nm. The average particle size of the primary particles of the low refractive index nanoparticles is preferably 1nm to 200nm, more preferably 5nm to 150nm, further preferably 10nm to 100nm, and most preferably 20nm to 80nm.
[0109] By setting the refractive index of the low-refractive-index nanoparticles and the average particle size of the primary particles within the above ranges, the refractive index of the light-shielding layer can be effectively reduced, thereby further improving the blackness.
[0110] As long as the material of the low refractive index nanoparticles meets the above conditions, it can be either an inorganic material or an organic material, or a mixed material or a composite material of an organic material and an inorganic material. As an inorganic material, for example, thiozeolite (Na5Al3F 14 , n d=1.33), cryolite (Na3AlF6, n d =1.35), sodium fluoride (NaF, n d =1.34), lithium fluoride (LiF, n d =1.36), aluminum fluoride (AlF3, n d =1.36), magnesium fluoride (MgF2, n d =1.38), calcium chloride (CaF2, n d =1.43), barium fluoride (BaF2, n d =1.48) and other fluorides, silicon oxide (silicon dioxide: SiO2, n d =1.47) and other oxides, calcium carbonate (CaCO3, n d =1.50) and other carbonates.
[0111] In addition, as an organic material, for example, acrylic resin (n d =1.49~1.50), styrene resin, silicone resin (n d = about 1.43), fluororesin (n d = about 1.35) etc. In addition, an organic-inorganic hybrid material (organic-inorganic nanocomposite material) composed of a metal oxide and an organic molecule can also be used.
[0112] From the viewpoint of chemical stability, among the materials of the above-mentioned low-refractive-index nanoparticles, magnesium fluoride, calcium fluoride, lithium fluoride, calcium carbonate, silicon oxide (silicon dioxide), and the like are preferably used.
[0113] As low refractive index nanoparticles, nano spherical particles (spherical nanoparticles), nano hollow particles (hollow nanoparticles), nano clay particles, nano fiber particles, etc. can be cited. In particular, by using nano hollow particles, the refractive index of the light shielding layer is further reduced, and diffuse reflection is reduced, so it is effective to improve blackness. As nano hollow particles, hollow silica nanoparticles, etc. can be used.
[0114] In addition, low-refractive index nanoparticle (except the low-refractive index chain structure) can also use the structure different from the low-refractive index chain structure composition or the structure identical with the low-refractive index chain structure composition separately or by mixing two or more.According to such structure, blackness can be further improved.For example, it can be confirmed that, compared with the situation of adding chain silicon dioxide separately, by using chain silicon dioxide and magnesium fluoride nanoparticle simultaneously, reflectivity descends in the whole visible light domain including the short wavelength side, and can obtain the black closer to pure black.
[0115] The total content of black microparticles, chain structures and low refractive index nanoparticles in the light-shielding layer of the black light-shielding component of the present invention is not particularly limited as long as the desired properties can be obtained, but when the light-shielding layer as a whole is set to 100 volume %, the total content is preferably 40 volume % to 95 volume %, and more preferably 60 volume % to 90 volume %.
[0116] In addition, for the mixing ratio under the situation of using chain structure and low-refractive index nanoparticle, as long as desired characteristic can be obtained, there is no particular limitation, but relative to the total amount of chain structure and low-refractive index nanoparticle, low-refractive index nanoparticle (except low-refractive index chain structure) is preferably 1 volume %~90 volume %, more preferably 10 volume %~80 volume %.By adjusting the mixing ratio of chain structure and low-refractive index nanoparticle (except low-refractive index chain structure) in light-shielding layer to above-mentioned scope, more excellent low glossiness and blackness can be obtained.In addition, according to said structure, the interface of substrate and light-shielding layer and the interface of particle and resin component are fully bonded, therefore, light-shielding layer can not be peeled off when processing, and excellent processability can be realized.
[0117] The volume content (volume occupancy) of the low refractive index nanoparticles (excluding the low refractive index chain structures) in the light shielding layer can also be determined by converting a cross-sectional photograph of the light shielding layer into an area occupancy calculated by image analysis or the like.
[0118] In the present invention, as the constituent components of the light shielding layer, a leveling agent, a thickener, a pH adjuster, a lubricant, a dispersant, a defoaming agent, etc. may be further added as necessary.
[0119] As the lubricant, in addition to polytetrafluoroethylene (PTFE) particles which are solid lubricants, polyethylene wax, silicone particles, etc. can also be used.
[0120] The above components are added to an organic solvent or water and mixed and stirred to prepare a uniform coating liquid. Examples of the organic solvent include methyl ethyl ketone, toluene, propylene glycol monomethyl ether acetate, ethyl acetate, butyl acetate, methanol, ethanol, isopropyl alcohol, and butanol.
[0121] The light shielding layer is formed by directly applying the obtained coating liquid to the surface of the substrate or the anchor layer formed in advance and drying. The coating method is not particularly limited, and spray coating, bar coating, roll coating, doctor blade coating, etc. can be used.
[0122] The coating liquid can be suitably used as an excellent black coating material by appropriately changing the concentration and the solvent according to the application.
[0123] The thickness of the light shielding layer in the present invention is preferably 1 μm to 100 μm, more preferably 2 μm to 50 μm, and even more preferably 3 μm to 25 μm.
[0124] By setting the thickness of the light-shielding layer to the above range, the desired blackness and anti-reflection effect can be appropriately obtained. In addition, the thickness of the light-shielding layer is the height from the substrate surface to the base portion of the light-shielding layer that is not more prominent than the black particles. The thickness of the above-mentioned light-shielding layer can be measured based on JIS K7130.
[0125] Hereinafter, the characteristics of the black light shielding member of the present invention will be described.
[0126] (1) Glossiness
[0127] The glossiness of the surface of the black light-shielding member of the present invention on which the light-shielding layer is formed is preferably 1% or less, more preferably 0.8% or less, further preferably 0.6% or less, and most preferably 0.4% or less with respect to incident light at an incident angle of 60°. By adjusting the glossiness of the black light-shielding member of the present invention with respect to incident light at an incident angle of 60° to the above range, flare and ghosting phenomena caused by diffuse reflection of light can be more effectively prevented.
[0128] The above glossiness can be obtained by measuring the specular glossiness at an incident angle of 60° in accordance with JIS Z8741.
[0129] (2) Chromaticity in the black and blue directions
[0130] The L value of the surface of the black light-shielding member of the present invention on which the light-shielding layer is formed is preferably 10 or less, more preferably 8 or less, and further preferably 7 or less. By adjusting the L value of the black light-shielding member of the present invention to the above range, the blackness is high, the black color is prominent, and the design is excellent, so it can be suitably used as a camera unit of a mobile phone such as a smartphone.
[0131] The L value is an L* value representing brightness in the L*a*b* color space calculated based on JIS Z8781-4. In addition, a* and b* are chromaticities representing hue and saturation, a* represents the red direction, -a* represents the green direction, b* represents the yellow direction, and -b* represents the blue direction. In the present invention, -b* is a value closer to 0 than 0.8, that is, b* is preferably greater than -0.8 and less than 0.8, and more preferably greater than -0.4 and less than 0.4. By setting b* to the above range, the bluish color of the black light-shielding component can be suppressed, and it can be suitable for use in applications requiring a black color closer to pure black.
[0132] (3) Spectral reflectivity
[0133] The spectral reflectivity of the surface of the black light-shielding component of the present invention on which the light-shielding layer is formed relative to light in the visible light region is preferably 0.8% or less, and more preferably 0.65% or less. By adjusting the spectral reflectivity of the black light-shielding component of the present invention to the above range, a black color closer to pure black can be achieved. In addition, since the problem of increased spectral reflectivity becomes more serious in the lower wavelength region, the reflectivity of light with a wavelength of 360nm is sometimes used for judgment in this specification.
[0134] The spectral reflectance can be measured by a spectrophotometer (CM-5: manufactured by Konica Minolta Co., Ltd.) in accordance with JIS Z8722.
[0135] (4) Bonding strength
[0136] The bonding strength of the surface of the black light-shielding component of the present invention on which the light-shielding layer is formed is preferably 1N / 25mm or more, more preferably 2N / 25mm or more, further preferably 4N / 25mm or more, and most preferably 6N / 25mm or more. By adjusting the bonding strength of the black light-shielding component of the present invention to the above range, it is possible to prevent the light-shielding layer coating from peeling off during processing, thereby improving processability.
[0137] Adhesion can be determined by measuring the resistance when 31B tape (manufactured by Nitto Denko Corporation) affixed to the light shielding layer is peeled off in a 180° direction in accordance with JIS Z0237. The 31B tape can be affixed to the light shielding layer using a 2 kg roller.
[0138] Example
[0139] The present invention will be described in more detail with reference to the following Examples, but the present invention is not limited to these Examples. In the Examples, "%" and "part" represent mass % and mass part unless otherwise specified.
[0140] <Structure of black light shielding member>
[0141] (1) Base material
[0142] (1-1) Polyimide film Kapton 50MBC (thickness 12 μm), manufactured by DU PONT-TORAY CO., LTD.
[0143] (2) Light-shielding layer
[0144] (a) Microparticles
[0145] (a1) Porous carbon particles with an average particle size of 3 μm and a refractive index of about 1.55
[0146] (a2) Carbon particles average particle size: 250 nm, refractive index: 1.80
[0147] (a3) Acrylic resin microparticles Average particle size: 3 μm, refractive index: 1.49
[0148] (b) Chain structure
[0149] (b1) Chain silica: Average particle size: 12 nm
[0150] (b2) Chain alumina: Average particle size: 10 nm
[0151] (c) Low refractive index nanoparticles
[0152] (c1) Magnesium fluoride: average particle size: 50 nm, refractive index: about 1.38
[0153] (c2) Spherical silica: average particle size: 45 nm, refractive index: about 1.44
[0154] (c3) Spherical silica: average particle size: 12 nm, refractive index: about 1.44
[0155] (c4) Hollow silica: average particle size: 60nm, refractive index: about 1.30
[0156] (d) Resin
[0157] (d1) Acrylic resin: Paraclon Precoat 200 (Japanese: パラクロンプレコート200), manufactured by Negami Industries Co., Ltd.
[0158] (d2) Acrylic resin: Acridic A801 (Japanese: アクリディックA801), manufactured by DIC Corporation
[0159] (e) Curing agent
[0160] (e1) Polyisocyanate: Takenate D110N, manufactured by Mitsui Chemicals, Inc.
[0161] (Examples 1 to 10, Comparative Examples 1 to 6, Reference Examples 1 to 2)
[0162] The components of the light-shielding layer were added to a solvent at the mixing ratio (solid content mass) shown in Tables 1 to 2, and stirred and mixed to obtain a coating liquid. Here, methyl ethyl ketone and toluene were used as the solvent.
[0163] The coating liquids of the compositions in Table 1 and Table 2 were applied to one surface of a polyimide film substrate and then dried at 150° C. for 5 minutes to form a light shielding layer. The polyimide film was not provided with an anchor layer, but the coating liquid was directly applied to the substrate surface.
[0164] Tables 1 and 2 show the results of evaluation of the average film thickness, glossiness with respect to incident light at an incident angle of 60°, L value, b* value, and spectral reflectance of the light-shielding layer coating films obtained by the above-mentioned methods.
[0165] Tables 1 and 2 also show the results of evaluation of glossiness, L value, b* value, and spectral reflectance with respect to incident light at an incident angle of 60° according to the following evaluation criteria.
[0166] (Evaluation criteria for glossiness relative to incident light at an incident angle of 60°)
[0167] ×: 1% or more (does not satisfy the required characteristics of the present invention)
[0168] ○: 0.4% or more and less than 1% (excellent)
[0169] ◎: Less than 0.4% (very excellent)
[0170] (Evaluation criteria of L value)
[0171] ×: more than 10 (does not satisfy the required characteristics of the present invention)
[0172] ○: More than 7 points and less than 10 points (excellent)
[0173] ◎: 7 or less (very good)
[0174] (Evaluation criteria of b* value)
[0175] ×: less than -0.8, or more than 0.8
[0176] ○: -0.8 or more and less than -0.4, or more than 0.4 and less than 0.8
[0177] ◎: -0.4 or more and 0.4 or less
[0178] (Evaluation criteria of spectral reflectance in the short wavelength region: Evaluation is performed based on the reflectance of light at 360 nm)
[0179] ×: more than 0.8% (does not meet the requirements of the present invention)
[0180] ○: More than 0.65% and 0.8% or less (excellent)
[0181] ◎: 0.65% or less (very excellent)
[0182] (Evaluation criteria for bonding strength)
[0183] ×: Less than 3N / 25mm (including cases where the film peels off and cannot be measured)
[0184] ○: 3N / 25mm or more
[0185] Reference Example 1 in Table 1 shows the results of evaluating the characteristics of a sample made from the composition of an existing general shading component. The shading component of Reference Example 1 has a structure in which a shading layer containing a resin component, a matting agent and a black pigment is covered on a substrate. In addition, in Reference Example 1, the matting agent is acrylic resin microparticles (colorless and transparent), and the black pigment is carbon microparticles. It can be considered that in such an existing shading component, the fine concavo-convex shape on the surface of the shading layer formed by the matting agent causes light to be scattered, and the light is absorbed by the black pigment dispersed in the resin component, thereby reducing reflected light, thereby achieving low gloss.
[0186] However, it can be confirmed that in Reference Example 1, the bonding strength is 10.7 N / 25 mm, which is good, but the glossiness at 60° is 2.7%, the L value is as high as 26.5, and the reflectivity is high in the entire visible light range, and the low glossiness and blackness at the target level of the present invention cannot be obtained. This is because the light-shielding layer of Reference Example 1 has a high refractive index because carbon particles are dispersed in the light-shielding layer, and the difference in refractive index with the air layer and the aggregation of carbon particles increase the diffuse reflected light on the surface of the light-shielding layer, and the diffuse reflected light is scattered by the uneven shape of the surface and appears white.
[0187] [Table 1]
[0188]
[0189] Reference Example 2 shows the results of evaluating the characteristics of a sample made of acrylic resin particles (colorless and transparent) added as black particles instead of matting agents in order to reduce the L value, that is, to increase the blackness. The light-shielding component of Reference Example 2 has a structure in which a light-shielding layer containing a resin component and black particles is covered on a substrate. It can be seen that in the light-shielding component of Reference Example 2, if the glossiness at 60° is 0.1%, low gloss can be achieved, and if the L value is 7.8, it is greatly reduced compared with Reference Example 1, and high blackness can be obtained. However, in Reference Example 2, the bonding strength is as low as 0.1N / 25mm, and it can be expected that the powder constituting the light-shielding layer will fall off even if it is only lightly touched during processing, making it difficult to put it into practical use. It can be considered that this is because in Reference Example 2, in order to reduce the L value to the desired value, the proportion of the resin component in the light-shielding layer is reduced by increasing the amount of black particles added, so that the substrate and the light-shielding layer and the resin component and the black particles cannot be fully bonded.
[0190] In Comparative Example 1, the amount of black particles is set to 1 / 2 of that of Reference Example 2, and spherical silica nanoparticles (average particle size: 45nm, refractive index: 1.44) are added as low refractive index nanoparticles. It can be confirmed that the sample of Comparative Example 1 has a low glossiness if the glossiness at 60° is 0.1%, and has a better blackness than Reference Example 2 if the L value is 6.7. It can be considered that this is because, by dispersing low refractive index nanoparticles in the light-shielding layer, as described above, the refractive index of the light-shielding layer is reduced, and the refractive index difference with the air layer is reduced, thereby reducing the scattered light on the surface of the light-shielding layer, and then the scattered light is absorbed and reflected by the black particles, so that the light is significantly attenuated. In addition, it can be confirmed that in Comparative Example 1 containing black particles and low refractive index nanoparticles, the bonding strength is also above 3N / 25mm, and the adhesiveness is also good.
[0191] However, it can be confirmed that, as shown in Table 1 and Figure 3 As shown, in Comparative Example 1, the spectral reflectivity of visible light on the short wavelength side rises sharply. It can be considered that in Comparative Example 1, since the particle size of the spherical silica nanoparticles is relatively large, although the visible light on the long wavelength side is transmitted, the visible light on the short wavelength side is easily reflected. In this way, it can be expected that in Comparative Example 1 where the spectral reflectivity on the short wavelength side is high, the application of a black shading component close to pure black with excellent design properties is relatively difficult.
[0192] Next, a light-shielding layer coating film was prepared and evaluated in the same manner as in Comparative Example 1 except that the average particle size of the spherical silica nanoparticles was changed from 45 nm to 12 nm (Comparative Example 2).
[0193] It was confirmed that in Comparative Example 2, the glossiness at 60° was 0.1% and the L value was 6.6, which was similar to Comparative Example 1, the film had low glossiness and high blackness, and also good adhesiveness.
[0194] In addition, it can be confirmed that, as shown in Table 1 and Figure 3 As shown in FIG. 1 , in Comparative Example 2, the spectral reflectance on the short wavelength side is particularly reduced compared to Comparative Example 1. This is considered to be because the average particle size of the spherical silica nanoparticles in Comparative Example 2 is smaller than that in Comparative Example 1. Figure 2 As shown in (C), the reflection of the incident light is limited to the portion where the spherical silica nanoparticles are densely packed, and thus the reflection of the incident light on the surface is suppressed.
[0195] However, if Figure 3 As shown, in Comparative Example 2, the spectral reflectance increases and exceeds 0.8% on the short wavelength side, and there is room for improvement in application as a black light shielding member having excellent design properties and close to pure black.
[0196] It can be confirmed that in Example 1, in which chain silica (average particle size: 12 nm) is added instead of the spherical silica nanoparticles of Comparative Examples 1 and 2, the glossiness is low, the blackness is high, and the adhesion is good, as in Comparative Examples 1 and 2. Figure 3 As shown, it can be seen that in Example 1, in the entire visible light range, if the spectral reflectance is less than 0.8%, excellent reflection characteristics are shown, and the b* value is close to zero, and a black color close to pure black can be achieved. It is believed that this is because the aggregation of particles is suppressed by adding a chain structure, and a space containing air is formed between the particles forming the chain structure, and the refractive index of the light-shielding layer is reduced.
[0197] A sample was prepared and evaluated in the same manner as in Example 1 except that chained alumina was added instead of chained silica in Example 1 (Example 10). It was confirmed that in Example 10, the glossiness at 60° was 0.1%, the L value was 7.1, and it was low gloss and high blackness, and the adhesion was good, as in Example 1. Moreover, it was found that in Example 10, in the entire visible light range, if the spectral reflectance was 0.8% or less, excellent reflection characteristics were shown, the b* value was also close to zero, and a black color close to pure black could be achieved.
[0198] As described above, it can be confirmed that in Examples 1 and 10 containing a chain structure, the increase in the spectral reflectance on the short wavelength side is suppressed, and a lower value of the spectral reflectance at 360 nm can be obtained compared to Comparative Examples 1 and 2 not containing a chain structure. It can be seen that by using a chain structure, the phenomenon of black being bluish is suppressed regardless of its material, and a black color closer to pure black can be achieved.
[0199] In addition, when comparing Example 1 and Example 10, in Example 1 using a low refractive index chain structure, i.e., chain silica, a lower spectral reflectance can be obtained in the entire visible light range. Therefore, it can be considered that it is preferable to use a low refractive index chain structure as the chain structure.
[0200] Next, the following further studies were conducted using chain silica, which is a low-refractive-index chain structure, as the chain structure.
[0201] In Example 2, low-refractive nanoparticles, i.e., magnesium fluoride, are further added to the structure of Example 1. As shown in Table 1, it can be seen that in Example 2, low gloss and good adhesion can be obtained in the same manner as in Example 1. In addition, it can be confirmed that the L value of Example 2 is 5.2, and the blackness is further improved compared to Example 1. In addition, as shown in Tables 1 and Figure 4 As shown, it can be seen that in Example 2, the spectral reflectance is further reduced in the entire visible light range compared to Example 1, and a black color closer to pure black can be obtained.
[0202] It can be seen that in Comparative Examples 3 and 4, where spherical silica nanoparticles with average particle diameters of 45 nm and 12 nm were used instead of the chain silica of Example 2, Figure 4 As shown in FIG. 1 , the spectral reflectance on the short wavelength side rises sharply, and as shown in Table 1, the b* value also shifts to the blue side, and a black color close to pure black as in Example 2 is not obtained.
[0203] It can be seen that in Comparative Example 5, in which hollow nano-silica particles with an average particle size of 60 nm are used instead of the chain silica of Example 2, the spectral reflectance on the short wavelength side decreases compared to Comparative Examples 3 and 4, and the b* value also tends to zero, and the blue bias is improved, but the result of Example 2 is not achieved.
[0204] From the above results, it was confirmed that when low-refractive-index nanoparticles are further added to the black light-shielding member of the present invention containing a chain structure, a significant synergistic effect can be obtained.
[0205] Table 2 shows the results of evaluating various properties of samples prepared by setting the addition amount (mass) of black fine particles and chain silica to be the same and changing the total addition amount of black fine particles and chain silica relative to the adhesive resin component (Example 3, Example 1 and Example 4).
[0206] It can be seen that in Example 3, where the total amount of the black particles and the chain structure is 80% by volume and the light-shielding layer is 100% by volume, a black color with low gloss, high blackness and suppressed bluish color can be obtained. Although not described in the table, it can be confirmed that Example 3 has sufficient bonding strength.
[0207] In contrast, in Example 1 and Example 4, in which the total amount of black fine particles and chain structures relative to the volume of the entire shading layer is increased to 82 volume % and 83 volume %, respectively, there is a tendency for the L value to decrease and the reflectivity to decrease in the entire wavelength domain including the low wavelength side, and it can be confirmed that the addition of particles is effective for achieving a black color close to pure black. However, the addition of a large amount of particles will lead to a decrease in the bonding strength of the shading layer and an increase in cost. Therefore, it can be considered that if the shading layer as a whole is set to 100 volume %, the total content of black fine particles and chain structures in the black shading component of the present invention is preferably 50 volume % to 95 volume %, and more preferably 60 volume % to 90 volume %.
[0208] In Examples 5, 6 and 2, the volume ratio of the total amount of black microparticles, chain structures (chain silica) and low-refractive index nanoparticles (magnesium fluoride) relative to the volume of the entire light-shielding layer is set to be constant, and the volume ratio of the chain structures (chain silica) and low-refractive index nanoparticles (magnesium fluoride) is also set to be constant, and the volume ratio of the black fine particles relative to the volume total amount of the chain structures (chain silica) and low-refractive index nanoparticles is changed. The results of evaluating the various properties of each sample are shown in Table 2.
[0209] In Examples 5, 6 and 2, the total amount of black particles, chain silicon dioxide and magnesium fluoride is 82% when the light shielding layer as a whole is set to 100% by volume. In addition, the content of black particles relative to the light shielding layer as a whole in Examples 5, 6 and 2 is 70%, 71% and 73% by volume, respectively.
[0210] It is found that a black color with low gloss, high blackness and suppressed bluish tint can be obtained in Example 5. Although not shown in the table, it was confirmed that Example 5 had sufficient adhesive strength.
[0211] It can be confirmed that in Example 6, the L value is lowered compared to Example 5, the reflectance is lowered in the entire wavelength range, and the b* value is closer to zero, so that black closer to pure black can be obtained.
[0212] It can be confirmed that in Example 2, the L value decreases, the reflectivity decreases in the entire wavelength range, and the b* value is biased toward zero, and a black color closer to pure black can be obtained compared to Example 5. Therefore, there is a tendency that the higher the content of black particles relative to the entire light-shielding layer, the lower the b* value.
[0213] From the above structure, it can be confirmed that the content of black fine particles is important for obtaining a black color with a high blackness and closer to pure black.
[0214] [Table 2]
[0215]
[0216] In Examples 1, 7, 8, 9 and Comparative Example 6 in Table 2, the volume of the black particles relative to the volume of the entire light-shielding layer was set to 73% or 74%, and the content of chain silica relative to the total amount of the chain structure and the black particles was set to 10 volume %, 7.7 volume %, 5.3 volume %, 2.7 volume % and 0 volume %, respectively. In addition, Example 1 did not contain magnesium fluoride, and Comparative Example 6 did not contain chain silica.
[0217] It can be seen that in Examples 1, 7, 8 and 9, the L value and b* value are low (close to zero), and the spectral reflectivity in the entire wavelength range also meets the required values of the present invention. In contrast, it can be seen that in Comparative Example 6 that does not contain a chain structure, the L value increases, the b* value is far away from zero, and the spectral reflectivity etc. increase significantly in the entire wavelength range. From the above results, the effect of the present invention containing a chain structure can be confirmed.
[0218] Industrial Applicability
[0219] The present invention has high industrial applicability as a black light-shielding component for optical elements such as camera units of mobile phones, etc. Moreover, the coating liquid for forming the light-shielding layer of the black light-shielding component of the present invention, that is, the coating liquid containing black microparticles, chain structures and resin components, also has industrial applicability as a black paint.
Claims
1. A black light-shielding component, comprising a substrate and a light-shielding layer formed on at least one surface of the substrate, characterized in that: The light shielding layer contains black fine particles, a chain structure and a resin component.
2. The black light shielding member according to claim 1, wherein: The chain structure includes a low-refractive-index chain structure.
3. The black light shielding member according to claim 1, wherein: The chain structure includes chain silicon dioxide.
4. The black light shielding member according to any one of claims 1 to 3, wherein: The light shielding layer further includes low-refractive index nanoparticles in addition to the low-refractive index chain structure.
5. The black light shielding member according to claim 4, wherein: The low refractive index nanoparticles include magnesium fluoride particles.
6. The black light shielding member according to claim 1, wherein: The total content of the black fine particles and the chain structure in the light-shielding layer is 50% to 95% of the volume of the entire light-shielding layer.
7. The black light shielding member according to claim 4, wherein: The total content of the black fine particles, the chain structure and the low refractive index nanoparticles in the light shielding layer is 40% to 95% of the volume of the entire light shielding layer.
8. The black light shielding member according to claim 1, wherein: The content of the chain structure is 1% to 50% of the total volume of the black fine particles and the chain structure.
9. A black light-shielding component, comprising a substrate and a light-shielding layer formed on at least one surface of the substrate, characterized in that: The light shielding layer contains black particles, chain structures and resin components. The spectral reflectance of the black light-shielding member at a wavelength of 360 nm on the surface on which the light-shielding layer is formed is 0.8% or less.
10. The black light shielding member according to claim 9, wherein: The chain structure includes chain silicon dioxide.
11. The black light shielding member according to claim 9 or 10, wherein: Also included are magnesium fluoride particles.
12. A composition for black paint, characterized in that: Contains black particles, chain structures and resin components.
13. The black paint composition according to claim 12, wherein: The chain structure includes chain silicon dioxide.
14. The black paint composition according to claim 12 or 13, wherein: Also included are magnesium fluoride particles.