Adsorption material for preparing wafer from semiconductor as well as preparation method and application of adsorption material
By forming a specific film on a polypropylene adsorption substrate, adsorption materials such as γ-aminopropyltriethoxysilane are used to solve the problem of chip loss of polypropylene meltblown materials in semiconductor preparation, and the adsorption performance is improved. Wafer yield.
Patent Information
- Application Number
- CN202410922898.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
AI Technical Summary
Polypropylene meltblown materials are prone to chip loss during semiconductor wafer preparation, resulting in a decrease in cleanliness and a decrease in wafer yield.
The combination of polypropylene adsorption substrate and a specific film consisting of γ-aminopropyltriethoxysilane, ammonium persulfate, isopropyl alcohol, polyvinyl alcohol and anhydrous ethanol, and is prepared by spraying and drying to form Adsorbent material with a thickness of 0.03 to 0.07mm is used to adsorb strong acids, strong alkalis and particulate matter.
Effectively control chip loss, improve the yield rate of semiconductor workshops, enhance adsorption performance, and make up for the shortcomings of existing polypropylene adsorption materials.
Smart Images

Figure CN118874431A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of adsorption materials, and in particular to an adsorption material for semiconductor wafer preparation, a preparation method and application thereof. Background Art
[0002] Polypropylene meltblown material is an important nonwoven fabric material. It is made of polypropylene as the main raw material through meltblown fiber technology. There are several main methods for its preparation: 1) Hydrogenation control method: The melt index (M) of PP is adjusted by adjusting the amount of hydrogenation during the polymerization process, but this method is not widely used. 2) Degradation method: Add peroxide degradation agent to conventional PP material for controllable chemical degradation, reduce the relative molecular weight, and obtain PP material with a higher melt index. This is the main method for producing special PP materials for meltblowing in China. 3) Metallocene catalyst direct polymerization method: The metallocene catalyst system has the characteristics of high activity and single active center, and can directly prepare high-fluidity PP in the reactor. This PP has low volatility, low molding temperature, and narrow and uniform relative molecular weight distribution, which is very suitable for the production of meltblown nonwoven fabrics. 4) Post-addition controllable degradation agent method: For example, the IRGATEC CR76 new meltblown special controllable degradation agent developed by Ciba Fine Chemicals is different from the peroxide degradation agent. This degradation agent is actually a PP masterbatch containing hindered amine esters with hydroxyl groups. Polypropylene meltblown material has good mechanical properties, high heat resistance and chemical stability. It can be used as packaging material, filtration and adsorption material, etc. and has a wide range of uses.
[0003] In the process of preparing semiconductor wafers, etching is an important step, in which strong acids and alkalis such as concentrated sulfuric acid and high-concentration sodium hydroxide are used to remove unwanted parts of the material. In order to deal with the strong acid and alkali waste liquid generated during the etching process, polypropylene melt-blown material adsorption cotton, pillows, strips, etc. are widely used in the market. However, these melt-blown materials have the following main problems in application:
[0004] Problem 1: Meltblown materials are prone to chipping; due to its unique structure and manufacturing process, polypropylene meltblown materials are prone to produce fine fibers or particles during use, the so-called "chipping". These dropped fibers or particles will not only reduce the cleanliness of the wafer processing plant, but may also directly adhere to the wafer surface, affecting the performance and yield of the wafer.
[0005] Problem 2: Reduced cleanliness leads to reduced wafer yield; wafer manufacturing has extremely high requirements for environmental cleanliness, and any tiny impurities may have a significant impact on the performance of the wafer. When polypropylene melt-blown materials produce chips, these tiny fibers or particles will spread in the factory and pollute the processing environment. This not only increases the difficulty and cost of cleaning, but more importantly, these impurities may adhere to the surface of the wafer, causing defects or performance degradation of the wafer, thereby reducing the wafer yield. Summary of the invention
[0006] In order to solve the above problems, the present invention provides an adsorption material for semiconductor wafer preparation, a preparation method and application thereof.
[0007] In a first aspect, the present invention provides an adsorption material for semiconductor wafer preparation, the adsorption material comprising a polypropylene adsorption substrate and a film attached to the surface of the polypropylene adsorption substrate, the raw materials for preparing the film comprising a first solution and a second solution;
[0008] The first solution comprises the following components: γ-aminopropyltriethoxysilane, ammonium persulfate and isopropyl alcohol;
[0009] The second solution comprises the following components: polyvinyl alcohol and anhydrous ethanol.
[0010] Furthermore, the polypropylene-based adsorption substrate includes at least one of polypropylene meltblown fabric and polypropylene spunbond fabric.
[0011] Furthermore, the first solution comprises the following components in weight percentage:
[0012] Gamma-aminopropyltriethoxysilane 2%-5%, ammonium persulfate 2%-5% and isopropyl alcohol 90%-96%.
[0013] Further, the second solution comprises the following components in weight percentage:
[0014] Polyvinyl alcohol 2%-5% and anhydrous ethanol 95%-98%.
[0015] Furthermore, the thickness of the film is 0.03-0.07 mm.
[0016] In a second aspect, the present invention provides a method for preparing an adsorption material for semiconductor wafer preparation according to any one of the first aspects, the preparation method comprising the following steps:
[0017] Spraying the first solution onto the surface of the polypropylene-based adsorption substrate, and then performing a first drying to obtain an adsorption material intermediate;
[0018] The second solution is sprayed on the surface of the adsorption material intermediate, and then a second drying is performed to obtain the adsorption material.
[0019] Furthermore, the spraying amount of the first solution is 0.03-0.07 L / m 2 The spraying amount of the second solution is 0.03~0.07L / m 2 .
[0020] Furthermore, the first drying step includes the following process: entering into an infrared drying device at 60-80° C. for 180-240 seconds; and the second drying method is air drying and curing.
[0021] In a third aspect, the present invention provides the use of the adsorption material for semiconductor manufacturing wafers as described in any one of the first aspect and the second aspect for adsorbing strong acids, strong bases and particulate matter during the etching process of semiconductor manufacturing wafers.
[0022] The above technical solution provided by the embodiment of the present invention has at least the following advantages compared with the prior art:
[0023] An embodiment of the present invention provides an adsorption material for semiconductor wafer preparation. The adsorption material provided by the present invention forms a specific film on a polypropylene adsorption substrate, which can not only effectively adsorb strong acids, strong alkalis and particulate matter in the semiconductor wafer etching process, but also effectively control chip shedding, thereby improving the yield rate of semiconductor workshops, and making up for the shortcomings of existing polypropylene adsorption materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0026] Figure 1 A flow chart of a method for preparing an adsorption material for semiconductor wafer preparation provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0029] In a first aspect, the present invention provides an adsorption material for semiconductor wafer preparation, the adsorption material comprising a polypropylene adsorption substrate and a film attached to the surface of the polypropylene adsorption substrate, the raw materials for preparing the film comprising a first solution and a second solution;
[0030] The first solution comprises the following components: γ-aminopropyltriethoxysilane, ammonium persulfate and isopropyl alcohol;
[0031] The second solution comprises the following components: polyvinyl alcohol and anhydrous ethanol.
[0032] An embodiment of the present invention provides an adsorption material for semiconductor wafer preparation. The adsorption material provided by the present invention forms a specific film on a polypropylene adsorption substrate, which can not only effectively adsorb strong acids, strong alkalis and particulate matter in the semiconductor wafer etching process, but also effectively control chip shedding, thereby improving the yield rate of semiconductor workshops, and making up for the shortcomings of existing polypropylene adsorption materials.
[0033] In some specific embodiments, the polypropylene-based adsorption substrate includes at least one of a polypropylene meltblown fabric and a polypropylene spunbond fabric.
[0034] In some specific embodiments, the first solution comprises the following components by weight percentage:
[0035] Gamma-aminopropyltriethoxysilane 2%-5%, ammonium persulfate 2%-5% and isopropyl alcohol 90%-96%.
[0036] In some specific embodiments, the second solution comprises the following components by weight percentage:
[0037] Polyvinyl alcohol 2%-5% and anhydrous ethanol 95%-98%.
[0038] In some specific embodiments, the film has a thickness of 0.03-0.07 mm.
[0039] In a second aspect, the present invention provides a method for preparing an adsorption material for semiconductor wafer preparation according to any one of the first aspects, such as Figure 1 As shown, the preparation method comprises the following steps:
[0040] Spraying the first solution onto the surface of the polypropylene-based adsorption substrate, and then performing a first drying to obtain an adsorption material intermediate;
[0041] The second solution is sprayed on the surface of the adsorption material intermediate, and then a second drying is performed to obtain the adsorption material.
[0042] In some specific embodiments, the spraying amount of the first solution is 0.03-0.07 L / m 2 The spraying amount of the second solution is 0.03~0.07L / m 2 .
[0043] In some specific embodiments, the first drying step includes the following process: entering into an infrared drying device at 55-80° C. for 120-18 seconds; the second drying method is air drying and curing.
[0044] In a third aspect, the present invention provides the use of the adsorption material for semiconductor manufacturing wafers as described in any one of the first aspect and the second aspect for adsorbing strong acids, strong bases and particulate matter during the etching process of semiconductor manufacturing wafers.
[0045] It should be noted that the components and raw materials involved in the adsorption material for semiconductor wafer preparation and its preparation method and application provided in the embodiment of the present invention, if there is no special limitation or description, can be directly commercially available products or homemade according to the existing preparation process, such as polypropylene meltblown cloth and polypropylene spunbond cloth. At the same time, the operation steps involved, if there is no specific description, can be carried out with reference to the existing technology or with existing equipment; for example, the spraying in the preparation method can be carried out with the existing conventional spraying device, and the present invention document will not repeat them one by one.
[0046] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0047] Example 1
[0048] This example provides an adsorption material for semiconductor wafer preparation, the adsorption material includes a polypropylene adsorption substrate and a film attached to the surface of the polypropylene adsorption substrate, and the raw materials for preparing the film include a first solution and a second solution;
[0049] The polypropylene-based adsorption substrate is a polypropylene meltblown cloth;
[0050] In percentage by weight, the first solution comprises the following components:
[0051] γ-aminopropyltriethoxysilane 3.5%, ammonium persulfate 3% and isopropyl alcohol 93.5%;
[0052] In weight percentage, the second solution comprises the following components:
[0053] Polyvinyl alcohol 3% and anhydrous ethanol 97%.
[0054] The method for preparing the above-mentioned adsorption material for semiconductor wafer preparation comprises the following steps:
[0055] Spraying the first solution onto the surface of the polypropylene-based adsorption substrate, and then performing a first drying to obtain an adsorption material intermediate;
[0056] Spraying the second solution on the surface of the adsorption material intermediate, and then performing a second drying to obtain the adsorption material;
[0057] Wherein, the spraying volume of the first solution is 0.05L / m 2 The spraying amount of the second solution is 0.07L / m 2 .
[0058] The first drying step includes the following processes: drying in an infrared drying device at 60° C. for 120 seconds; and the second drying method is air drying and curing.
[0059] Example 2
[0060] This example provides an adsorption material for semiconductor wafer preparation, the adsorption material includes a polypropylene adsorption substrate and a film attached to the surface of the polypropylene adsorption substrate, and the raw materials for preparing the film include a first solution and a second solution;
[0061] The polypropylene-based adsorption substrate is a polypropylene meltblown cloth;
[0062] In percentage by weight, the first solution comprises the following components:
[0063] γ-aminopropyltriethoxysilane 2%, ammonium persulfate 2% and isopropyl alcohol 96%;
[0064] In weight percentage, the second solution comprises the following components:
[0065] Polyvinyl alcohol 2% and anhydrous ethanol 98%.
[0066] The method for preparing the above-mentioned adsorption material for semiconductor wafer preparation comprises the following steps:
[0067] Spraying the first solution onto the surface of the polypropylene-based adsorption substrate, and then performing a first drying to obtain an adsorption material intermediate;
[0068] Spraying the second solution on the surface of the adsorption material intermediate, and then performing a second drying to obtain the adsorption material;
[0069] Wherein, the spraying volume of the first solution is 0.05L / m 2 The spraying amount of the second solution is 0.07L / m 2 .
[0070] The first drying step includes the following processes: drying in an infrared drying device at 60° C. for 120 seconds; and the second drying method is air drying and curing.
[0071] Example 3
[0072] This example provides an adsorption material for semiconductor wafer preparation, the adsorption material includes a polypropylene adsorption substrate and a film attached to the surface of the polypropylene adsorption substrate, and the raw materials for preparing the film include a first solution and a second solution;
[0073] The polypropylene-based adsorption substrate is a polypropylene meltblown cloth;
[0074] In percentage by weight, the first solution comprises the following components:
[0075] γ-aminopropyltriethoxysilane 5%, ammonium persulfate 5% and isopropyl alcohol 90%;
[0076] In weight percentage, the second solution comprises the following components:
[0077] Polyvinyl alcohol 5% and anhydrous ethanol 95%.
[0078] The method for preparing the above-mentioned adsorption material for semiconductor wafer preparation comprises the following steps:
[0079] Spraying the first solution onto the surface of the polypropylene-based adsorption substrate, and then performing a first drying to obtain an adsorption material intermediate;
[0080] Spraying the second solution on the surface of the adsorption material intermediate, and then performing a second drying to obtain the adsorption material;
[0081] Wherein, the spraying volume of the first solution is 0.05L / m 2 The spraying amount of the second solution is 0.07L / m 2 .
[0082] The first drying step includes the following processes: drying in an infrared drying device at 60° C. for 120 seconds; and the second drying method is air drying and curing.
[0083] Comparative Example 1
[0084] This example provides an adsorption material for semiconductor wafer preparation and a preparation method thereof, which is different from Example 1 only in that the amount of γ-aminopropyltriethoxysilane is 7%, and the amount of isopropanol is 90% (i.e., the amount of γ-aminopropyltriethoxysilane is too much and the amount of isopropanol is reduced accordingly); the remaining steps and parameters are the same.
[0085] Comparative Example 2
[0086] This example provides an adsorption material for semiconductor wafer preparation and a preparation method thereof, which is different from Example 1 only in that the amount of γ-aminopropyltriethoxysilane is 1%, and the amount of isopropanol is 94.5% (i.e., the amount of γ-aminopropyltriethoxysilane is too little and the amount of isopropanol is increased accordingly); the remaining steps and parameters are the same.
[0087] Comparative Example 3
[0088] This example provides an adsorption material and a preparation method for semiconductor wafer preparation. The only difference from Example 1 is that the amount of polyvinyl alcohol is 7%, and the amount of anhydrous ethanol is 93% (that is, the amount of polyvinyl alcohol is too much and the amount of anhydrous ethanol is reduced accordingly); the remaining steps and parameters are the same.
[0089] Comparative Example 4
[0090] This example provides an adsorption material and a preparation method for semiconductor wafer preparation. The only difference from Example 1 is that the amount of polyvinyl alcohol is 0.5%, and the amount of anhydrous ethanol is 99.5% (that is, the amount of polyvinyl alcohol is too little and the amount of anhydrous ethanol is increased accordingly); the remaining steps and parameters are the same.
[0091] Test Case
[0092] In this example, the adsorption materials obtained from the above embodiments and comparative examples (as test samples) and untreated polypropylene meltblown cloth (as basic control) are used in the chip wafer synthesis process of a thousand-level factory to adsorb strong acids and alkalis. Before applying the adsorption material, the detected particles were: 4910 at 0.3 microns, 10237 at 0.5 microns, 17867 at 1 micron, 4934 at 3 microns, 1450 at 5 microns, and 676 at 10 microns; the total number of particles was N1; the total number of particles after applying the above adsorption materials was N2. According to formula 1: adsorption rate (%) = (N1-N2) / N1×100%, the adsorption performance of each adsorption material is calculated; and according to formula 2: adsorption performance improvement value (%) = test sample adsorption rate - basic control adsorption rate. The test results are shown in Table 1. In addition, observe whether "chipping" occurs during use, and the results are shown in Table 2.
[0093] Table 1
[0094] Test samples Adsorption rate (%) Adsorption performance improvement value (%) Polypropylene meltblown cloth 13.15 - Example 1 90.04 85.4 Example 2 88.12 85.1 Example 3 93.18 85.9 Comparative Example 1 91.16 85.6 Comparative Example 2 79.82 83.5 Comparative Example 3 95.88 86.3 Comparative Example 4 89.15 85.2
[0095] Table 2
[0096] Test samples Whether there is "chipping" Polypropylene meltblown cloth "Cut off" is very serious Example 1 Very little "chipping" Example 2 Very little "chipping" Example 3 Very little "chipping" Comparative Example 1 Very little "chipping" Comparative Example 2 A small amount of "chipping" Comparative Example 3 Very little "chipping" Comparative Example 4 Very little "chipping"
[0097] It can be seen from Tables 1 and 2 above that the adsorption material provided by the present invention forms a specific film on a polypropylene adsorption substrate, which can not only effectively adsorb strong acids, strong bases and particulate matter in the semiconductor wafer etching process, but also effectively control chip shedding, thereby improving the yield rate of semiconductor workshops, and making up for the shortcomings of existing polypropylene adsorption materials.
[0098] Various embodiments of the present invention may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0099] In the present invention, in the absence of contrary instructions, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the specification of the present invention, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or plural, respectively.
[0100] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.
Claims
1. An adsorption material for semiconductor wafer preparation, characterized in that: The adsorption material includes a polypropylene adsorption substrate and a film attached to the surface of the polypropylene adsorption substrate, and the raw materials for preparing the film include a first solution and a second solution; The first solution comprises the following components: γ-aminopropyltriethoxysilane, ammonium persulfate and isopropyl alcohol; The second solution comprises the following components: polyvinyl alcohol and anhydrous ethanol.
2. The adsorption material for semiconductor wafer preparation according to claim 1, characterized in that: The polypropylene-based adsorption substrate includes at least one of a polypropylene meltblown fabric and a polypropylene spunbond fabric.
3. The adsorption material for semiconductor wafer preparation according to claim 1, characterized in that: In percentage by weight, the first solution comprises the following components: Gamma-aminopropyltriethoxysilane 2%-5%, ammonium persulfate 2%-5% and isopropyl alcohol 90%-96%.
4. The adsorption material for semiconductor wafer preparation according to claim 1, characterized in that: In weight percentage, the second solution comprises the following components: Polyvinyl alcohol 2%-5% and anhydrous ethanol 95%-98%.
5. The adsorption material for semiconductor wafer preparation according to claim 1, characterized in that: The thickness of the film is 0.03-0.07 mm.
6. A method for preparing an adsorption material for semiconductor wafer preparation according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: Spraying the first solution onto the surface of the polypropylene-based adsorption substrate, and then performing a first drying to obtain an adsorption material intermediate; The second solution is sprayed on the surface of the adsorption material intermediate, and then a second drying is performed to obtain the adsorption material.
7. The method for preparing an adsorption material for semiconductor wafer preparation according to claim 6, characterized in that: The spraying amount of the first solution is 0.03-0.07 L / m 2 The spraying amount of the second solution is 0.03-0.07 L / m 2 .
8. The method for preparing an adsorption material for semiconductor wafer preparation according to claim 6, characterized in that: The first drying step includes the following process: Enter into the infrared drying device at 55-80°C and bake for 120-180 seconds; the second drying method is air drying and curing.
9. Use of the adsorption material for semiconductor manufacturing wafers according to any one of claims 1 to 8 for adsorbing strong acids, strong bases and particulate matter during the etching process of semiconductor manufacturing wafers.