Resin composition for molding, method for producing sealing structure, and sealing structure
By using a resin composition of an epoxy resin composition and an inorganic filler material under low temperature conditions, the problems in the prior art that the resin composition requires high temperature for curing and the sealing structure has insufficient adhesion are solved, achieving high mechanical strength and waterproofing. Excellent sealing effect.
Patent Information
- Application Number
- CN202380027928.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-29
AI Technical Summary
Existing resin compositions require high-temperature treatment during the curing process, and there is room for improvement in the adhesion and waterproofness of the sealed structure, especially when sealing with structures such as electronic components or stators.
Provided is a resin composition for molding, which includes an epoxy resin, a curing agent and a curing catalyst, combined with an inorganic filler material, can be cured under low temperature conditions, has excellent bending elastic modulus and glass transition temperature, and can be passed through a transfer molding machine and Specific process conditions form a sealed structure.
It is possible to improve the tightness and waterproofness of sealed electronic components or stator structures at low temperatures, reduce the risk of thermal damage, and improve the mechanical strength and heat resistance of sealed structures.
Smart Images

Figure CN118872047A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a molding resin composition, a method for producing a sealing structure, and a sealing structure. Background Art
[0002] In order to protect electronic components such as semiconductor parts and structures such as stators from the external environment, the method of sealing with thermosetting resins is widely used. In particular, the transfer molding method using epoxy resin as the sealing resin has excellent economical and productivity and is suitable for mass production, so it has become the mainstream of resin sealing.
[0003] As a technology for using a resin material for a stator core, there is a technology described in Patent Document 1 (Japanese Patent Application Laid-Open No. 2003-284277). This document describes a rotating electric machine having: a stator having a plurality of coils wound at predetermined intervals on a stator core formed by stacking a plurality of electromagnetic steel sheets, a rotor held rotatably relative to the stator, and a cooling frame to fix the stator, wherein a highly thermally conductive composite material composed of a thermosetting resin having an anisotropic structure in the resin component is arranged in a slot of a winding portion of the stator, and by this structure, a rotating electric machine is provided in which heat generated by the coil is easily transferred and has good heat dissipation.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2003-284277 Summary of the invention
[0007] Technical issues to be solved by the invention
[0008] However, in the prior art resin composition, in order to cure, it is necessary to treat at a high temperature, and there is room for improvement in operability. In addition, in the sealing structure using the prior art resin composition, there is room for improvement in the adhesion and waterproofness with the structure such as electronic components or stators, and sometimes the sealing structure has a defective condition.
[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a molding resin composition that can be cured at a low temperature and can improve the adhesion and waterproofness when sealing a structure such as an electronic component or a stator.
[0010] Means for solving technical problems
[0011] The inventors of the present invention have studied and, as a result, have completed the invention provided below and solved the above-mentioned problems.
[0012] According to the present invention, there are provided the following molding resin composition, method for producing a sealing structure, and sealing structure.
[0013] [1] A molding resin composition that can be used to seal a substrate on which an electronic component is mounted, a stator core having a plurality of slots formed along a circumferential direction and fixed to the substrate, and a plurality of coils housed in the slots, the molding resin composition comprising an epoxy resin, one or both of a curing agent and a curing catalyst, and an inorganic filler.
[0014] The flexural modulus of a cured product obtained by curing the molding resin composition at 140° C. for 2 minutes at 25° C. (in accordance with JIS K6911:2006) is 0.1 GPa or more and 30 GPa or less.
[0015] [2] The molding resin composition according to the above [1], wherein the glass transition temperature (Tg) measured by the following (Method 1) is 140°C to 300°C.
[0016] (Method 1)
[0017] Using a transfer molding machine, the molding resin composition was molded into a test piece of 80 mm × 10 mm × 4 mm under the conditions of a mold temperature of 175 ° C, an injection pressure of 6.9 MPa, and a curing time of 90 seconds, and cured at 175 ° C for 2 hours. The thermal expansion coefficient of the obtained test piece was measured using a thermomechanical analyzer at a heating rate of 5 ° C / min. Then, based on the obtained measurement results, the glass transition temperature (Tg) (° C) of the cured product was calculated according to the inflection point of the thermal expansion coefficient.
[0018] [3] The molding resin composition as described in [1] or [2] above, wherein the epoxy resin contains one or more selected from the group consisting of phenol novolac type epoxy resin, cresol novolac type epoxy resin and trisphenol methane type epoxy resin.
[0019] [4] The molding resin composition as described in any one of [1] to [3] above, wherein the content of the epoxy resin is 3% by mass or more and 40% by mass or less when the solid content of the molding resin composition as a whole is set to 100% by mass.
[0020] [5] The molding resin composition according to any one of [1] to [4] above, wherein the molding resin composition contains the curing agent, and the curing agent contains a phenolic resin-based curing agent.
[0021] [6] The molding resin composition as described in [5] above, wherein the phenolic resin-based curing agent contains one or more selected from phenol novolac resin, cresol novolac resin, naphthol novolac resin and trisphenol methane type phenolic resin.
[0022] [7] The molding resin composition according to [5] or [6], wherein the content of the curing agent is 0.8% by mass or more and 12% by mass or less, when the solid content of the molding resin composition as a whole is 100% by mass.
[0023] [8] The molding resin composition according to any one of [1] to [7] above, wherein the molding resin composition contains the curing catalyst, and the curing catalyst contains an imidazole compound.
[0024] [9] The molding resin composition according to [8] above, wherein the content of the curing catalyst is 0.01% by mass or more and 2.0% by mass or less, based on 100% by mass of the solid content of the molding resin composition as a whole.
[0025]
[10] A molding resin composition as described in any one of [1] to [9] above, wherein the swirl length of the molding resin composition measured under the conditions of a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a curing time of 3 minutes is set as S1, and the swirl length of the molding resin composition measured under the conditions of a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a curing time of 3 minutes after the molding resin composition is left to stand at 25°C for 48 hours is set as S2, and S2 ≥ 0.8 × S1 is satisfied.
[0026]
[11] The molding resin composition according to any one of [1] to
[10] , wherein
[0027] The time for the torque value measured by the following (method 2) to reach 2 N·m is less than 100 seconds.
[0028] (Method 2)
[0029] The torque value of the molding resin composition was measured over time using CURELASTOMETER (registered trademark, vulcanizer) at a mold temperature of 140°C and an amplitude angle of ±0.25 degrees. The time (seconds) from the start of measurement until the torque value reached 2 N·m was calculated based on the measurement results.
[0030]
[12] The molding resin composition as described in any one of [1] to
[11] above, wherein the swirl length measured by the following (Method 3) is 70 cm or more.
[0031] (Method 3)
[0032] The molding resin composition was injected into a mold for measuring swirl length according to ANSI / ASTM D3123-72 using a low-pressure transfer molding machine at 175° C., an injection pressure of 6.9 MPa, and a holding time of 3 minutes to measure the flow length, which was taken as the swirl length (cm).
[0033]
[13] The molding resin composition according to any one of [1] to
[12] above, wherein
[0034] The gel time measured by the following (Method 4) is 30 seconds or more.
[0035] (Method 4)
[0036] The molding resin composition was injected into a mold for measuring the swirl length according to ANSI / ASTM D3123-72 using a low-pressure transfer molding machine at 175°C, an injection pressure of 6.9 MPa, and a holding time of 3 minutes. The time from the start of injection to the time when the molding resin composition solidified and no longer flowed was measured as the gel time (seconds).
[0037]
[14] The molding resin composition according to any one of [1] to
[13] above, wherein
[0038] The linear expansion coefficient α1 measured by the following (method 5) is 10.0 ppm / °C or less.
[0039] (Method 5)
[0040] The above-mentioned molding resin composition was injection molded using a low-pressure transfer molding machine under the conditions of a mold temperature of 175°C, an injection pressure of 9.8MPa, and a curing time of 3 minutes to obtain a 15mm×4mm×4mm molded product. Next, the obtained molded product was post-cured at 175°C for 4 hours to prepare a test piece. Then, for the obtained test piece, a thermomechanical analysis device was used to measure the average linear expansion coefficient α1 (ppm / °C) at 25 to 70°C under the conditions of a measurement temperature range of 0°C to 400°C and a heating rate of 5°C / min.
[0041]
[15] The molding resin composition according to any one of [1] to
[14] above, wherein
[0042] The thermal conductivity measured by the following (method 6) is 0.5 W / m·K or more.
[0043] (Method 6)
[0044] Using a transfer molding machine, the above-mentioned molding resin composition was injection molded under the conditions of a mold temperature of 175°C, an injection pressure of 6.9MPa, and a curing time of 90 seconds to obtain a molded body of 80mm×10mm×4mm. Next, the obtained molded body was post-cured at 175°C for 2 hours to obtain a test piece, and the thermal diffusion coefficient of the obtained test piece was measured using a laser flash method. In addition, an electronic densimeter was used to measure the specific gravity of the test piece used for the thermal conductivity coefficient measurement. In addition, a differential scanning calorimeter was used to measure the specific heat of the test piece used for the thermal conductivity coefficient and specific gravity measurement. Based on the measured values of the thermal diffusion coefficient, specific gravity, and specific heat, the thermal conductivity (W / m·K) in the thickness direction of the test piece was calculated.
[0045]
[16] A method for manufacturing a sealing structure, comprising:
[0046] The step of placing a substrate on which electronic components are mounted, a stator core having a plurality of slots formed along a circumferential direction and fixed to the substrate, and a plurality of coils received in the slots in a molding die in a transfer molding machine; and
[0047] A process for seal-molding the substrate, the stator core, and the coil in the mold using the molding resin composition described in any one of [1] to
[15] by transfer molding using the transfer molding machine to obtain a sealed structure.
[0048]
[17] The method for manufacturing a sealing structure according to
[16] above, wherein:
[0049] In the step of obtaining the sealed structure, the sealing molding is performed at a temperature not higher than the Tg of the cured product of the molding resin composition.
[0050]
[18] The method for producing a sealing structure according to
[16] or
[17] above, wherein:
[0051] As the above-mentioned process for obtaining the above-mentioned sealing structure, no post-curing process is performed.
[0052]
[19] A sealing structure comprising a sealed body and a sealing member provided so as to cover a part or the whole of the sealed body,
[0053] The sealed body includes a substrate on which electronic components are mounted, a stator core fixed to one surface of the substrate and having a plurality of slots formed along a circumferential direction, and a plurality of coils housed in the slots.
[0054] The sealing member is formed of a cured product of the molding resin composition according to any one of [1] to
[15] .
[0055] Effects of the Invention
[0056] According to the present invention, there is provided a molding resin composition which can be cured at a low temperature and can improve the adhesion and waterproofness when sealing a structure such as an electronic component or a stator. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1 It is a plan view of the sealed object and the sealing structure before and after molding in one example of the present embodiment.
[0058] Figure 2 It is a side view of the sealed object and the sealing structure before and after molding in one example of the present embodiment. DETAILED DESCRIPTION
[0059] Hereinafter, the embodiments of the present invention will be described using the drawings. In all the drawings, the same components are denoted by the same reference numerals, and the description thereof will be appropriately omitted.
[0060] In this specification, unless otherwise specified, the expression "X to Y" about a numerical range means greater than or equal to X and less than or equal to Y. In this specification, unless otherwise specified, the upper limit and lower limit of a numerical range can be arbitrarily combined.
[0061] <Molding resin composition>
[0062] The molding resin composition of this embodiment is used to seal a substrate carrying electronic components, a stator core having a plurality of slots formed along the circumferential direction and fixed on the above-mentioned substrate, and a plurality of coils accommodated in the above-mentioned slots. The above-mentioned molding resin composition contains an epoxy resin, a curing catalyst and an inorganic filler. The bending elastic modulus of a cured product obtained by curing the molding resin composition at 140°C for 2 minutes at 25°C (in accordance with JIS K6911:2006) is not less than 0.1GPa and not more than 30GPa.
[0063] The molding resin composition of this embodiment is used to seal a substrate on which electronic components are mounted, a stator core having a plurality of slots formed along the circumferential direction and fixed to the substrate, and a plurality of coils housed in the slots. The method of using the molding resin composition of this embodiment as a sealing material is described in detail below.
[0064] Regarding the molding resin composition of the present embodiment, in the cured product obtained by curing the molding resin composition at 140° C. for 2 minutes, the flexural modulus (according to JIS K6911:2006) at 25° C. is 0.1 GPa or more and 30 GPa or less. The molding resin composition of the present embodiment has a flexural modulus within the above numerical range, and thus can be cured at a low temperature, and can improve the adhesion and waterproofness when sealing a structure such as an electronic component or a stator.
[0065] Although the mechanism by which such an effect is achieved is still uncertain, it is believed that by having the bending elastic modulus within the above-mentioned numerical range, it is possible to suppress the occurrence of fine cracks in the cured product of the molding resin composition of this embodiment when it is subjected to certain loads, and as a result, the adhesion and waterproofness when sealing structures such as electronic components or stators can be improved.
[0066] Regarding the molding resin composition of the present embodiment, in the cured product obtained by curing the molding resin composition at 140° C. for 2 minutes, the lower limit of the bending modulus (according to JIS K6911:2006) at 25° C. is 0.1 GPa or more, preferably 1.0 GPa or more, more preferably 3.0 GPa or more, further preferably 5.0 GPa or more, further preferably 8.0 GPa or more, further preferably 10.0 GPa or more, further preferably 12.0 GPa or more, and further preferably 13.0 GPa or more. By setting the bending modulus to be above the above lower limit, a structure having excellent mechanical strength can be obtained even when curing at low temperature.
[0067] And, the upper limit value of the bending elastic modulus is below 30GPa, preferably below 27.0GPa, more preferably below 24.0GPa, and further preferably below 21.0GPa. By setting the bending elastic modulus to below the above-mentioned upper limit value, the stress accumulated in the cured product becomes sufficiently small, reducing warping. Thus, the adhesion and waterproofness during the structures such as the sealed electronic components or stators can be improved, and the structure is not prone to undesirable conditions.
[0068] Here, the flexural modulus of the molding resin composition of the present embodiment at 25° C. can be measured, for example, by the following method.
[0069] The resin composition was injection molded using a low pressure transfer molding machine at a mold temperature of 140°C, an injection pressure of 9.8 MPa, and a curing time of 2 minutes to obtain a molded product having a length of 80 mm, a width of 10 mm, and a thickness of 4 mm. The obtained molded product was subjected to a heat treatment at 200°C for 4 hours as post-curing to obtain a test piece, and the bending modulus was measured at an ambient temperature of 25°C in accordance with JIS K6911:2006. As a low pressure transfer molding machine, for example, KTS-15 or KTS-30 (manufactured by KOHTAKI Corporation) can be used.
[0070] Hereinafter, each component used for the molding resin composition of this embodiment is demonstrated.
[0071] [Epoxy resin]
[0072] Examples of the epoxy resin used in the molding resin composition of the present embodiment include novolac epoxy resins such as phenol novolac epoxy resins and cresol novolac epoxy resins, bisphenol A epoxy resins and bisphenol F epoxy resins, aromatic glycidylamine epoxy resins such as N,N-diglycidyl aniline, N,N-diglycidyl toluidine, diaminodiphenylmethane glycidylamine, and aminophenol glycidylamine, hydroquinone epoxy resins, biphenyl epoxy resins, and stilbene epoxy resins. Aromatic epoxy resins such as aralkyl epoxy resins such as phenol aralkyl epoxy resins having a phenylene skeleton and / or a biphenylene skeleton, naphthol aralkyl epoxy resins having a phenylene skeleton and / or a biphenylene skeleton, and aliphatic epoxy resins such as alicyclic epoxy resins such as vinylcyclohexene dioxide, dicyclopentadiene oxide, and alicyclic diepoxy-adipate. These may be used alone or in combination of two or more.
[0073] Among these, the epoxy resin used in the molding resin composition of the present embodiment preferably contains one or more selected from phenol novolac type epoxy resins, cresol novolac type epoxy resins, and trisphenol methane type epoxy resins.
[0074] From the viewpoint of further improving the adhesion and waterproofness when sealing structures such as electronic components or stators, when the solid content of the molding resin composition as a whole is set to 100% by mass, the lower limit of the content of the epoxy resin in the molding resin composition of the present embodiment is preferably 3% by mass or more, more preferably 4% by mass or more, further preferably 5% by mass or more, further preferably 6% by mass or more, and further preferably 7% by mass or more.
[0075] Furthermore, from the viewpoint of being able to obtain a structure having excellent mechanical strength even when cured at low temperatures, when the solid content of the molding resin composition as a whole is set to 100% by mass, the upper limit of the content of the epoxy resin is preferably 40% by mass or less, more preferably 30% by mass or less, further preferably 20% by mass or less, and further preferably 15% by mass or less.
[0076] From the viewpoint of further improving the adhesion and waterproofness when sealing structures such as electronic components or stators, and from the viewpoint of being able to obtain a structure with excellent mechanical strength even when cured at low temperatures, when the solid content of the molding resin composition as a whole is set to 100 mass%, the content of the epoxy resin in the molding resin composition of the present embodiment is preferably 3 mass% to 40 mass%, more preferably 4 mass% to 30 mass%, further preferably 5 mass% to 20 mass%, further preferably 6 mass% to 20 mass%, and further preferably 7 mass% to 15 mass%.
[0077] (Curing agent)
[0078] The molding resin composition of the present embodiment contains one or both of a curing agent and a curing catalyst. In order to make the epoxy resin three-dimensionally crosslinked, the molding resin composition of the present embodiment preferably contains a curing agent. In the case of containing a curing agent as an essential component, it is more preferably containing a phenolic resin curing agent. As a phenolic resin curing agent, for example, phenolic varnish type phenolic resins such as phenol novolac resin, cresol novolac resin, and naphthol novolac resin; polyfunctional phenolic resins such as trisphenol methane type phenolic resins; terpene modified phenolic resins, dicyclopentadiene modified phenolic resins and other modified phenolic resins; aralkyl type phenolic resins such as phenol aralkyl resins with phenylene skeletons and / or biphenylene skeletons, naphthol aralkyl resins with phenylene and / or biphenylene skeletons; bisphenol compounds such as bisphenol A and bisphenol F, etc., these can be used alone or in combination of two or more.
[0079] The preferred phenolic resin curing agent of the molding resin composition of the present embodiment contains one or more than two kinds selected from phenol novolac resin, cresol novolac resin, naphthol novolac resin and trisphenol methane type phenolic resin. By such a phenolic resin curing agent, the balance of flame retardancy, moisture resistance, electrical properties, curability, storage stability, etc. becomes better. Especially from the viewpoint of curability, for example, the hydroxyl equivalent of the phenolic resin curing agent can be set to more than 90g / eq and less than 250g / eq.
[0080] Furthermore, examples of the curing agent that can be used together include a polyaddition type curing agent, a catalyst type curing agent, a condensation type curing agent, and the like.
[0081] Examples of the polyaddition curing agent include aliphatic polyamines such as diethylenetriamine (DETA), triethylenetetramine (TETA), and meta-xylene diamine (MXDA); aromatic polyamines such as diaminodiphenylmethane (DDM), meta-phenylenediamine (MPDA), and diaminodiphenyl sulfone (DDS); polyamine compounds including dicyandiamide (DICY) and organic acid dihydrazides; acid anhydrides including alicyclic acid anhydrides such as hexahydrophthalic anhydride (HHPA) and methyltetrahydrophthalic anhydride (MTHPA); aromatic acid anhydrides such as trimellitic anhydride (TMA), pyromellitic anhydride (PMDA), and benzophenonetetracarboxylic acid (BTDA); polyphenol compounds such as novolac-type phenolic resins and phenol polymers; polythiol compounds such as polysulfides, thioesters, and thioethers; isocyanate compounds such as isocyanate prepolymers and blocked isocyanates; organic acids such as carboxylic acid-containing polyester resins, and the like.
[0082] Examples of catalyst-type curing agents include tertiary amine compounds such as benzyldimethylamine (BDMA) and 2,4,6-tris-dimethylaminomethylphenol (DMP-30); imidazole compounds such as 2-methylimidazole and 2-ethyl-4-methylimidazole (EMI24); and Lewis acids such as BF3 complexes.
[0083] Examples of the condensation type curing agent include urea resins such as resol phenolic resins and methylol-containing urea resins; and melamine resins such as methylol-containing melamine resins.
[0084] In the case of using such other curing agents, relative to all curing agents, the lower limit of the content of the phenolic resin curing agent is preferably more than 20 mass %, more preferably more than 30 mass %, more preferably more than 50 mass %, more preferably more than 70 mass %, more preferably more than 90 mass %. If the content of the phenolic resin curing agent is more than the above-mentioned lower limit, then the curability at low temperature can be maintained, and good fluidity is exhibited. In addition, the upper limit of the content of the phenolic resin curing agent is not particularly limited, and relative to all curing agents, it is preferably less than 100 mass %.
[0085] The lower limit of the total value of the content of the curing agent in the molding resin composition of the present embodiment is not particularly limited, when the solid component of the molding resin composition is set to 100 mass %, preferably more than 0.8 mass %, more preferably more than 1 mass %, more preferably more than 1.5 mass %, more preferably more than 2 mass %, more preferably more than 3 mass %, more preferably more than 4 mass %. If the total value of the content of the curing agent is more than the above-mentioned lower limit, good curability can be obtained. And, the upper limit of the total value of the content of the curing agent relative to the molding resin composition is not particularly limited, relative to the molding resin composition as a whole, preferably less than 12 mass %, more preferably less than 10 mass %, more preferably less than 8 mass %.
[0086] In addition, the phenolic resin and epoxy resin as curing agents are preferably combined in a manner that the equivalent ratio (EP) / (OH) of the number of epoxy groups (EP) in the molding resin composition to the number of phenolic hydroxyl groups (OH) of all phenolic resins is 0.8 or more and 1.6 or less. If the equivalent ratio is within the above range, sufficient curing characteristics can be obtained when the obtained molding resin composition is molded. Among them, when a resin other than the phenolic resin that can react with the epoxy resin is used in combination, it is sufficient to adjust the equivalent ratio appropriately.
[0087] [Curing catalyst]
[0088] In the case where the molding resin composition of the present embodiment contains a curing catalyst as an essential component, an imidazole compound is preferably used as the curing catalyst used for the molding resin composition of the present embodiment. The imidazole compound may contain, for example, imidazole compounds selected from: imidazole, 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-phenylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole and 2-phenyl-4-methyl-5-hydroxymethylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-benzyl-2-phenylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole and 2-phenyl-4-methyl-5-hydroxymethylimidazole. One or more of ethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl (1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl (1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4-methylimidazolyl (1')]-ethyl-s-triazine, isohydrouric acid adduct of 2,4-diamino-6-[2'-methylimidazolyl (1')]-ethyl-s-triazine, isohydrouric acid adduct of 2-phenylimidazole, and isohydrouric acid adduct of 2-methylimidazole.
[0089] When using imidazole compounds as curing catalysts, when the solid content of the molding resin composition is set to 100% by mass as a whole, the content of the imidazole compounds is preferably more than 0.01% by mass, more preferably more than 0.03% by mass, more preferably more than 0.05% by mass, more preferably more than 0.1% by mass, more preferably more than 0.3% by mass, more preferably more than 0.5% by mass, more preferably more than 1.0% by mass. By setting the content of the imidazole compounds to more than the above-mentioned lower limit, the adhesion and waterproofness during the sealing of electronic components or stators can be improved. And, the curing property at low temperatures during sealing molding can also be improved. On the other hand, when the solid content of the molding resin composition is set to 100% by mass as a whole, the content of the imidazole compounds is preferably less than 2.0% by mass, more preferably less than 1.5% by mass. By setting the content of the imidazole compounds to less than the above-mentioned upper limit, the fluidity during transfer molding can be improved, which contributes to the improvement of filling properties.
[0090] In addition to the imidazole compound, the curing catalyst may also contain a phosphorus atom-containing compound selected from, for example, organic phosphines, tetrasubstituted phosphonium compounds, phosphobetaine compounds, adducts of phosphine compounds and quinone compounds, adducts of phosphonium compounds and silane compounds; and one or more of amine curing catalysts other than imidazole compounds such as 1,8-diazabicyclo(5,4,0)undecene.
[0091] Examples of the organic phosphine include primary phosphines such as ethylphosphine and phenylphosphine; secondary phosphines such as dimethylphosphine and diphenylphosphine; and tertiary phosphines such as trimethylphosphine, triethylphosphine, tributylphosphine and triphenylphosphine.
[0092] Examples of the tetrasubstituted phosphonium compound include compounds represented by the following general formula (4).
[0093]
[0094] In the above general formula (4), P represents a phosphorus atom. 4 , R 5 , R 6 and R 7 represents an aromatic group or an alkyl group. A represents an anion of an aromatic organic acid having at least one functional group selected from hydroxyl, carboxyl, and mercapto on the aromatic ring. AH represents an aromatic organic acid having at least one functional group selected from hydroxyl, carboxyl, and mercapto on the aromatic ring. x and y are numbers from 1 to 3, z is a number from 0 to 3, and x=y.
[0095] The compound represented by the general formula (4) can be obtained, for example, as follows, but is not limited thereto. First, a tetrasubstituted phosphonium halide, an aromatic organic acid, and a base are uniformly mixed in an organic solvent, and an aromatic organic acid anion is generated in the solution system. Then, if water is added, the compound represented by the general formula (4) can be precipitated. In the compound represented by the general formula (4), it is preferred that R bonded to the phosphorus atom 4 , R 5 , R 6 and R 7 A is a phenyl group, and AH is a compound having a hydroxyl group on an aromatic ring, i.e., a phenol, and A is an anion of the phenol. Examples of the phenol include monocyclic phenols such as phenol, cresol, resorcinol, and catechol, condensed and polycyclic phenols such as naphthol, dihydroxynaphthalene, and anthracene, bisphenols such as bisphenol A, bisphenol F, and bisphenol S, and polycyclic phenols such as phenylphenol and biphenol.
[0096] Examples of the phosphobetaine compound used as a curing catalyst include compounds represented by the following general formula (5).
[0097]
[0098] In the above general formula (5), P represents a phosphorus atom. 8 represents an alkyl group having 1 to 3 carbon atoms, R 9 represents a hydroxyl group. f is a number from 0 to 5, and g is a number from 0 to 3.
[0099] The compound represented by the general formula (5) can be obtained, for example, by first contacting a triaromatic substituted phosphine as a tertiary phosphine with a diazonium salt, and then replacing the triaromatic substituted phosphine with a diazo group of the diazonium salt. However, the present invention is not limited thereto.
[0100] Examples of the adduct of a phosphine compound and a quinone compound used as a curing catalyst include compounds represented by the following general formula (6).
[0101]
[0102] In the above general formula (6), P represents a phosphorus atom. 10 , R 11 and R 12 represents an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 12 carbon atoms, and they may be the same or different. 13 , R 14 and R 15 represents a hydrogen atom or a hydrocarbon group having 1 to 12 carbon atoms, and they may be the same or different, and R 14 With R 15 Can be bonded to form a ring structure.
[0103] As the phosphine compound used for the adduct of the phosphine compound and the quinone compound, for example, triphenylphosphine, tri(alkylphenyl)phosphine, tri(alkoxyphenyl)phosphine, trinaphthylphosphine, tribenzylphosphine, etc., which have no substitution or have a substituent such as an alkyl group or an alkoxy group on the aromatic ring, are preferred, and the substituent such as the alkyl group or the alkoxy group includes a group having 1 to 6 carbon atoms. From the viewpoint of easy availability, triphenylphosphine is preferred.
[0104] Examples of the quinone compound used for the adduct of the phosphine compound and the quinone compound include benzoquinone and anthraquinones. Among them, p-benzoquinone is preferred from the viewpoint of storage stability.
[0105] As a method for producing an adduct of a phosphine compound and a quinone compound, an adduct can be obtained by contacting and mixing an organic tertiary phosphine and a benzoquinone in a solvent in which both can be dissolved. As the solvent, a solvent with low solubility for the adduct among ketones such as acetone or methyl ethyl ketone is preferred. However, it is not limited to this.
[0106] Among the compounds represented by the general formula (6), from the viewpoint of reducing the thermal elastic modulus of the cured product of the molding resin composition, R bonded to the phosphorus atom is preferably 10 , R11 and R 12 is phenyl, and R 13 , R 14 and R 15 A compound in which a hydrogen atom is added to 1,4-benzoquinone and triphenylphosphine.
[0107] Examples of the adduct of a phosphonium compound and a silane compound used as a curing catalyst include compounds represented by the following general formula (7).
[0108]
[0109] In the above general formula (7), P represents a phosphorus atom and Si represents a silicon atom. 16 , R 17 , R 18 and R 19 They represent organic groups or aliphatic groups having aromatic rings or heterocyclic rings, and they may be the same or different. 20 For the group Y 2 and Y 3 Bonded organic group. 21 For the group Y 4 and Y 5 Bonded organic group. 2 and Y 3 The proton-donating group releases a proton, and the group Y in the same molecule 2 and Y 3 Bonds to silicon atoms to form a chelate structure. 4 and Y 5 The proton-donating group releases a proton, and the group Y in the same molecule 4 and Y 5 Bonds to silicon atoms to form a chelate structure. 20 and R 21 They can be the same or different. 2 , Y 3 , Y 4 and Y 5 They can be the same or different. 1 It is an organic group having an aromatic ring or a heterocyclic ring or an aliphatic group.
[0110] In the general formula (7), as R 16 , R 17 , R 18 and R 19For example, phenyl, methylphenyl, methoxyphenyl, hydroxyphenyl, naphthyl, hydroxynaphthyl, benzyl, methyl, ethyl, n-butyl, n-octyl and cyclohexyl can be mentioned. Among these, aromatic groups having substituents such as alkyl, alkoxy, hydroxyl, etc., such as phenyl, methylphenyl, methoxyphenyl, hydroxyphenyl, hydroxynaphthyl, or unsubstituted aromatic groups are more preferred.
[0111] In addition, in the general formula (7), R 20 For Y 2 and Y 3 Similarly, R 21 For the group Y 4 and Y 5 Bonded organic group. 2 and Y 3 The proton-donating group releases a proton, and the group Y in the same molecule 2 and Y 3 Bonded with silicon atoms to form a chelate structure. 4 and Y 5 The proton-donating group releases a proton, and the group Y in the same molecule 4 and Y 5 Bonds to silicon atoms to form a chelate structure. 20 and R 21 They may be the same or different from each other, and the group Y 2 , Y 3 , Y 4 and Y 5 They may be the same or different. 2 -R 20 -Y 3 -and-Y 4 -R 21 -Y 5 -is composed of a group formed by releasing two protons from a proton donor. As the proton donor, an organic acid having at least two carboxyl groups or hydroxyl groups in the molecule is preferred. An aromatic compound having at least two carboxyl groups or hydroxyl groups on adjacent carbon atoms constituting an aromatic ring is further preferred. An aromatic compound having at least two hydroxyl groups on adjacent carbon atoms constituting an aromatic ring is more preferred. Examples thereof include catechol, pyrogallol, 1,2-dihydroxynaphthalene, 2,3-dihydroxynaphthalene, 2,2'-biphenol, 1,1'-bi-2-naphthol, salicylic acid, 1-hydroxy-2-naphthoic acid, 3-hydroxy-2-naphthoic acid, chloranilic acid, tannic acid, 2-hydroxybenzyl alcohol, 1,2-cyclohexanediol, 1,2-propylene glycol and glycerol. Among these, catechol, 1,2-dihydroxynaphthalene and 2,3-dihydroxynaphthalene are more preferred.
[0112] In addition, Z in the general formula (7)1 It represents an organic group having an aromatic ring or a heterocyclic ring, or an aliphatic group. Specific examples thereof include aliphatic hydrocarbon groups such as methyl, ethyl, propyl, butyl, hexyl and octyl, or aromatic hydrocarbon groups such as phenyl, benzyl, naphthyl and biphenyl, and reactive substituents such as glycidoxy, mercapto, and amino groups such as alkyl and vinyl groups, such as glycidoxypropyl, mercaptopropyl, and aminopropyl. Among these, methyl, ethyl, phenyl, naphthyl and biphenyl are more preferred from the viewpoint of thermal stability.
[0113] As a method for producing an adduct of a phosphonium compound and a silane compound, a silane compound such as phenyltrimethoxysilane and a proton donor such as 2,3-dihydroxynaphthalene are added to a flask containing methanol and dissolved, and then a sodium methoxide-methanol solution is added dropwise under stirring at room temperature. Furthermore, if a solution of a tetrasubstituted phosphonium halide such as tetraphenylphosphonium bromide dissolved in methanol is added dropwise under stirring at room temperature, crystals are precipitated. If the precipitated crystals are filtered, washed with water, and vacuum dried, an adduct of a phosphonium compound and a silane compound can be obtained. However, it is not limited thereto.
[0114] When the solid component of the molding resin composition is set to 100% by mass as a whole, the content of the curing catalyst in the molding resin composition of the present embodiment is preferably more than 0.1% by mass, more preferably more than 0.3% by mass, more preferably more than 0.5% by mass, more preferably more than 1.0% by mass. By setting the content of the curing catalyst to more than the above-mentioned lower limit, the curability of the molding resin composition during transfer molding can be effectively improved, and the curability at low temperatures can be improved. On the other hand, when the solid component of the molding resin composition is set to 100% by mass as a whole, the content of the curing catalyst is preferably less than 2.0% by mass, more preferably less than 1.7% by mass, more preferably less than 1.5% by mass. By setting the content of the curing catalyst to less than the above-mentioned upper limit, the fluidity during sealing can be improved, which contributes to the improvement of filling properties.
[0115] [Inorganic filler]
[0116] As the inorganic filling material used for the molding resin composition of the present embodiment, for example, fused silica such as fused crushed silica and fused spherical silica, crystalline silica, alumina, kaolin, talc, clay, mica, asbestos, wollastonite, glass powder, glass flakes, glass beads, glass fiber, silicon carbide, silicon nitride, aluminum nitride, carbon black, graphite, titanium dioxide, calcium carbonate, calcium sulfate, barium carbonate, magnesium carbonate, magnesium sulfate, barium sulfate, cellulose, aramid, wood, pulverized powder obtained by crushing the cured product of phenolic resin molding material or epoxy resin molding material, etc. are enumerated. Among them, preferably fused crushed silica, fused spherical silica, crystalline silica and other silica, more preferably fused spherical silica. And, wherein, from the cost aspect, preferably calcium carbonate, wollastonite. The inorganic filling material can use one, or two or more can be used in combination.
[0117] Average particle size D of inorganic filler 50 The average particle size D of the inorganic filler is preferably 0.01 μm or more and 75 μm or less, and more preferably 0.05 μm or more and 50 μm or less. 50 When the average particle size D of the inorganic filler is within the above range, the filling property in the mold during molding is improved. 50 The upper limit of the average particle size D is set to 75 μm or less, and the filling property is further improved. 50 It is a volume-converted average particle size measured using a laser diffraction measuring device RODOS SR model (SYMPATEC HEROS & RODOS).
[0118] Furthermore, the molding resin composition of this embodiment may contain two or more particles having different average particle sizes D 50 Spherical silica is used as an inorganic filler. This improves fluidity and filling properties during transfer molding.
[0119] When the solid component of the molding resin composition is set to 100% by mass as a whole, the content of the inorganic filler in the molding resin composition of the present embodiment is preferably more than 50% by mass, more preferably more than 60% by mass, more preferably more than 65% by mass, more preferably more than 70% by mass, more preferably more than 75% by mass. If the content of the inorganic filler is more than the above-mentioned lower limit, the increase of the moisture absorption caused by the solidification of the obtained molding resin composition and the reduction of intensity can be reduced. And, when the solid component of the molding resin composition is set to 100% by mass as a whole, the content of the inorganic filler is preferably less than 93% by mass, more preferably less than 91% by mass, more preferably less than 90% by mass. If the content of the inorganic filler is less than the above-mentioned upper limit, the obtained molding resin composition has good fluidity, and has good formability. Therefore, the manufacturing stability of the sealing structure is improved, and the structure with excellent balance of yield rate and durability can be obtained.
[0120] And, when using silica such as fused crushed silica, fused spherical silica, crystalline silica as inorganic filler, when the inorganic filler of the molding resin composition is set to 100% by mass as a whole, the content of silica is preferably 40% by mass or more, more preferably 60% by mass or more, and further preferably 75% by mass or more. If the content of silica is above the above lower limit, the balance of curability and fluidity of the molding resin composition during transfer molding becomes better.
[0121] In this case, the upper limit of the content of silica is not particularly limited, but is, for example, 100 mass % or less when the entire inorganic filler in the molding resin composition is taken as 100 mass %.
[0122] When an inorganic filler is used in combination with a metal hydroxide such as aluminum hydroxide or magnesium hydroxide or an inorganic flame retardant such as zinc borate, zinc molybdate, or antimony trioxide, the total amount of the inorganic flame retardant and the inorganic filler is preferably within the range of the content of the inorganic filler.
[0123] [Other ingredients]
[0124] The molding resin composition of the present embodiment may contain other components such as an adhesion promoter, wax, a coupling agent, a colorant, a flame retardant, a release agent, and a stress reducing agent, in addition to the above-mentioned components, as necessary.
[0125] (Sealing agent)
[0126] In order to improve the curability at low temperature, the molding resin composition of the present embodiment preferably contains a close-fitting auxiliary agent. The close-fitting auxiliary agent used in the molding resin composition of the present embodiment is not particularly limited, and examples thereof include triazole compounds, and examples of the triazole compound include compounds having 1,2,4-triazole rings and compounds having 1,2,3-triazole rings. As specific compounds, for example, 3-amino-1,2,4-triazole, 4-amino-1,2,3-triazole, 3-amino-1,2,4-triazole-5-carboxylic acid, 3-mercapto-1,2,4-triazole, 4-mercapto-1,2,3-triazole, 3,5-diamino-1,2,4-triazole, 3,5-dimercapto-1,2,4-triazole, 4,5-dimercapto-1,2,3-triazole, 3-amino-5-mercapto-1,2,4-triazole, 4-amino-5-mercapto-1,2,3-triazole, 3-hydrazino-4-amino-5-mercapto-1,2,4-triazole, and 5-mercapto-1,2,4-triazole-3-methanol can be mentioned, and one of these can be used or two or more can be used in combination. Among these, compounds having at least one mercapto group are preferred.
[0127] The lower limit of the content of the adhesion aid in the molding resin composition of the present embodiment is, for example, preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and further preferably 0.07% by mass or more, when the solid content of the molding resin composition as a whole is set to 100% by mass. Thus, the curability at low temperatures can be further improved.
[0128] And, as the upper limit of the content of the adhesion aid, for example, when the solid content of the molding resin composition is set to 100 mass %, it is preferably 10 mass % or less, more preferably 5 mass % or less, further preferably 1 mass % or less, further preferably 0.5 mass % or less, further preferably 0.3 mass % or less. Thus, the adhesion and waterproofness when sealing structures such as electronic components or stators with the molding resin composition of the present embodiment can be improved.
[0129] (wax)
[0130] The molding resin composition of the present embodiment preferably contains a wax having a melting point of 30° C. to 90° C. By containing such a wax, the molding resin composition has good melting properties at the temperature used in transfer molding, thereby improving fluidity during sealing and improving filling properties. Examples of such waxes include natural waxes such as carnauba wax, synthetic waxes such as montanic acid ester wax and oxidized polyethylene wax, and higher fatty acids such as zinc stearate and metal salts thereof.
[0131] When the solid component of the molding resin composition is set to 100 mass %, the amount of wax is, for example, 0.05 mass % or more and 2.0 mass % or less. When the solid component of the molding resin composition is set to 100 mass %, the lower limit of the amount of wax is preferably 0.1 mass % or more, more preferably 0.2 mass % or more. When the solid component of the molding resin composition is set to 100 mass %, the upper limit of the amount of wax is preferably 1.5 mass % or less, more preferably 1.0 mass % or less. By coordinating wax with the above range, the obtained molding resin composition has excellent fluidity and filling property when transfer molding.
[0132] (Coupling agent)
[0133] In order to improve the adhesion between the epoxy resin and the inorganic filler, the molding resin composition of the present embodiment may contain a coupling agent such as a silane coupling agent. Examples of the coupling agent include epoxy silane, amino silane, ureido silane, and mercapto silane.
[0134] Examples of the epoxysilane include γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. Examples of aminosilanes include γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-phenyl-γ-aminopropyltriethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltriethoxysilane, N-6-(aminohexyl)-3-aminopropyltrimethoxysilane, and N-(3-(trimethoxysilylpropyl)-1,3-benzenedimethanane. Examples of ureidosilanes include Gamma-ureidopropyl triethoxysilane, hexamethyldisilazane, etc. can be cited. Ketones or aldehydes can also be reacted to protect the primary amino site of aminosilane and used in the form of a potential aminosilane coupling agent. In addition, as aminosilane, secondary amino groups can also be present. In addition, as mercaptosilane, for example, gamma-mercaptopropyl trimethoxysilane and 3-mercaptopropyl methyl dimethoxysilane can be cited. In addition, silane coupling agents that exhibit the same function as mercaptosilane coupling agents by thermal decomposition of bis (3-triethoxysilyl propyl) tetrasulfide and bis (3-triethoxysilyl propyl) disulfide can also be cited. In addition, these silane coupling agents can be pre-coordinated with substances obtained by hydrolysis reaction. These silane coupling agents can be used alone or in combination of two or more.
[0135] From the viewpoint of connection moldability, mercaptosilane is preferred; from the viewpoint of fluidity, aminosilane is preferred; and from the viewpoint of adhesion, epoxysilane is preferred.
[0136] As the lower limit of the content of the coupling agent such as the silane coupling agent in the molding resin composition of the present embodiment, when the solid component of the molding resin composition is set to 100 mass %, it is preferably more than 0.01 mass %, more preferably more than 0.05 mass %, more preferably more than 0.1 mass %, more preferably more than 0.2 mass %. If the content of the coupling agent such as the silane coupling agent is more than the above-mentioned lower limit, the interfacial strength of the epoxy resin and the inorganic filler material will not be reduced, and the adhesion and waterproofness during the structural bodies such as the sealing electronic components or stators can be improved. And, as the upper limit of the content of the coupling agent such as the silane coupling agent, when the solid component of the molding resin composition is set to 100 mass %, it is preferably less than 1 mass %, more preferably less than 0.8 mass %, more preferably less than 0.6 mass %, more preferably less than 0.4 mass %. If the content of coupling agents such as silane coupling agents is below the above upper limit, the interfacial strength between the epoxy resin and the inorganic filler will not decrease, and the adhesion and waterproofness when sealing structures such as electronic components or stators can be improved. In addition, if the content of coupling agents such as silane coupling agents is below the above upper limit, the water absorption of the cured product of the molding resin composition can be prevented from increasing.
[0137] [characteristic]
[0138] The lower limit of the glass transition temperature (Tg) of the molding resin composition of the present embodiment measured by the following (method 1) is preferably 140°C or more, more preferably 150°C or more, further preferably 155°C or more, further preferably 160°C or more, and further preferably 165°C or more. When the glass transition temperature (Tg) is above the lower limit, the molding resin composition of the present embodiment can be cured even at low temperatures, and the heat resistance of the cured product of the molding resin composition of the present embodiment is improved.
[0139] In addition, the upper limit of the glass transition temperature (Tg) is not particularly limited, and is, for example, 300° C. or lower, 250° C. or lower, or 220° C. or lower.
[0140] (Method 1)
[0141] Using a transfer molding machine, the molding resin composition was molded into a test piece of 80 mm × 10 mm × 4 mm under the conditions of a mold temperature of 175 ° C, an injection pressure of 6.9 MPa, and a curing time of 90 seconds, and then cured at 175 ° C for 2 hours. Then, a thermomechanical analyzer was used to measure the thermal expansion coefficient of the obtained test piece at a heating rate of 5 ° C / min. Then, based on the obtained measurement results, the glass transition temperature (Tg) (°C) of the cured product was calculated according to the inflection point of the thermal expansion coefficient.
[0142] Here, the cured product for measuring the glass transition temperature is obtained by, for example, curing the resin composition at 175° C. for 2 hours.
[0143] Specifically, the glass transition temperature Tg can be obtained as follows: a test piece is obtained by injection molding the resin composition under the conditions of a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a curing time of 90 seconds using a low-pressure transfer molding machine, and the obtained test piece is cured at 175°C for 2 hours, and then the test piece is measured using a thermomechanical analysis device under the conditions of a measurement temperature range of 0°C to 320°C and a heating rate of 5°C / minute, and then calculated based on the obtained measurement results. As a low-pressure transfer molding machine, for example, KTS-15 and KTS-30 (manufactured by KOHTAKI Corporation.) can be used. In addition, as a thermomechanical analysis device, for example, TMA / SS6000 (manufactured by Seiko Instruments Inc.) or TMA7100 (manufactured by Hitachi High-Tech Science Corporation, Hitachi High-Tech Science Corporation) can be used.
[0144] The molding resin composition of this embodiment preferably sets the swirl length measured under the conditions of mold temperature 175°C, injection pressure 9.8MPa, and curing time 3 minutes as S1, and after the molding resin composition is placed at 25°C for 48 hours, the swirl length measured under the conditions of mold temperature 175°C, injection pressure 9.8MPa, and curing time 3 minutes is set as S2, and S2≥0.8×S1 is satisfied. Thus, it can be cured at low temperature, and the adhesion and waterproofness when sealing structures such as electronic components or stators can be improved, and in addition, the long-term storage property can also be improved.
[0145] The upper limit of the time for the torque value measured by the following (method 2) of the molding resin composition of the present embodiment to reach 2N·m is preferably less than 100 seconds, more preferably less than 70 seconds, further preferably less than 50 seconds, and further preferably less than 30 seconds. The molding resin composition of the present embodiment can be molded even at low temperatures by the time for the torque value to reach 2N·m being less than the above upper limit.
[0146] Furthermore, the lower limit of the time required for the torque value to reach 2 N·m is not particularly limited, and may be, for example, 0.1 seconds or more or 1 second or more.
[0147] (Method 2)
[0148] The torque value of the molding resin composition was measured over time using CURELASTOMETER (registered trademark, vulcanizer) at a mold temperature of 140°C and an amplitude angle of ±0.25 degrees. The time (seconds) from the start of the measurement until the torque value reached 2 N·m was calculated based on the measurement results.
[0149] As the CURELASTOMETER (registered trademark), for example, CURELASTO METER (registered trademark) MODEL 7 (manufactured by A&D Company, Limited) or the like can be used.
[0150] The swirl length of the molding resin composition of the present embodiment measured by the following (method 3) is preferably 70 cm or more, more preferably 80 cm or more, and further preferably 90 cm or more. When the swirl length is above the above lower limit, the adhesion and waterproofness when sealing structures such as electronic components or stators can be further improved.
[0151] Furthermore, the swirl length is preferably 180 cm or less, more preferably 160 cm or less, and even more preferably 140 cm or less. When the swirl length is equal to or less than the upper limit, the long-term storage stability of the molding resin composition of the present embodiment can be improved.
[0152] (Method 3)
[0153] The molding resin composition was injected into a mold for measuring swirl length according to ANSI / ASTM D 3123-72 using a low pressure transfer molding machine at 175°C, an injection pressure of 6.9 MPa, and a holding time of 3 minutes to measure the flow length, which was taken as the swirl length (cm).
[0154] As the low-pressure transfer molding machine, for example, the above-mentioned KTS-15 and KTS-30 (manufactured by KOHTAKI Corporation) and the like can be used.
[0155] The gel time of the molding resin composition of the present embodiment measured by the following (Method 4) is preferably 30 seconds or more, more preferably 40 seconds or more, and further preferably 50 seconds or more. When the gel time is equal to or greater than the above lower limit, the long-term storage stability of the molding resin composition of the present embodiment can be improved.
[0156] Furthermore, the gel time is preferably 80 seconds or less, more preferably 70 seconds or less, and even more preferably 60 seconds or less. When the gel time is equal to or less than the upper limit, the adhesion and waterproofness when sealing a structure such as an electronic component or a stator can be further improved.
[0157] (Method 4)
[0158] The molding resin composition was injected into a mold for measuring the swirl length according to ANSI / ASTM D 3123-72 using a low-pressure transfer molding machine at 175°C, an injection pressure of 6.9 MPa, and a holding time of 3 minutes. The time from the start of injection to the time when the molding resin composition solidified and no longer flowed was measured as the gel time (seconds).
[0159] As the low-pressure transfer molding machine, for example, the above-mentioned KTS-15 and KTS-30 (manufactured by KOHTAKI Corporation) and the like can be used.
[0160] The lower limit of the linear expansion coefficient α1 of the molding resin composition of the present embodiment measured by the following (Method 5) is not particularly limited, and is, for example, 0.8 ppm / °C or more, 1.0 ppm / °C or more, or 1.2 ppm / °C or more.
[0161] Furthermore, the linear expansion coefficient α1 is preferably 10.0 ppm / °C or less, more preferably 5.0 ppm / °C or less, further preferably 3.0 ppm / °C or less, and further preferably 2.0 ppm / °C or less. When the linear expansion coefficient α1 is below the upper limit, the adhesion and waterproofness when sealing a structure such as an electronic component or a stator can be further improved.
[0162] (Method 5)
[0163] Using a low-pressure transfer molding machine, the molding resin composition was injection molded under the conditions of a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a curing time of 3 minutes to obtain a 15mm×4mm×4mm molded product. Next, the obtained molded product was post-cured at 175°C for 4 hours to prepare a test piece. Then, for the obtained test piece, a thermomechanical analysis device was used to measure the average linear expansion coefficient α1 (ppm / °C) at 25 to 70°C under the conditions of a measurement temperature range of 0°C to 400°C and a heating rate of 5°C / min.
[0164] As the low pressure transfer molding machine, for example, the above-mentioned KTS-15 and KTS-30 (manufactured by KOHTAKI Corporation) can be used. In addition, as the thermomechanical analysis apparatus, for example, the above-mentioned TMA / SS6000 (manufactured by Seiko Instruments Inc.) or TMA7100 (manufactured by Hitachi High-Technologies Corporation) can be used.
[0165] The thermal conductivity of the molding resin composition of the present embodiment measured by the following (Method 6) is preferably 0.5 W / m·K or more, more preferably 0.6 W / m·K or more, further preferably 0.7 W / m·K or more, and further preferably 0.8 W / m·K or more. When the thermal conductivity is greater than the above lower limit, the heat of the electronic component in the molded body using the molding resin composition of the present embodiment can be effectively released.
[0166] Furthermore, the thermal conductivity is preferably 3.5 W / m·K or less, more preferably 3.3 W / m·K or less, further preferably 3.1 W / m·K or less, further preferably 2.9 W / m·K or less, and further preferably 2.8 W / m·K or less. When the thermal conductivity is below the above upper limit, the influence of heat from the outside on the electronic component inside the molded body using the molding resin composition of the present embodiment can be suppressed.
[0167] (Method 6)
[0168] Using a transfer molding machine, the molding resin composition was injection molded under the conditions of a mold temperature of 175°C, an injection pressure of 6.9MPa, and a curing time of 90 seconds to obtain a molded body of 80mm×10mm×4mm. Next, the obtained molded body was post-cured at 175°C for 2 hours to obtain a test piece. For the obtained test piece, the thermal diffusion coefficient was measured using a laser flash method. In addition, an electronic densimeter was used to measure the specific gravity of the test piece used for the thermal conductivity coefficient measurement. In addition, a differential scanning calorimeter was used to measure the specific heat of the test piece used for the thermal conductivity coefficient and specific gravity measurement. Based on the measured values of the thermal diffusion coefficient, specific gravity, and specific heat, the thermal conductivity (W / m·K) in the thickness direction of the test piece was calculated.
[0169] As the transfer molding machine, for example, the above-mentioned KTS-15 and KTS-30 (manufactured by KOHTAKI Corporation.) can be used. In addition, when the thermal diffusion coefficient is measured by the laser flash method, for example, a xenon flash analyzer LFA447 (manufactured by NETZSCH) can be used. In addition, as an electronic specific gravity meter, for example, SD-200L (manufactured by Alfa Mirage Co., Ltd.) can be used. And as a differential scanning calorimeter, for example, DSC8230 (manufactured by Rigaku Corporation) can be used.
[0170] [use]
[0171] The molding resin composition of the present embodiment can be used to seal a substrate on which electronic components are mounted, a stator core having a plurality of slots formed along the circumferential direction and fixed to the substrate, and a plurality of coils housed in the slots. The stator having the molding resin composition of the present embodiment as a sealing material can be applied to a motor (motor) as a rotating electrical machine (motor, generator, or motor / generator dual-purpose machine).
[0172] <Sealing structure>
[0173] Hereinafter, a sealing structure 200 using the molding resin composition according to the present embodiment will be described with reference to the drawings.
[0174] Figure 1 Schematically showing a top view of the sealed body 100 and the sealing structure 200 before and after molding. Figure 2 The figures schematically show side views of the sealed object 100 and the sealing structure 200 before and after molding. (a) and (c) schematically show the sealed object 100 before molding, and (b) and (d) schematically show the sealing structure 200 after molding.
[0175] The sealing structure 200 of the present embodiment comprises: a sealed body 100 including a substrate 10 on which an electronic component 11 is mounted, a stator core 20 fixed to one surface of the substrate 10 and having a plurality of slots 21 formed along the circumferential direction, and a plurality of coils 30 accommodated in the slots 21; and a sealing member 50 provided in a manner covering a part or all of the sealed body 100. The sealing member 50 is composed of a cured product of the molding resin composition of the present embodiment.
[0176] In the sealed structure 200 of the present embodiment, the sealed body 100 sealed by the molding resin composition of the present embodiment includes a substrate 10 carrying an electronic component 11, a stator core 20 fixed to one surface of the substrate 10 and having a plurality of slots 21 formed along the circumferential direction, and a plurality of coils 30 housed in the slots 21.
[0177] like Figure 1 As shown, the substrate 10 is a substrate on which electronic components 11 are mounted on one or both of one surface and another surface opposite to the one surface. Figure 1 As shown, the substrate 10 has, for example, a flat plate shape.
[0178] The substrate 10 may have a solder resist layer on one side on which the electronic component 11 is mounted. The solder resist layer may be formed using a solder resist forming resin composition commonly used in the field of semiconductor devices. In this embodiment, for example, the solder resist layer may be provided on one side and the other side of the substrate 10.
[0179] The solder resist layer provided on one surface, or both of one surface and the other surface of the substrate 10 is formed of, for example, a resin composition containing an organic silicon compound. Thereby, a solder resist layer having excellent surface smoothness can be realized.
[0180] like Figure 1 As shown in (a), the electronic component 11 is mounted on one surface and the other surface of the substrate 10, for example. On the other hand, the electronic component 11 may be provided only on one surface of the substrate 10 and not provided on the other surface of the substrate 10.
[0181] As the electronic component 11, for example, there can be cited light-emitting elements such as LED chips, biological detectors for detecting biological potentials such as brain waves / myographic potentials or physiological activities such as blood pressure / pulse, general detectors for detecting environmental information such as pressure / temperature / position / humidity / light / sound / acceleration, portable power sources such as capacitors, sound modules, communication modules and the like, or wiring connecting the above components.
[0182] Here, preferably, the lead 40 is connected to the substrate 10 and the electronic component 11. Before being sealed by the molding resin composition of the present embodiment, the lead 40 is connected to the substrate 10 and the electronic component 11, thereby the lead 40 can be sealed together with the connection portion between the substrate 10 and the electronic component 11 by the sealing member 50 described later, and as a result, the waterproofness of the sealing structure 200 of the present embodiment can be improved.
[0183] The stator core 20 is Figure 1 As shown in (a), when viewed from the axial end, a plurality of grooves 21 are provided along the circumferential direction. Figure 1 As shown in (a), four grooves 21 are provided. Figure 2 As shown in (c), the stator core 20 is fixed to one surface of the substrate 10 on which the electronic component 11 is mounted.
[0184] The stator core 20 may be provided by stacking a plurality of electromagnetic steel sheets in the axial direction and closely fixing them, or may be provided by molding a resin composition.
[0185] The coil 30 is, for example, a flat wire U-shaped and is wound so as to be accommodated in two separated slots 21. The coil 30 has a first coil end and a second coil end. The first coil end protrudes to one side in the axial direction of the stator core 20. The second coil end protrudes to the other side in the axial direction of the stator core 20. That is, the coil 30 has a pair of coil ends protruding to both sides of the axial direction of the stator core 20, respectively.
[0186] like Figure 1 (b) and Figure 2 As shown in (d), the sealing member 50 seals the substrate 10 on which the electronic component 11 is mounted, the stator core 20 fixed to one surface of the substrate 10 and having a plurality of slots 21 formed along the circumferential direction, and the plurality of coils 30 accommodated in the slots 21. That is, the sealing member 50 is provided in a manner of covering a part or the whole of the sealed body 100, which includes the substrate 10 on which the electronic component 11 is mounted, the stator core 20 fixed to one surface of the substrate 10 and having a plurality of slots 21 formed along the circumferential direction, and the plurality of coils 30 accommodated in the slots 21.
[0187] As the material of the sealing member 50 , the above-mentioned molding resin composition is used.
[0188] At this time, if Figure 1 (b) and Figure 2 As shown in (d), the lead wires 40 are preferably sealed by a sealing member 50 together with the connection portion between the substrate 10 and the electronic component 11. In this way, the waterproof property of the sealing structure 200 of the present embodiment can be improved.
[0189] <Method for manufacturing sealing structure>
[0190] Hereinafter, a method for producing a sealing structure using the molding resin composition of the present embodiment will be described.
[0191] The method for manufacturing a sealing structure of the present embodiment includes the steps of: placing a substrate on which electronic components are mounted, a stator core having a plurality of slots formed along a circumferential direction and fixed to the substrate, and a plurality of coils housed in the slots in a molding die in a transfer molding machine; and
[0192] A step of seal-molding the substrate, the stator core, and the coil in the mold with the molding resin composition of the present embodiment by transfer molding using the transfer molding machine to obtain a sealed structure.
[0193] The above process of obtaining the above sealing structure is carried out, for example, at a temperature of 80°C or higher and lower than 180°C and a pressure of 1MPa or higher and 15MPa or lower. Preferably, the above process is carried out at a temperature of 120°C or higher and 170°C or lower and a pressure of 3MPa or higher and 12MPa or lower. Thus, a sealing structure having excellent adhesion and waterproof properties can be obtained.
[0194] In this case, the step of obtaining the sealed structure is preferably performed by sealing and molding at a temperature lower than the Tg of the cured product of the molding resin composition.
[0195] The above-mentioned process of obtaining the above-mentioned sealing structure may include:
[0196] (A) a molding process using transfer molding, compression molding, etc.; and
[0197] (B) A post-curing step of heating the molded body after the molding step.
[0198] In a general sealing process, after the above-mentioned (A), the above-mentioned (B) is performed for the purpose of curing the epoxy resin and obtaining a good cross-linked structure.
[0199] In contrast, in a preferred mode of this embodiment, the post-curing step (B) is not performed, and only the molding step (A) is performed. In this way, productivity is improved, and thermal damage caused by post-curing, that is, thermal damage to the stator core, coil and substrate as the sealing object, can be suppressed, and a good sealing structure can be obtained.
[0200] In the present embodiment, the molding resin composition is configured such that the flexural modulus of a cured product obtained by curing at 140° C. for 2 minutes at 25° C. (in accordance with JIS K6911:2006) is 0.1 GPa to 30 GPa. Therefore, even if (B) is omitted, a good crosslinked structure can be obtained.
[0201] Furthermore, in the present embodiment, the molding temperature in (A) is preferably set to a temperature below Tg (°C) of the cured product obtained from the molding resin composition, more preferably below (Tg-10°C), and most preferably below (Tg-30°C). Furthermore, the molding temperature is preferably below 160°C, more preferably below 140°C, and most preferably below 130°C.
[0202] By molding at such a low temperature, thermal damage to the stator core, coil, and substrate to be sealed can be suppressed, and a good sealing structure can be obtained.
[0203] The lower limit of the molding temperature is not particularly limited as long as the molding resin composition can be sufficiently cured, and can be, for example, (Tg-80° C.) or higher, or 90° C. or higher.
[0204] The post-curing temperature during the post-curing of (B) is also preferably in the same range as the above-mentioned molding temperature. That is, it is preferably set to a temperature below Tg (°C) of the cured body obtained from the molding resin composition, more preferably below (Tg-10°C), and most preferably below (Tg-30°C). In addition, the molding temperature is preferably below 160°C, more preferably below 140°C, and most preferably below 130°C. By performing post-curing at such a low temperature, thermal damage to the sealed object can be suppressed, and a good sealed structure can be obtained. There is no particular restriction on the lower limit of the molding temperature, for example, it can be set to above (Tg-80°C), and can be set to above 90°C.
[0205] In a normal sealing process, the temperature of (A) or (B) is usually set to a temperature exceeding the Tg (°C) of the cured product obtained from the molding resin composition. In contrast, in the present embodiment, the temperature range of the low temperature domain is preferred. In the present embodiment, the molding resin composition is constructed in such a way that the bending modulus of elasticity at 25°C (according to JIS K6911:2006) of the cured product obtained by curing at 140°C for 2 minutes is 0.1 GPa or more and 30 GPa or less, so even if the temperature of (A) or (B) is set to a low temperature, a good cross-linked structure can be obtained.
[0206] As mentioned above, although embodiment of this invention was demonstrated, these are examples of this invention, and various structures other than this are also employable.
[0207] Example
[0208] Hereinafter, the present invention will be described based on Examples and Comparative Examples, but the present invention is not limited thereto.
[0209] (Example 1 to Example 4, Comparative Example 1 to Comparative Example 2)
[0210] <Preparation of molding resin composition>
[0211] For each of the Examples and Comparative Examples, a molding resin composition was prepared in the following manner.
[0212] First, each component shown in Table 1 was mixed using a mixer. Then, the obtained mixture was roll-kneaded, and then cooled and pulverized to obtain a molding resin composition in the form of a powder or granular body.
[0213] The detailed information of each component in Table 1 is as follows. The scheme shown in Table 1 represents the content (mass %) of each component relative to the entire resin composition.
[0214] (Inorganic filler)
[0215] Inorganic filler 1: fused spherical silica (manufactured by Denka Company Limited, product name "FB-950")
[0216] Inorganic filler 2: fused spherical silica (manufactured by Denka Company Limited, product name "FB-105")
[0217] Inorganic filler 3: Alumina (manufactured by Denka Company Limited, product name "DAW-02")
[0218] (Coupling agent)
[0219] Coupling agent 1: N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Dow Corning Toray Co., Ltd., product name "CF-4083")
[0220] (Epoxy resin)
[0221] Epoxy resin 1: o-cresol novolac type epoxy resin (manufactured by DIC CORPORATION, product name "EPICRON N-670")
[0222] (Curing agent)
[0223] Curing agent 1: Phenol aralkyl type resin containing biphenylene skeleton (produced by Meiwa Chemicals Co., Ltd., product name "MEH-7851SS")
[0224] Curing agent 2: triphenylmethane type phenol novolac resin (produced by Meiwa Chemicals Co., Ltd., product name "MEH-7500")
[0225] (Sealing agent)
[0226] · Adhesive additive 1: 3-amino-1,2,4-triazole (curing catalyst)
[0227] Curing catalyst 1: 2-phenylimidazole
[0228] Curing catalyst 2: 2-phenyl-4,5-dihydroxymethylimidazole (coloring material)
[0229] Coloring material 1: Carbon black (manufactured by Mitsubishi Chemical Corporation, product name "Carbon #5")
[0230] <Evaluation of performance of molding resin composition>
[0231] The obtained molding resin composition was evaluated for the following items. The evaluation results are shown in Table 1 below.
[0232] (Flexural modulus)
[0233] The resin composition was injection molded using a low pressure transfer molding machine (manufactured by KOHTAKI Corporation, KTS-30) at a mold temperature of 140°C, an injection pressure of 9.8 MPa, and a curing time of 2 minutes to obtain a molded product having a length of 80 mm, a width of 10 mm, and a thickness of 4 mm. The obtained molded product was subjected to a heat treatment at 200°C for 4 hours as a post-curing to obtain a test piece, and the flexural modulus (GPa) was measured at an ambient temperature of 25°C in accordance with JIS K 6911:2006.
[0234] (Low temperature moldability)
[0235] Using CURELASTOMETER (registered trademark) (manufactured by A&D Company, Limited, CURELASTOMETER (registered trademark, vulcanizer) MODEL7), the torque value of the obtained molding resin composition was measured over time under the conditions of mold temperature 140°C and amplitude angle ±0.25 degrees. According to the measurement results, the time (seconds) from the start of the measurement to the torque value reaching 2N·m was calculated. According to the time (seconds) when the torque value reaches 2N·m, the low temperature moldability was evaluated according to the following standards.
[0236] A: The time it takes for the torque value to reach 2N·m is less than 30 seconds (this is the case in the example)
[0237] B: The time for the torque value to reach 2N·m is more than 30 seconds and less than 100 seconds
[0238] C: The time for the torque value to reach 2N·m is more than 100 seconds (adhesion / waterproofness)
[0239] for A glass epoxy substrate (a substrate on which an IC package and an aluminum electrolytic capacitor are mounted) is injection molded on the substrate in a manner to a thickness of 2 cm using a low-pressure transfer molding machine (manufactured by KOHTAKI Corporation, KTS-30) at a mold temperature of 140° C., an injection pressure of 3 to 5 MPa, and a curing time of 2 minutes without post-curing to obtain a substrate sealed body.
[0240] Then, the substrate sealed body was immersed in a pure water bath with a depth of 15 to 100 cm for 1000 hours. After natural drying, the continuity of the circuit wiring on the substrate was confirmed using a tester.
[0241] A: No poor conduction
[0242] B: There is poor conduction (short circuit, increased resistance, etc.)
[0243] (Swirl length / Gel time)
[0244] The molding resin composition of each example and each comparative example was injected into a mold for measuring the swirl length according to ANSI / ASTM D 3123-72 using a low-pressure transfer molding machine (manufactured by KOHTAKI Corporation, "KTS-15") at 175°C, an injection pressure of 6.9 MPa, and a holding time of 3 minutes, and the flow length was measured as the swirl length (cm). In addition, the time from the start of injection until the molding resin composition solidified and no longer flowed was measured as the gel time (seconds).
[0245] Among them, the swirl length is a parameter of fluidity, and the larger the value is, the better the fluidity is.
[0246] (Linear expansion coefficient α1)
[0247] The linear expansion coefficient of the obtained molding resin composition was measured for each embodiment and each comparative example. A low-pressure transfer molding machine ("KTS-30" manufactured by KOHTAKI Corporation) was used to perform injection molding under the conditions of a mold temperature of 175°C, an injection pressure of 9.8MPa, and a curing time of 3 minutes to obtain a 15mm×4mm×4mm molded product. Next, the obtained molded product was post-cured at 175°C for 4 hours to prepare a test piece. Then, for the obtained test piece, a thermomechanical analyzer (manufactured by Seiko Instruments Inc., TMA100) was used to measure the average linear expansion coefficient α1 (ppm / °C) at 25 to 70°C under the conditions of a measurement temperature range of 0°C to 400°C and a heating rate of 5°C / minute.
[0248] (Glass transition temperature (Tg))
[0249] The glass transition temperature of the molding resin composition of each embodiment and each comparative example is measured in accordance with JIS K 6911:2006. That is, for each embodiment and each comparative example, the molding resin composition is molded into a test piece of 80 mm × 10 mm × 4 mm using a transfer molding machine (manufactured by KOHTAKI Corporation, "KTS-15") under the conditions of a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a curing time of 90 seconds. Then, post-curing is performed at 175°C for 2 hours. A thermomechanical analyzer (manufactured by Seiko Instruments Inc., TMA / SS6000) is then used to measure the thermal expansion coefficient of the obtained test piece at a heating rate of 5°C / min. Next, based on the obtained measurement results, the glass transition temperature (Tg) (°C) of the cured product is calculated from the inflection point of the thermal expansion coefficient.
[0250] (Thermal conductivity)
[0251] For the molding resin composition of each embodiment and each comparative example, injection molding was performed using a transfer molding machine (manufactured by KOHTAKI Corporation, "KTS-15") under the conditions of a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a curing time of 90 seconds to obtain a molded body of 80 mm×10 mm×4 mm. Then, the obtained molded body was post-cured at 175°C for 2 hours to obtain a test piece. For the obtained test piece, the thermal diffusion coefficient was measured using a laser flash method (xenon flash analyzer LFA447 manufactured by NETZSCH). In addition, the specific gravity of the test piece used for the thermal conductivity measurement was measured using an electronic densimeter SD-200L manufactured by Alfa Mirage Co., Ltd. In addition, the specific heat of the test piece used for the thermal conductivity and specific gravity measurement was measured using a differential scanning calorimeter DSC8230 manufactured by Rigaku Corporation. Based on the measured values of the thermal diffusion coefficient, specific gravity, and specific heat, the thermal conductivity (W / m·K) in the thickness direction of the test piece was calculated.
[0252] (Room temperature storage)
[0253] The room temperature storage properties of the molding resin compositions of each embodiment and each comparative example were measured. Using a low-pressure transfer molding machine ("KTS-30" manufactured by KOHTAKI Corporation), the molding resin compositions of each embodiment and each comparative example were injected under the conditions of a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a curing time of 3 minutes, and the flow length was measured, and the swirl length at this time was set as S1.
[0254] Furthermore, after the molding resin composition of each Example and each Comparative Example was left to stand at 25° C. for 48 hours, the flow length was measured under the same conditions as above, and the swirl length at this time was defined as S2.
[0255] The above S1 and S2 were evaluated according to the following criteria.
[0256] A: Satisfies S2≥0.8×S1.
[0257] B: Satisfies S2<0.8×S1.
[0258] [Table 1]
[0259]
[0260] The molding resin compositions of the examples can all be cured at low temperatures and have excellent adhesion and waterproof properties when sealing structures such as electronic components and stators.
[0261] This application claims priority based on Japanese patent application No. 2022-058500 filed on March 31, 2022, and all the disclosed contents thereof are incorporated herein by reference.
[0262] Description of Reference Numerals
[0263] 10 - substrate, 11 - electronic component, 20 - stator core, 21 - slot, 30 - coil, 40 - lead wire, 50 - sealing component, 100 - sealed body, 200 - sealing structure.
Claims
1. A molding resin composition that can be used to seal a substrate on which an electronic component is mounted, a stator core having a plurality of slots formed along a circumferential direction and fixed to the substrate, and a plurality of coils housed in the slots, wherein the molding resin composition is characterized in that: contain: Epoxy resin, One or both of a curing agent and a curing catalyst, and Inorganic filling materials, The flexural modulus of a cured product obtained by curing the molding resin composition at 140° C. for 2 minutes at 25° C. according to JIS K6911:2006 is 0.1 GPa or more and 30 GPa or less.
2. The molding resin composition according to claim 1, characterized in that The glass transition temperature Tg measured by the following method 1 is 140°C to 300°C, Method 1: The molding resin composition was molded into a test piece of 80 mm × 10 mm × 4 mm using a transfer molding machine under the conditions of a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a curing time of 90 seconds. The test piece was post-cured at 175°C for 2 hours, and then the thermal expansion coefficient of the obtained test piece was measured using a thermomechanical analyzer at a heating rate of 5°C / min. Then, based on the obtained measurement results, the glass transition temperature Tg of the cured product was calculated according to the inflection point of the thermal expansion coefficient, in °C.
3. The molding resin composition according to claim 1 or 2, characterized in that The epoxy resin contains one or more selected from the group consisting of phenol novolac epoxy resin, cresol novolac epoxy resin and trisphenol methane epoxy resin.
4. The molding resin composition according to any one of claims 1 to 3, characterized in that When the solid content of the molding resin composition as a whole is 100% by mass, the content of the epoxy resin is 3% by mass or more and 40% by mass or less.
5. The molding resin composition according to any one of claims 1 to 4, characterized in that The molding resin composition contains the curing agent, and the curing agent contains a phenolic resin-based curing agent.
6. The molding resin composition according to claim 5, characterized in that The phenolic resin-based curing agent contains one or more selected from the group consisting of phenol novolac resin, cresol novolac resin, naphthol novolac resin and trisphenol methane type phenolic resin.
7. The molding resin composition according to claim 5 or 6, characterized in that When the solid content of the molding resin composition as a whole is 100% by mass, the content of the curing agent is 0.8% by mass or more and 12% by mass or less.
8. The molding resin composition according to any one of claims 1 to 7, characterized in that The molding resin composition contains the curing catalyst, and the curing catalyst contains an imidazole compound.
9. The molding resin composition according to claim 8, characterized in that When the solid content of the molding resin composition as a whole is 100% by mass, the content of the curing catalyst is 0.01% by mass or more and 2.0% by mass or less.
10. The molding resin composition according to any one of claims 1 to 9, characterized in that The swirl length of the molding resin composition measured under the conditions of a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a curing time of 3 minutes is set as S1. After the molding resin composition is placed at 25°C for 48 hours, the swirl length measured under the conditions of a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a curing time of 3 minutes is set as S2, and S2≥0.8×S1 is satisfied.
11. The molding resin composition according to any one of claims 1 to 10, characterized in that The time it takes for the torque value measured by the following method 2 to reach 2N·m is less than 100 seconds. Method 2: use The torque value of the molding resin composition was measured over time under the conditions of a mold temperature of 140° C. and an amplitude angle of ±0.25 degrees. Based on the measurement results, the time from the start of the measurement until the torque value reached 2 N·m was calculated in seconds.
12. The molding resin composition according to any one of claims 1 to 11, characterized in that The swirl length measured by the following method 3 is more than 70 cm, Method 3: The molding resin composition was injected into a mold for measuring swirl length according to ANSI / ASTM D3123-72 using a low-pressure transfer molding machine at 175° C., an injection pressure of 6.9 MPa, and a holding time of 3 minutes to measure the flow length, which was used as the swirl length in cm.
13. The molding resin composition according to any one of claims 1 to 12, characterized in that The gel time measured by the following method 4 is 30 seconds or more, Method 4: Using a low-pressure transfer molding machine, the molding resin composition is injected into a mold for measuring the swirl length in accordance with ANSI / ASTM D3123-72 under the conditions of 175°C, an injection pressure of 6.9 MPa, and a holding time of 3 minutes. The time from the start of injection to the time when the molding resin composition solidifies and no longer flows is measured as the gel time in seconds.
14. The molding resin composition according to any one of claims 1 to 13, characterized in that The linear expansion coefficient α1 measured by the following method 5 is 10.0 ppm / °C or less, Method 5: The molding resin composition was injection molded using a low-pressure transfer molding machine at a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a curing time of 3 minutes to obtain a molded product of 15 mm × 4 mm × 4 mm. The molded product was then post-cured at 175°C for 4 hours to prepare a test piece. A thermomechanical analyzer was used to measure the average linear expansion coefficient α1 at 25 to 70°C in a measuring temperature range of 0°C to 400°C and a heating rate of 5°C / min. The unit is ppm / °C.
15. The molding resin composition according to any one of claims 1 to 14, characterized in that The thermal conductivity measured by the following method 6 is 0.5 W / m·K or more, Method 6: The molding resin composition was injection molded using a transfer molding machine under the conditions of a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a curing time of 90 seconds to obtain a molded body of 80 mm×10 mm×4 mm. The obtained molded body was then post-cured at 175°C for 2 hours to obtain a test piece. The thermal diffusion coefficient of the obtained test piece was measured using a laser flash method, and the specific gravity of the test piece for measuring the thermal conductivity coefficient was measured using an electronic densimeter. Furthermore, the specific heat of the test piece for measuring the thermal conductivity coefficient and specific gravity was measured using a differential scanning calorimeter. Based on the measured values of the thermal diffusion coefficient, specific gravity, and specific heat, the thermal conductivity of the test piece in the thickness direction was calculated in W / m·K.
16. A method for manufacturing a sealing structure, characterized in that: include: A step of placing a substrate on which electronic components are mounted, a stator core having a plurality of slots formed along a circumferential direction and fixed to the substrate, and a plurality of coils received in the slots in a molding die in a transfer molding machine; and A step of seal-molding the substrate, the stator core, and the coil in the molding die with the molding resin composition according to any one of claims 1 to 15 by transfer molding using the transfer molding machine to obtain a sealed structure.
17. The method for manufacturing a sealing structure according to claim 16, characterized in that: In the step of obtaining the sealed structure, sealing molding is performed at a temperature not higher than the Tg of the cured product of the molding resin composition.
18. The method for manufacturing a sealing structure according to claim 16 or 17, characterized in that: As the step of obtaining the sealing structure, no post-curing step is performed.
19. A sealing structure, characterized in that: A sealed body and a sealing member provided so as to cover a part or the whole of the sealed body. The sealed body includes a substrate on which electronic components are mounted, a stator core fixed to one surface of the substrate and having a plurality of slots formed along a circumferential direction, and a plurality of coils housed in the slots. The sealing member is composed of a cured product of the molding resin composition according to any one of claims 1 to 15.