Method and apparatus for producing nanoscale particles for energy storage materials
By using an electrospace-stabilized slurry method in a media mill and using a polyelectrolyte dispersant to produce nanoscale particles in wet grinding, the problems of particle agglomeration and mill clogging are solved, and high-efficiency, low-energy consumption nanoscale particles are achieved. Pellets production, suitable for industrial scale.
Patent Information
- Application Number
- CN202380027471.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-15
- Filing Date
- 2023-03-15
- Publication Date
- 2024-10-29
AI Technical Summary
When producing nanoscale particles, especially in the submicron size range, the existing technology is prone to particle agglomeration and mill screen clogging, resulting in low grinding efficiency and high energy consumption, and is difficult to implement in industrial-scale manufacturing.
Adopting the electrosterically stabilized slurry method, by adding polyelectrolytes as electrosteric dispersants in the media mill, electrostatic and steric stabilization mechanisms are used to separate particles and reduce agglomeration, and are operated in wet grinding to form particles smaller than 1 micron. Nanoscale particles.
It effectively avoids particle agglomeration and mill screen clogging, improves grinding efficiency, reduces energy consumption, and is suitable for industrial-scale manufacturing, capable of producing nanoscale particles with a particle size of less than 1 micron.
Smart Images

Figure CN118872087A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to U.S. Patent Application No. 17 / 654,915, filed on March 15, 2022, which is incorporated herein by reference in its entirety. Technical Field
[0003] The present disclosure generally relates to methods and apparatus for producing ultrafine particles for various industrial and commercial purposes, including the preparation of energy storage materials and / or devices. More specifically, the present disclosure relates to methods and apparatus for producing nanoscale particles using electrosterically stabilized slurries in media mills such as ball mills, planetary mills, cone mills, and stirred media mills. The nanoscale particles can be used in the production of energy storage materials, for example as battery precursor materials for use in electrodes and / or separators for batteries and capacitors. Background Art
[0004] Media grinding generally refers to a process in which media particles of relatively large size are broken into relatively small sizes by applying mechanical work. Traditional grinding methods include dry grinding and wet grinding. In dry grinding, air (or an inert gas) is used to keep the particles in suspension while applying mechanical work to the particles. However, as the particle size decreases, the fine particles tend to agglomerate in response to van der Waals forces, which limits the ability of dry grinding. In contrast, wet grinding uses liquids such as water or organic solvents such as alcohols, aldehydes and ketones to control the reagglomeration of fine particles. In this way, wet grinding is typically used for the pulverization of submicron-sized particles. Another process for preparing submicron particles is jet grinding. This is a dry method using supersonic air or steam. However, it is very expensive because it is highly energy-consuming.
[0005] In conventional practice, wet mills typically include grinding media that, when subjected to mechanical work such as stirring or agitation, exert sufficient force to break up particles suspended in a liquid medium. Grinding devices are classified by the method used to apply mechanical work to the media. The work applied in a wet mill can include stirring, tumbling, vibratory motion, planetary motion, agitation, and ultrasonic grinding, among others.
[0006] Of the aforementioned mill types, stirred media mills, which utilize balls of various sizes as their grinding media and agitation as their method of applying mechanical work, have several advantages for particle comminution, including high energy efficiency, high solids handling, narrow size distribution of product output, and the ability to produce a uniform slurry. Variables that may be considered in using stirred media mills include, for example, agitator speed, suspension flow rate, residence time, slurry viscosity and concentration, solid size of feed particles, grinding media (i.e., ball) size, media fill rate (i.e., amount of beads in the mill chamber), and desired product size.
[0007] However, despite these advantages, stirred media mills have several disadvantages when the desired product particle size is reduced to less than about 1 micron and especially less than about 500 nanometers. For example, in the submicron particle size range, the behavior of the product suspension (slurry) is increasingly affected by particle-particle interactions. Due to these interactions, spontaneous agglomeration of particles can occur, and the viscosity of the product suspension increases. When the product particle size is less than about 1 micron, these interactions can cause a state of equilibrium between agglomeration, deagglomeration and pulverization, thereby causing no further pulverization even when the energy input is increased. In addition, particle agglomeration together with the increase in the viscosity of the product suspension (which increases the required power consumption due to the high load on the electric mill) can cause blocking of the media mill screen and no further flow of the suspension, thereby preventing any particles from leaving the mill as a product.
[0008] Various methods have been tried to suppress these reagglomeration effects. For example, electrostatic stabilization methods have been used to maintain particle separation during grinding. As illustrated in Figure 1, electrostatic stabilization includes generating similar charges on the surface of colloidal particles so that the particles repel each other, thereby dispersing the suspension of particles. The electrostatic stabilization method can be performed by adjusting the pH of the product suspension. The regulation of pH can be controlled by adding an acid or base (including weak acids and strong acids and weak bases and strong bases). Alternatively, the electrostatic stabilization method can be performed by adding anionic or cationic dispersants to the product suspension. These dispersants electrostatically stabilize the product suspension by adding positive or negative charges to the particles when the dispersant is adsorbed on the surface of the particles.
[0009] However, these electrostatic methods have several disadvantages, making them difficult to implement in industrial scale manufacturing. In particular, with electrostatic methods, the method needs to be constantly monitored and regulated due to the fact that as the particle size decreases, their surface area increases, and any acid / base or dispersant added becomes less effective. As the specific surface area of the particles increases exponentially and the particle size decreases, more and more amounts of acid, base or dispersant are required, and if their amount deviates even slightly from the required amount, the entire suspension tends to flocculate, and grinding will no longer be possible due to a sudden increase in viscosity and blocking of the mill screen.
[0010] In other examples, steric stabilization methods have been used to maintain particle separation during grinding. The steric stabilization method utilizes a nonionic or electrically neutral dispersant to separate particles in the suspension. As illustrated in Figure 2, steric stabilization includes adsorbing a relatively long-chain polymer compound onto the surface of the particle. A portion of the polymer is strongly attached to the surface of the particle, but the remaining polymer can spread freely in the liquid medium of the suspension. If the liquid medium is a good solvent for the polymer, the mutual penetration of the polymer chains, i.e., the interaction of the polymer on the individual particles, is not energetically favorable. As a result, the individual particles repel each other (repel each other between particles), thereby dispersing the suspension.
[0011] However, similar to electrostatic methods, these steric methods have several disadvantages that make them difficult to implement in industrial-scale manufacturing. For example, steric stabilizing dispersants have the disadvantage that large amounts of dispersant are required as smaller and smaller particle sizes are produced. During grinding, the surface area of the particles increases exponentially, and the adsorption of these dispersants on the particle surface decreases, making the grinding process difficult to control.
[0012] One area of particular growing interest in processes that can realize the benefits from nanoscale particles is energy storage materials and systems. A large number of efforts are ongoing to develop renewable energy sources, combined with cost-effective energy storage, such as batteries, to store electricity during excess generation and supply during peak demand. In this regard, the development of low-cost, scalable energy storage systems with sufficient cycle life and safety is critical. In addition, obtaining high energy density without compromising safety is also important for many applications, such as electric vehicles and consumer electronics, such as mobile phones and laptop computers.
[0013] With respect to nanoscale particles and energy storage materials (e.g., for batteries), it is known that certain material factors can greatly affect performance. For example, increasing the surface area of the electrode will lead to improvements in the efficiency of the electrochemical reaction and promote ion exchange between the electrode and the electrolyte, especially within the anode, because the higher surface area allows for shorter diffusion paths for lithium ions between the anode particles. However, larger surface areas do have some limitations due to degradation of the interaction of the electrolyte at the electrode surface, resulting in loss of capacity and thermal stability. Therefore, nanoparticles hold great promise in increasing surface area without such capacity loss, which would promote fast charging, efficient discharge rates, and improved battery capacity.
[0014] The size, shape and tortuosity of the electrode pores will also significantly affect the transport rate of ions (such as lithium ions) through the electrolyte maintained in the porous structure of the electrode. The electrode microstructure produced by the manufacturing process has a direct impact on the energy density, power, life and reliability of lithium-ion batteries. In this way, a better understanding of the interconnectivity of adjacent pores, closed pores and channels that may be generated during the manufacturing process helps to ensure optimal electrolyte and electrode interactions. Knowing the tortuosity of the porous electrode and electrolyte interface can determine whether the performance limitations of the battery cell are due to its microstructure.
[0015] Other physical properties also show a large impact. For example, particle shape will affect properties such as packing density, because spherical particles will be more densely packed than fibrous or flaky particles. The density of electrodes such as graphite anodes has an impact on their ability to withstand degradation under challenging load and discharge operations. Higher anode electrode particle density reduces porosity, resulting in a lower active surface area of the electrode. This reduces the electrode / electrolyte contact area. Similarly, the electrode pore structure has a direct impact on the particle-to-particle contact between the active material and the conductive diluent. By controlling the porosity, higher intra-electrode conductivity can be achieved to ensure sufficient electron exchange and sufficient void space for electrolyte entry / transport of lithium ions (for example) for intercalation of the cathode. In contrast, pore blockage / obstruction during intercalation can lead to capacity decay.
[0016] Chemical composition is not the only way to influence the electrochemical properties of electrode materials. In order to obtain the best possible performance from cathode materials, particle size and morphology also need to be considered. In addition, successful lithiation is the most important factor in limiting the capacity of cathode materials. Precursors with different physical properties such as particle size and porosity have different requirements for lithiation time and temperature. In addition to porosity, particle size distribution has an impact on the final volumetric capacity and cycle stability.
[0017] The particle size of the electrode material is also important due to the effect on capacity, cycling and coulombic efficiency. The particle size will affect the amount of solid-state diffusion of lithium ions intercalated at the electrode. Smaller particles, especially nanoparticles, will result in smaller volume changes during cycling. This contributes to less mechanical stress, increased hardness and greater fracture resistance. Interestingly, it is reported that a wide particle size distribution can increase energy density more than a monodisperse distribution. In this way, controlling and customizing the particle size distribution can lead to the ability to make available custom adjustments, which will lead to high power (monodisperse) or high energy density (polydisperse) materials.
[0018] One such application that could benefit from such regulation and control is lithium-ion battery production. The advantages of nanoparticles with respect to lithium-ion battery applications are specifically that (i) they provide new reactions that cannot occur in micron-sized particles (e.g., the reaction of transition metal compounds with Li to result in Li2 X matrix, wherein X = O, S, F or N); (ii) nanostructured materials provide short path lengths for Li+ ion diffusion and electron transport compared to micron-sized particles and can therefore enhance charge / discharge rates; (iii) short path lengths for electron transport can allow the use of materials with low electronic conductivity; (iv) increased electrode / electrolyte contact area can also lead to enhanced charge / discharge rates; and (v) nanomaterials can accommodate large volume expansion / contraction associated with Li+ ion transport and retain electrode integrity, resulting in longer cycle life. Unfortunately, despite these promising effects, disadvantages include (i) high surface area can increase undesirable electrode / electrolyte reactions, leading to the formation of a solid electrolyte interface (SEI), resulting in self-discharge of the cell, poor cycling, low calendar life and poor safety; and (ii) poor packing of particles.
[0019] It would be desirable, therefore, to provide an improved method for producing particles in the submicron range using a wet grinding process. The wet grinding process would advantageously maintain particle separation as the particle size is reduced to less than 1 micron, thereby avoiding agglomeration and mill screen clogging. Furthermore, the wet grinding process would advantageously be suitable for industrial scale manufacturing to the extent that extremely tight control of any additives would not be required to prevent flocculation or a dramatic increase in viscosity of the product suspension. Such an improved method, when used in conjunction with specific precursor materials suitable for use in energy storage devices, would advantageously provide submicron particulate materials that can be used to prepare improved energy storage materials such as electrodes and separators for batteries, supercapacitors, and the like. Furthermore, other desirable features and characteristics of the isolator assembly will become apparent from the subsequent detailed description and appended claims, taken in conjunction with the accompanying drawings and the foregoing background technology. Summary of the invention
[0020] Disclosed herein are methods and apparatus for producing nanoscale particles using an electrosterically stabilized slurry in a media mill. According to one embodiment, the method for producing nanoscale particles includes adding a feed substrate suspension to a media mill. The feed substrate suspension includes a liquid carrier medium and feed substrate particles. The method also includes adding an electrosteric dispersant to the feed substrate suspension in the media mill. The electrosteric dispersant includes a polyelectrolyte, various examples of which are listed in more detail below. Further, the method includes operating the media mill for a period of time to comminute the feed substrate particles to form a nanoscale particle having a diameter (D) of less than about one micron. 90 ) particle size and recycled for further grinding of the nanoparticles from the media mill.
[0021] According to another embodiment, a media mill apparatus configured for producing nanoscale particles comprises a grinding chamber, an agitator extending into the grinding chamber, a grinding medium disposed within the grinding chamber, and a feed substrate suspension comprising a liquid carrier medium and feed substrate particles disposed within the grinding chamber and interspersed with the grinding medium. The media mill apparatus also includes an electrosteric dispersant comprising a polyelectrolyte mixed within the feed substrate suspension. The agitator is configured to apply mechanical work to the grinding medium for a period of time, thereby causing the grinding medium to break up the feed substrate particles to form nanoparticles having a diameter (D) of less than about one micron. 90 ) nanometer-scale particles of particle size.
[0022] According to another embodiment, a method for producing nanoscale particles in a media mill including grinding media is provided, wherein the method includes adding a feed substrate suspension to the media mill. The feed substrate suspension includes a liquid carrier medium (including water or an organic solvent) and feed substrate particles (including any solid material that needs to be ground to a small size), such as organic and inorganic solids, glass, graphene, metals, minerals, ores, silicon oxide, diatomaceous earth, clay, organic and inorganic pigments, pharmaceutical materials or carbon black. The feed substrate particles are present in the feed substrate suspension in an amount of about 5% to about 70% by weight of the feed substrate suspension, or about 5%-about 40% by weight. The method also includes adding an electric spatial dispersant to the feed substrate suspension in the media mill. The electric spatial dispersant includes a polyelectrolyte. The polyelectrolyte includes a polymer or copolymer having a charged functional group or an inorganic affinity group. The electric spatial dispersant is added in an amount of about 2% to about 20% by weight of the feed substrate particles. The method further includes operating the media mill for a period of time from about 10 minutes to about 6000 minutes to comminute the feed substrate particles to form a substrate having a particle size (D) of less than about one micron. 90 ) particle size, recycling the nano-sized particles from the media mill for further grinding, and separating the nano-sized particles from the grinding media. Further, the method includes drying the nano-sized particles after separating the nano-sized particles from the grinding media.
[0023] In additional embodiments, a method is provided for preparing nanoscale particles of electrochemical materials. The method includes adding a feed substrate suspension to a media mill. The feed substrate suspension includes a liquid carrier medium and electrochemical feed substrate particles. The method also includes adding an electrosteric dispersant to the feed substrate suspension in the media mill. The electrosteric dispersant includes a polyelectrolyte, various examples of which are listed in more detail below. Further, the method includes operating the media mill for a period of time to comminute the feed substrate particles to form a nanoscale particle having a diameter (D) of less than about one micron. 90) particle size and recycled for further grinding of the nanoscale particles from the media mill. The method includes optionally drying the nanoscale particles after separating the nanoscale particles from the grinding media, such as by spray drying. In some embodiments, recycling and further grinding of the nanoscale particles from the media mill prepares a slurry, and the method includes directly spray drying the slurry to produce the nanoscale particles as a dry powder.
[0024] This Summary is provided to introduce a selection of concepts in a simplified form that are further described below in the Detailed Description. This Summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used as an aid in determining the scope of the claimed subject matter.
[0025] BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The present disclosure will hereinafter be described in conjunction with the following drawings, wherein like numerals represent like elements, and wherein:
[0027] FIG1 is a conceptual illustration showing particle separation of a product suspension using electrostatic methods as practiced in the prior art;
[0028] FIG2 is a conceptual illustration showing separation of product suspension particles using a spatial approach as practiced in the prior art;
[0029] Figure 3A and 3B is a schematic diagram of a wet media mill that can be used to grind particles in a continuous process according to some embodiments of the present disclosure;
[0030] Figure 4 is a conceptual illustration showing separation of product suspension particles using an electrospatial approach according to some embodiments of the present disclosure;
[0031] Figure 5 is a flow chart illustrating a method for wet media milling according to some embodiments of the present disclosure;
[0032] Figures 6A-6E is a graph illustrating average particle size diameters of particles produced according to some examples of the present disclosure;
[0033] Figure 7 is a flow chart illustrating a method for preparing energy storage materials via wet media grinding and spray drying according to some embodiments of the present disclosure;
[0034] Fig. 8A and 8B is a scanning electron microscope (SEM) micrograph of the feed material used in the examples;
[0035] Fig. 9 is a SEM micrograph of spray-dried agglomerates of primary particles prepared in the Examples; and
[0036] Figures 10A-10E are SEM micrographs of spray-dried agglomerates prepared in the Examples, showing various views of the primary nanoparticles therein.
[0037] Detailed Description
[0038] The following detailed description is merely exemplary in nature and is not intended to limit the present invention or the application and use of the present invention. As used herein, the word "exemplary" means "used as an example, instance or illustration". Therefore, any embodiment described herein as "exemplary" need not be interpreted as being preferred or advantageous over other embodiments. In addition, as used herein, numerical sequences such as "first", "second", "third", etc., such as first, second and third components, merely represent multiple different singles, unless specifically limited by language in the appended claims. All embodiments and implementations described herein are exemplary embodiments, which are provided to enable those skilled in the art to make or use the present invention, rather than to limit the scope of the present invention as defined by the claims. In addition, it is not intended to be bound by any explicit or implicit theory presented in the aforementioned technical field, background technology, content of the invention or the following detailed description.
[0039] Embodiments of methods and apparatus for producing nanoscale particles using electrosterically stabilized slurries in media mills are disclosed herein. The disclosed embodiments utilize electrosteric (electrostatic and steric) stabilization of ultrafine (submicron) particles in a wet grinding method using an electrosteric dispersant. An electrosteric dispersant is a polymer that is capable of electrostatically and sterically stabilizing a suspension of product particles. Using an electrosteric dispersant reduces the use of the dispersant, requires controlling the amount of dispersant used to strict standards, and effectively avoids agglomeration of particles. This achieves improved grinding efficiency and reduced energy consumption for wet grinding methods because the viscosity of the suspension remains low, and further because the likelihood of mill screen clogging is reduced due to the reduced likelihood of agglomeration.
[0040] Nanoscale particles according to the present disclosure may represent a variety of substances that can be used in various industries. For example, particles that can be ground as described herein may include inorganic and organic solids, minerals, ores, silicon oxides, diatomaceous earth, clays, organic and inorganic pigments, pharmaceutical materials, carbon black, paint additives, pigments, photographic materials, cosmetics, chemicals, metal powders that can be used as catalysts and carriers, stationary phase particles that can be used for analytical and preparative chromatographic separations of chemical compounds, powdered toners, therapeutic and diagnostic imaging agents, pharmaceutically active agents, medicaments, plant and herbal extracts, drugs, prodrugs, pharmaceutical formulations, etc. As further described below, the method is used in some embodiments to prepare nanoscale particles for use in preparing electrochemical materials such as electrodes, separators, etc. for energy storage devices.
[0041] According to the methods of the present disclosure, nanoparticles have been shown to have a diameter less than one micrometer, such as less than 800 nanometers (nm) or less than 500 nm. 90 ) average particle size. As described in the following examples, a particle size having a D of about 5 microns was used. 90 The average particle size of the input particles was about 100 nm to about 200 nm. 10 Average particle size, D of about 150 to about 250 nm 50 The average particle size and D of about 250nm to about 350nm 90 The product particles have an average particle size. It is expected that the product particles have an average particle size in the aforementioned size range or in the aforementioned size range and about 100 microns or less (e.g., about 50 microns or less, or about 30 microns or less, or about 10 microns or less). 90 ) input size anywhere between will be used in almost any industrial or commercial application currently practiced. The following provides more details about the wet media grinding method and the electrosteric dispersant used in the grinding method. Specifically, the following together with Figure 3A (vertical wet media mill) and Figure 3B (Horizontal Media Mill) Two embodiments of the mill are disclosed.
[0042] Wet Media Grinding
[0043] In the wet grinding method, the repeated collision of the grinding media with the ground solid particulate material, i.e. the ground substrate, causes the repeated rupture of the substrate and the accompanying substrate particle size reduction. When the wet media grinding method is used to reduce the size of the particles of the substrate, the method is usually carried out in a mill, which includes a grinding chamber containing grinding media, a solid material or substrate to be ground, and a liquid carrier in which the medium and substrate are suspended. The contents of the grinding chamber are stirred or agitated with a stirrer that transfers mechanical work and energy to the grinding media. The grinding media accelerated in the energy collision that can crush, fragment, rupture or otherwise reduce the size of the solid substrate material and cause the overall reduction of the substrate particle size and the average (average) or median (mean) particle size distribution of the substrate to be overall reduced and collide with the substrate. The example of a suitable wet grinding system includes a ball mill, a planetary ball mill, a circulating stirred media mill, a basket stirred media mill, an ultrasonic media mill, etc.
[0044] The grinding media are usually selected from various dense and hard materials, such as sand, steel, silicon carbide, ceramics, zirconium silicate, zirconium and yttrium oxide (such as yttria-stabilized zirconium oxide), glass, aluminum oxide, titanium and some polymers, such as cross-linked polystyrene and methyl methacrylate. The media geometry can vary depending on the application, although spherical spheres or column beads are often used. In some embodiments, the grinding media can have a variety of sizes and size distributions, including large grinding media particles and smaller grinding media particles. Suitable liquid carriers for grinding media and substrates include water, aqueous saline solutions, buffered aqueous solutions, organic solvents such as ethanol, methanol, butanol, hexane, hydrocarbons, kerosene, water containing PEG, ethylene glycol, toluene, petroleum-based solvents, aromatic solvents such as mixtures of xylene and toluene, heptane, etc. Usually, the solvent will be selected based on the substrate (product) particles.
[0045] Wet media mills that can be used to reduce the particle size of solid substrates can be operated in batch mode or in continuous or semi-continuous mode. Wet media mills that operate in continuous mode can include a separator or screen for retaining grinding media together with relatively large particles of solid substrates ground in the grinding area or grinding chamber of the mill, while allowing smaller particles of the ground substrate, i.e., product substrate particles, to leave the grinding chamber in a recirculation or discontinuous passing mode. Recycling can be in the form of a slurry, suspension, dispersion or colloid of the substrate suspended in a fluid carrier phase, which is moved from the grinding chamber to a storage container and returned to the grinding chamber by means of a pump, for example. The separator or screen can be located at the outlet of the grinding chamber, including, for example, a rotating gap separator, a screen, a screen, a centrifugal auxiliary screen and a similar device that physically limits the passage of grinding media from the mill. Retention of the grinding media occurs because the size of the grinding media is greater than the size of the opening, and the substrate particles of reduced size can pass through the opening.
[0046] Figure 3A An exemplary vertical wet media mill 15 configured for use in accordance with some embodiments of the present disclosure is described, wherein reference numerals correspond to features described below:
[0047] 10: Motor
[0048] 11: Axis
[0049] 12: Entry port
[0050] 13: Loading level
[0051] 14: Blender
[0052] 15: Media Mill
[0053] 16: Grinding Room
[0054] 17: Secondary screen
[0055] 19: Export wire mesh
[0056] 20: Egress port
[0057] 31: Ingress port
[0058] 32: Collector
[0059] 33: Pipeline system
[0060] 34: Pump
[0061] 35: Pipeline system
[0062] An exemplary wet media mill 15 is now described in terms of its general operation. In an embodiment, grinding media (not shown) and a fluid carrier containing an electrosteric dispersant may be added to the grinding chamber 16 of the media mill 15 through the inlet port 12. (Electrosteric dispersants are described in more detail below.) During this time of loading the media mill 15, the agitator 14 may optionally be in operation, and the outlet port 20 may be open to allow the fluid carrier to exit from the media mill 15, or it may be closed to contain the fluid carrier. Optionally, a secondary larger screen 17 including openings may be provided in the media mill 15 through which the grinding media may pass.
[0063] The grinding chamber 16 can then be loaded with the solid substrate to be ground and optionally additional fluid carrier (optionally including additional electrosteric dispersant). In addition, the grinding chamber 16 can also be loaded with a defoamer as known in the art to prevent bubble formation during the grinding process. In an embodiment, once all the fluid carrier and substrate are added, the slurry can have a solid content of about 5% by weight to about 40% by weight, for example, about 10% by weight to about 40% by weight, or about 15% by weight to about 40% by weight, or about 20% by weight to about 40% by weight. The outlet port 20 of the grinding chamber 16 can then be closed and the media mill 15 can be loaded to level 13. The fluid carrier can be transferred to the collector 32 via the inlet port 31 using a pipe system 35 by means of a pump 34. The fluid carrier can be pumped back to the inlet port 12 of the media mill 15 from the collector 32 via the pipe system 33.
[0064] The contents of the media mill 15 are agitated or stirred by an agitator 14 driven by a motor 10 and connected to a shaft 11, preferably at high speed or using high acceleration and deceleration. The time period of agitation to produce a product according to the present disclosure can range, for example, from about 10 minutes to about 6000 minutes or longer, such as about 10 minutes to about 3000 minutes, or about 10 minutes to about 1000 minutes. The fluid carrier is continuously recycled from the grinding chamber 16 to the collector 32. This recycling can continue until a minimum or desired substrate particle size is obtained, such as within the average particle size range described above. During this process, additional electrosteric dispersants can be added as needed.
[0065] At the end of the process, residual product particles of the ground solid substrate remaining in the media can be transferred from the grinding chamber 16 to a collector 32 as a dispersion in a fluid carrier, optionally under pressure or with the aid of a pump 24. Substantially all of the grinding media remains in the grinding chamber 16, and the product substrate particles are separated as a dispersion in a fluid carrier substantially free of grinding media. The product substrate particles produced according to the present disclosure can have a diameter (D) of less than about one micron, e.g., less than about 800 nm or less than about 500 nm. 90 ) particle size. As is known in the art, the fluid carrier can be removed by drying or baking. In some embodiments, the electrosteric dispersant can remain in the ground product after drying, but in other embodiments, the electrosteric dispersant can be removed, for example, by baking in a kiln. The removal of the electrosteric dispersant will depend on the final product requirements and the intended application. In some embodiments, as further described below, a dispersion of particles of the ground solid substrate in a fluid carrier product can be spray dried (e.g., using high pressure air through a nozzle via a pump to form droplets, and then heating the droplets) to separate and produce nanoparticles as a dry powder.
[0066] Figure 3BAn alternative embodiment of a stirred media mill, namely a horizontal media mill, is presented. Figure 3B Many physical components of the implementation are similar to Figure 3A , because both implementations achieve the same functionality. However, in Figure 3B In the figures, with reference to the functions (A) to (E) described, the specific functions occurring in each area of the mill are noted. As described, at function (A), the energy input into the mill through the shaft is dissipated inside the suspension. At function (B), friction occurs in the suspension near the chamber wall of the agitator. At function (C), displacement occurs within the suspension during the approach of two or more pieces of grinding media toward each other. At function (D), the grinding media contact each other without causing stress to the suspended particles. In addition, at function (E), the grinding media may be temporarily deformed after contact.
[0067] Electrosteric Dispersant
[0068] More details are now provided regarding the electrosteric dispersants used in the wet media milling methods of the present disclosure. The electrosteric dispersants provide electrosteric stabilization to the product particles. Electrosteric stabilization is a combination of electrostatic and steric stabilization. Reference Figure 4 Electrosteric stabilization involves adsorption of charged polymers (polyelectrolytes) on the surface of the colloidal product particles. The surface of the particles typically contains negative sites as well as positive sites. For example, such charged sites may include functional groups including, but not limited to, OH - , H + , O 2 - and O - etc. The relative concentration of each charge depends on many factors, including the properties of the particle, the oxidation state of the particle, and the pH of the system.
[0069] Polyelectrolytes are related to their overall electrical properties (i.e., positive or negative). Polyelectrolytes are strongly adsorbed on the surface of particles by attaching themselves to oppositely charged potential points on the particle surface. However, during the adsorption process, all ionic sites on each polyelectrolyte are not used. Although some ionic sites are used to adsorb polyelectrolytes on the surface of particles, other ionic sites are in the polymer part that spreads freely (trail) in the liquid medium. The similar charges of the combination related to the polymer chain and the particle surface in the solution give each particle the overall negative or positive charge of the particle-polymer composition. Each polymer-coated particle can repel similar charges related to other polymer-coated particles because such particles experience electronic repulsion. This electronic repulsion, together with the steric effect of the polymer, disperses the product suspension. In addition, because both electrostatic and spatial separation are achieved, particle separation is significantly stronger than independent electrostatic or spatial separation, resulting in the need for less dispersant, and less stringent control requirements for the amount of the dispersant used in the grinding method.
[0070] Polyelectrolytes suitable for use as electrical spatial dispersants according to the present disclosure include functional polymers having a number average molecular weight of at least about 500 g / mol, such as at least about 1000 g / mol, such as at least about 2000 g / mol. In some embodiments, the functional polymer may have a number average molecular weight of up to about five million or even fifty million g / mol. However, typically, the number average molecular weight will be less than about 500,000 g / mol, such as less than about 100,000 g / mol, or less than about 50,000 g / mol, or less than about 25,000 g / mol. In particular, the polyelectrolyte dispersant may be selected from the following: polymers and copolymers with charged functional groups or inorganic affinity groups, alkylammonium salts of polymers and copolymers, polymers and copolymers with acidic groups, functionalized comb copolymers and block copolymers, modified acrylate block copolymers, modified polyurethanes, modified and / or salified polyamines, phosphoric acid polyesters, polyethoxylates, polymers and copolymers with fatty acid groups, modified polyacrylates such as transesterified polyacrylates, modified polyesters such as acid-functional polyesters, polyphospholipids and mixtures thereof. As non-limiting examples, suitable electrosteric dispersants are sold under the trade names: Disperbyk-199 and Disperbyk-2010 (BYK GmbH, Wessel, Germany) and Flexisperse 225 and Flexisperse 300 (ICT, Cartersville, Georgia, USA). In embodiments, the product suspension in the wet media mill may have an electrosteric dispersant content of about 2 wt % to about 20 wt %, e.g., about 2 wt % to about 15 wt %, or about 5 wt % to about 15 wt %, based on the weight of the solid particles.
[0071] Grinding method
[0072] refer to Figure 5 , illustrates a flow chart of a method 500 for producing nanoscale particles. The method 500 includes a premixing step 502, i.e., when a feed substrate suspension is premixed with a dispersant in a separate tank. The feed substrate suspension includes a liquid carrier medium and feed substrate particles. The liquid carrier medium may include water or an organic solvent. The feed substrate particles may include organic or inorganic solids, glass, graphene, metals, minerals, ores, silicon oxide, diatomaceous earth, clay, organic and inorganic pigments, pharmaceutical materials, or carbon black. The feed substrate particles may be present in the feed substrate suspension in an amount of about 5% to about 70% by weight of the feed substrate suspension, or in an amount of about 5% to about 40% by weight. The electrosteric dispersant may be added in an amount of about 2% to about 20% by weight of the feed substrate particles. The electrosteric dispersant includes a polyelectrolyte. The polyelectrolyte may include a polymer or copolymer having a charged functional group or an inorganic affinity group.
[0073] Method 500 also includes a step 504 of adding grinding / milling media to the mill, i.e., the mill is filled with an appropriate amount of grinding / milling media. Grinding media are typically selected from various dense and hard materials, such as sand, steel, silicon carbide, ceramics, zirconium silicate, zirconium and yttrium oxides (e.g., yttria-stabilized zirconium oxide), glass, aluminum oxide, titanium, and some polymers, such as cross-linked polystyrene and methyl methacrylate. Media geometry can vary depending on the application, although spherical spheres or column beads are often used. In some embodiments, grinding media can have a variety of sizes and size distributions, including large grinding media particles and smaller grinding media particles.
[0074] Method 500 also includes step 506 of adding the premixed feed substrate suspension from step 502 to the media mill. The feed suspension may be added in a batch or continuous process. A defoamer may also be optionally added. Further, method 500 includes step 508 of operating the media mill for a period of time to pulverize the feed substrate particles to form particles having a diameter (D) of less than about one micron, or less than about 800 nm, or less than about 500 nm, or less than about 400 nm. 90 ) particle size. The period of time may be from about 10 minutes to about 6000 minutes, or from about 10 minutes to about 3000 minutes, or from about 10 minutes to about 1000 minutes. Additional electrosteric dispersant may be added during a period of time while the media mill is running.
[0075] In addition, method 500 includes a step 510 of recycling for further grinding the nanoscale particles from the media mill. A portion of this step may also include removing the nanoscale particles from the media mill, which may include separating the nanoscale particles from the grinding media. Optionally, method 500 may include a step 512 of drying the nanoscale particles after removing the nanoscale particles from the media mill. Optionally, method 500 may include a step 514 of separating the electrosteric dispersant from the nanoscale particles using a kiln and removing any organic matter after removing the nanoscale particles from the media mill. It should be understood that the various steps in method 500 may be repeated one or more times throughout the operation of the method.
[0076] Energy storage materials
[0077] As described above, in some embodiments the method prepares nanoscale particles for electrochemical materials, i.e., materials suitable for use in or as components of electrochemical devices (e.g., batteries, supercapacitors, etc.). In certain embodiments, the nanoscale particles for electrochemical materials are particularly useful in or as energy storage materials such as electrodes (e.g., cathodes or anodes) for energy storage materials such as electrodes (e.g., cathodes or anodes). In such embodiments, an electrochemical feed substrate is used in the method to prepare a feed substrate suspension.
[0078] The electrochemical feed substrate is not particularly limited, and may be or include any granular material suitable for use in the methods of the embodiments described herein. More particularly, the electrochemical feed substrate may be any material suitable for use in the media mill of the present embodiment to prepare nanoscale particles, which may then be used to prepare components of an electrochemical device. For example, in some embodiments the electrochemical feed substrate comprises an energy storage material selected from anode active materials and cathode active materials (i.e., materials capable of having anode or cathode properties, respectively), as described in further detail below. However, it will be understood that the electrochemical feed substrate may also include materials suitable for preparing nanoparticles that can be utilized in components other than electrodes, such as separators, current collectors, or even multi-purpose composite materials.
[0079] Regarding suitable energy storage materials, those skilled in the art will readily appreciate that various precursor compounds may be employed in the preparation of the electrode, and that certain compounds and compositions may be used in the anode in some applications and in the cathode in other applications. Therefore, the specific materials described herein are not limited to specific end applications unless otherwise described. In general, suitable anode energy storage materials may be classified as follows: intercalated anode materials (e.g., graphite, lithium titanate), alloyed anode materials (e.g., silicon, tin, germanium, and antimony compounds), or conversion anode materials (e.g., transition metal oxides, sulfides, etc.). Examples of specific anode active materials suitable for use in the method therefore include carbon-based anode materials, such as those selected from graphite, graphene, activated carbon, pyrolytic carbon, hard carbon, and combinations thereof. Similarly, lithium titanate-based anode materials may also be utilized. Additional examples include alloyed anode-type materials, such as those comprising transition metal oxides, sulfides, nitrides, phosphides, fluorides, or combinations thereof. In yet another embodiment, the energy storage material may include a silicon-based anode material, a tin-based anode material, a germanium-based anode material, an antimony-based anode material, an aluminum-based anode material, a magnesium-based anode material, or any combination thereof.
[0080] The energy storage material may include a cathode active material. The cathode active material may be an inorganic cathode active material, an organic cathode active material, a polymer cathode active material, or a combination thereof.
[0081] Examples include cathode active materials selected from metal oxides, metal phosphates, metal silicides, metal selenides, transition metal sulfides, and combinations thereof. In general, suitable cathode energy storage materials can be classified as follows: layered structure type anode materials (e.g., graphite, lithium titanate), spinel structure type, alloy type anode materials (e.g., silicon, tin, germanium, and antimony compounds), or conversion type anode materials (e.g., transition metal oxides, sulfides, etc.). Polyanionic cathode compounds can also be used.
[0082] The energy storage material utilized in the method can be selected based on the particular type of energy storage device that is used / made from the nanoscale particles. 2 The battery (also known as lithium-air battery) can use the following cathode, which is carbon-based (such as activated carbon, carbon black, etc.) or includes precious metals (such as gold, silver and palladium), non-precious metals (such as Ni / Ru particles, graphene-based Co / Cu bimetallic nanoparticles, etc.), transition metal oxides (such as Fe 2 O 3 , Fe 3 O 4 、NiO、CuO、Co 3 O 4 etc.), and transition metal carbides (such as Mo 2C), sulfides, and nitrides; each of these can be used. Lithium-sulfur (Li–S) batteries typically use high-capacity sulfur (S, 1675 mAhg -1 ) cathode and lithium metal anode. In such a device, lithium polysulfide is adsorbed on metal oxides such as TiO 2 、MnO 2 , Nb 2 O 5 , Fe 3 O 4 However, lithium polysulfide adsorbs on metal sulfides such as Ni 3 S 2 、SnS 2 , FeS, CoS 2 VS 2 and TiS 2 On. Such two types of materials can be utilized in this embodiment. In sodium ion batteries, the anode material is typically selected from graphite, hard carbon, soft carbon, titanium oxide, sodium titanate, and transition metal oxides, sulfides, nitrides and phosphides of the general formula MaXb, where M is Fe, Co, Ni, Cu and / or Mn, and X is O, N, F, S, Se, P, or H. Other materials include those where X is Si, Ge, Sn, Sb, or Bi. Other materials include cathode materials for zinc ion batteries, such as those based on MnO 2 、MnO、Mn 2 O 3 , Mn 3 O 4 and ZMn 2 O 4 cathode materials; and for zinc-air batteries, transition metal oxides such as MnCo 2 O 4 、Co 3 O 4 / MnCo 2 O 4 、Co 3 O 4 、NiCo 2 O 4 , or Fe 3 O 4 Similarly, V 2 O 5 and derivatives.
[0083] Returning to the method itself, refer to Figure 7 To illustrate the method of this embodiment. In particular, Figure 7A flow chart of a method at 600 is shown, which is a method for preparing nanoscale particles. The method 600 includes a premixing step 602, i.e., when a feed substrate suspension (i.e., electrochemical feed substrate particles) is premixed with a dispersant in a separate tank. The electrochemical feed substrate suspension includes a liquid carrier medium and feed substrate particles. The liquid carrier medium may include water or an organic solvent. The electrochemical feed substrate particles typically include one of the energy storage materials described above, or another compound for electrochemical use.
[0084] The method 600 also includes a step 604 of adding grinding / milling media to the mill, as described above. In some embodiments, the grinding media can have a variety of sizes and size distributions, including large grinding media particles and smaller grinding media particles. The method 600 also includes a step 606 of adding the premixed feed substrate suspension from step 602 to the media mill. The feed suspension can be added in a batch or continuous process. A defoaming agent can also be optionally added. Further, the method 600 includes the step 608 of operating the media mill for a period of time to comminute the feed substrate particles to form (e.g., having a diameter of less than about one micron, or less than about 800 nm, or less than about 500 nm, or less than about 400 nm) a feed substrate suspension having a diameter of less than about one micron, or less than about 800 nm, or less than about 500 nm, or less than about 400 nm. 90 ) particle size). Although not shown, method 600 typically includes a step of recycling the ground / unground feed substrate from the media mill, for example, for further grinding to achieve nanoscale particles. Part of this step may also include removing the nanoscale particles from the media mill, and may include separating the nanoscale particles from the grinding media, as in other embodiments described herein.
[0085] In some embodiments, method 600 includes a step 610 of drying the nano-sized particles after removing the nano-sized particles from the media mill. Typically, step 610 is performed by spray drying. For example, in some embodiments, the slurry obtained after the drinking process is pumped through a nozzle using high pressure air, which atomizes the liquid slurry into fine droplets. The droplets then pass through a heating chamber, where the liquid (e.g., evaporates and forms a dry powder. The dry powder is then pneumatically transported and collected in a cyclone separator and / or a bag filter. It will be understood that step 610 can be performed directly in sequence with step 608, i.e., the wet slurry containing the nano-sized particles now can be introduced into the spray dryer immediately after the grinding is completed.
[0086] Although not shown, it is understood that the method may include separating the electrosteric dispersant from the nanoparticles and removing any organic matter after removing the nanoparticles from the media mill. It is understood that each step in method 600 may be repeated one or more times throughout the run of the method.
[0087] The nanoscale particles prepared by the method can be used to prepare electrochemical materials. In this way, the electrochemical feed substrate can be considered as a precursor or intermediate for preparing one or more electrochemical materials. For example, in some embodiments, the nanoscale particles are used to prepare electrodes.
[0088] It has recently been shown that by reducing the solid electrolyte particle size and increasing the cathode active material particle size, cathode active material loadings of more than 50% by volume with high cathode utilization can be experimentally achieved, indicating that commercially relevant energy-intensive cathode composites can be obtained by simple mixing and pressing methods. It has also been shown that by using large cathode particles (≈12 μm) and small SE particles (≈1.5 μm), solid cathode composites with liquid-cell-level cathode volume loadings (≈50% by volume) can be prepared. In view of these observations, it will be understood that particle size optimization in the electrode can achieve commercially relevant cathode loadings. In addition, the nanoscale particles of the present embodiment can be easily pressed into electrodes (e.g., energy storage materials) by methods known to those skilled in the art. Example
[0089] The disclosure is now described by the following non-limiting examples. It should be noted that the following examples and methods are applicable to various changes and modifications without departing from the scope of the invention as defined by the appended claims. Therefore, it should be noted that the following examples should be interpreted as being illustrative only and not limiting in any way.
[0090] Examples 1-5: Preparation of Nanoparticles
[0091] Five different Example particle suspensions were prepared, which included water (as liquid medium), crystalline silica / quartz particles or diatomaceous earth particles (as solid substrate), defoamer and various types and amounts of polyelectrolytes (as electrosteric dispersants). The composition of each Example slurry is presented below in Table 1.
[0092] Table 1
[0093]
[0094] (1) Feed size measured using a laser particle analyzer (Microtrac S3500; available from Microtrac Retsch GmbH, Hahn, Germany)
[0095] (2) Flexisperse 225 available from Innovative Chemical Technologies (Cartersville, Georgia, USA)
[0096] (3) Di sperbyk 199 available from BYK-Chemie GmbH (Wesel, Germany)
[0097] (4) No defoaming agent is used
[0098] Each of the example particle suspensions was placed in a circulating stirred media mill (VMA Dispermat SL12, available from VMA-GETZMANN GmbH (Reichshof, Germany)) that also included yttria-stabilized zirconia (YSZ) beads as grinding media. Each example was subjected to wet media grinding in the stirred media mill for a period of time ranging from about 150 minutes to about 1000 minutes. After the grinding was completed, the D of the product particles was measured using a nanoparticle analyzer (Anton-Paar Litesizer 500 (available from Anton Paar GmbH, Graz, Austria)). 10 , D 50 and D 90 Average particle size. Figures 6A-6E The average particle size of each of Examples 1-5 as a function of milling time is presented in FIG. As shown in those figures, the process according to the present disclosure can easily achieve a D of about 100 nm to about 200 nm. 10 Average particle size, D of about 150 to about 250 nm 50 The average particle size and D of about 250nm to about 350nm 90 Average particle size.
[0099] Thus, the present disclosure provides embodiments of methods and apparatus for producing nanoscale particles using electrosterically stabilized slurries in a media mill. The method and apparatus advantageously maintain particle separation when the particle size is reduced to less than about 1 micron, thereby avoiding agglomeration and mill screen clogging. In addition, the method and apparatus are advantageously suitable for industrial scale manufacturing to the extent that no additives need to be strictly controlled to prevent flocculation or a sharp increase in viscosity of the product suspension.
[0100] General procedure for the preparation of nanoscale particles for energy storage devices
[0101] In preparing nano-sized particles, feed materials (e.g., quartz, diatomaceous earth, etc.) are combined with a solvent (e.g., water) along with a dispersant (e.g., Flexisperse 225 from ICT Chemicals) in a tank for 30 to 60 minutes. The resulting mixture is in the form of a liquid, slurry containing water and solids.
[0102] The slurry is then continuously recirculated through the stirred media mill for a specified amount of time. Grinding media (Y-ZrO 2Ceramic particles, with a size range of 0.05 mm-10 mm). Only one size of media was used during the test run. For example, in the test run, a 0.1 mm media size was loaded into the mill chamber. Mixtures of media sizes are not typically used in stirred media grinding processes. The grinding time is determined by the total amount of mill power input to the grinding process.
[0103] After the grinding process is complete, the slurry is pumped through a nozzle with high pressure air. The high pressure air atomizes the liquid slurry into fine droplets. These droplets then pass through a heater chamber where the liquid evaporates and forms a dry powder. The dry powder is then pneumatically transported and collected in a cyclone separator and / or bag filter.
[0104] Examples 6-7: Preparation of Nanoparticles
[0105] Example 6: 35 kg of a granular material having an initial particle size of D was placed in a tank. 90 =5 μm Minus i 1-5 (crystalline quartz) was mixed in 35 kg of water and 2.1 kg of Flexisperse 225 for 30 minutes. The mill was a Netzsch NEOS10 (which was a 10 L mill chamber) and was loaded with 27.83 kg of Y-Zr ceramic media with a size of 0.3 mm. The resulting slurry was then circulated through the mill for a total of 1380 minutes, consuming a total of 571 kWh of input electrical energy in the process. Fig. 8A SEM micrographs of feed material Minus i 1-5 are provided.
[0106] Example 7: 25 kg of a granular material having an initial particle size of D 90 = 75 μm Si lcos i l-75 (crystalline quartz) was mixed in 25 kg of water and 1.25 kg of Flexisperse 225 for 12 hours. The mill was a Netzsch NEOS10 (which was a 10L mill chamber) and was filled with 27.83 kg of Y-Zr ceramic media with a size of 0.3 mm. The slurry was then circulated through the mill for a total of 960 minutes, consuming a total of 404 kWh of input electrical energy in the process. Figure 8B SEM micrographs of feed material Si lcos i 1-75 are provided.
[0107] Fig. 9 SEM micrographs of spray-dried agglomerates of the nanoscale particles prepared in Examples 6 - 7 are provided. These round agglomerates have a particle size ranging from 5 μm to 50 μm and consist of primary nanoparticles. Figures 10A-10E Agglomerates are shown to contain primary nanoparticles. These nanoparticles have a diameter of about 100 nm to 200 nm.
[0108] It was found that the current method can easily grind 75 μm crystalline quartz to 100 nm. Because quartz is an extremely hard material and is often difficult to process, many battery precursor materials (which are typically known to be softer materials) can also be ground using the technology of this embodiment. Therefore, the method provides a convenient way to prepare electrochemical materials, such as battery precursors, even from difficult-to-process materials.
[0109] Although at least one exemplary embodiment is presented in the foregoing detailed description, it should be understood that there are a large number of variations. It should also be understood that the exemplary embodiments are only examples and are not intended to limit the scope, applicability or configuration of the invention in any way. On the contrary, the foregoing detailed description will provide a conventional roadmap for implementing the exemplary embodiments of the method and apparatus of the present invention to those skilled in the art. It should be understood that various changes can be made in the function and arrangement of the elements described in the exemplary embodiments without departing from the scope of the invention set forth in the appended claims.
Claims
1. A method for preparing nanoscale particles of electrochemical materials, include: adding a feed substrate suspension to a media mill, wherein the feed substrate suspension comprises a liquid carrier medium and electrochemical feed substrate particles; adding an electrosteric dispersant to the feed substrate suspension in the media mill, wherein the electrosteric dispersant comprises a polyelectrolyte; The media mill is operated for a period of time to comminute the electrochemical feed substrate particles to form a particle size (D) less than about one micron. 90 ) nanometer-scale particles of particle size; and Recirculation is used to further grind the nano-sized particles from the media mill.
2. The method of claim 1, wherein the liquid carrier medium comprises water or an organic solvent.
3. The method of claim 1, wherein the electrochemical feed substrate comprises an energy storage material selected from the group consisting of an anode active material and a cathode active material.
4. The method of claim 3, wherein the energy storage material comprises: (i) an intercalation-type anode material; (ii) an alloy-type anode material; (iii) a conversion-type anode material; or (iv) any combination of (i)-(iii).
5. The method of claim 3, wherein the energy storage material comprises: (i) a carbon-based anode material selected from graphite, graphene, activated carbon, pyrolytic carbon, hard carbon, and combinations thereof; (ii) a lithium titanate-based anode material; or (iii) both (i) and (ii).
6. The method of claim 3, wherein the energy storage material comprises an alloyed anode material comprising a transition metal oxide, sulfide, nitride, phosphide, fluoride, or a combination thereof.
7. The method of claim 3, wherein the energy storage material comprises: (i) a silicon-based anode material; (ii) a tin-based anode material; (iii) a germanium-based anode material; (iv) an antimony-based anode material; (v) an aluminum-based anode material; (vi) a magnesium-based anode material, or (vii) any combination of (i)-(vi).
8. The method of claim 3, wherein the energy storage material comprises an inorganic cathode active material, an organic cathode active material, a polymer cathode active material, or a combination thereof.
9. The method of claim 3, wherein the energy storage material comprises a cathode active material selected from the group consisting of metal oxides, metal phosphates, metal silicides, metal selenides, transition metal sulfides, and combinations thereof. 10 . The method according to claim 9 , wherein the cathode active material comprises a layered structure type cathode compound, a spinel structure type cathode compound, an olivine type cathode compound, a polyanion cathode compound, or a combination thereof.
11. The method of claim 1, wherein the electrochemical feed substrate comprises a separator material comprising an inorganic ceramic.
12. The method of claim 1, wherein the polyelectrolyte of the electrosteric dispersant comprises a polymer or copolymer having a charged functional group or an inorganic affinity group.
13. The method of claim 1, wherein the feed substrate suspension comprises: (i) about 5 wt % to about 70 wt % electrochemical feed substrate particles; (iii) about 2 to about 20 wt % electrosteric dispersant; or (iii) both (i) and (ii), based on the total weight of the feed substrate suspension.
14. The method according to claim 1, in: (i) the time period is from about 10 to about 6000 minutes; (ii) the nanoscale particles have a diameter (D) less than about 500 nm. 90 ) particle size; or (iii) both (i) and (ii).
15. The method of claim 1, wherein the media mill contains grinding media, and wherein recycling for further grinding the nanoscale particles from the media mill further comprises separating the nanoscale particles from the grinding media.
16. The method according to claim 15, in: (i) the grinding media comprises one or more of sand, steel, silicon carbide, ceramic, zirconium silicate, zirconium and yttrium oxides, glass, aluminum oxide, titanium, cross-linked polystyrene and methyl methacrylate; (ii) the grinding media is provided in the shape of one or more of spheres, beads and pillars; or (iii) both (i) and (ii).
17. The method of claim 1, further comprising drying the nanoscale particles from the media mill after recycling for further grinding.
18. The method of claim 17, wherein drying the nanoscale particles is performed by spray drying.
19. The method of claim 18, wherein further grinding the nanoscale particles from the media mill produces a slurry, and wherein the slurry is directly spray dried to produce the nanoscale particles as a dry powder.
20. An electrode comprising nano-sized particles prepared according to the method of claim 1.