High-olefin-selectivity C5-C10 alkane dehydrogenation catalyst as well as preparation method and application thereof
Through the method of coupling Pt catalyst with metal oxides supported by ZSM-5 molecular sieve, the problem of insufficient selectivity and stability of long-chain olefins in naphtha in the prior art is solved, and a catalyst with high selectivity and long-life life is achieved. The product selectivity of α-olefins and β-olefins is significantly improved.
Patent Information
- Application Number
- CN202411019186.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-29
AI Technical Summary
Existing catalysts are difficult to achieve high selectivity and stability dehydrogenation in naphtha to prepare long-chain α-olefins, and there are thermodynamic equilibrium limitations and side reaction problems, resulting in low selectivity of α-olefins and β-olefins and catalyst life. short.
The method of coupling the Pt catalyst with metal oxides by ZSM-5 molecular sieve-supported Pt catalyst is adopted. Through exchange treatment, recrystallization and calcination, the dispersion and stability of Pt are improved, combined with the synergistic effect of metal oxides, and the alkane dehydrogenation reaction is promoted. Reduce side effects.
High selective dehydrogenation of C5-C10 alkanes in naphtha was achieved, the catalyst life was more than 500 hours, and the selectivity of α-olefins and β-olefins reached 99%, which significantly improved the activity and stability of the catalyst.
Smart Images

Figure CN118874528A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalysts, and in particular to a high olefin selectivity C5-C10 alkane dehydrogenation catalyst, and a preparation method and application thereof. Background Art
[0002] Naphtha is a mixed liquid containing a variety of chemical raw materials, among which C5~C 10 Alkanes account for more than 55%. At present, they are mainly converted into basic chemicals such as olefins and aromatics through steam cracking and catalytic reforming. However, my country has not yet formed independent intellectual property rights for high-selectivity and high-stability catalysts for direct dehydrogenation of naphtha to produce long-chain α-olefins, and the research and development of such catalysts is basically blank.
[0003] At present, Pt-Sn / γ-Al2O3 with Al2O3 as carrier and Pt as active center is more common as industrial dehydrogenation catalyst. However, Pt-Sn / γ-Al2O3 is difficult to break through thermodynamic limitations as an industrial dehydrogenation catalyst, and the selectivity of α-olefins and β-olefins is low, and the stability is also poor. In addition, during the use of the catalyst, many parallel and series side reactions are involved, such as cracking, secondary dehydrogenation, isomerization and cyclization reactions, which will also reduce the selectivity of α-olefins and β-olefins and the life of the catalyst. Prucker et al. found that in the dehydrogenation reaction of n-octane on the Pt-Sn-K / Al2O3 catalyst, although the 1-octene content (~7%) was slightly increased compared with the thermodynamic equilibrium data, the distribution of olefin products still followed the thermodynamic equilibrium, and the selectivity of 2-, 3- and 4-olefins accounted for more than 90% of the olefins. It can be seen that although the presence of Pt greatly promotes the breaking of CH bonds and provides the possibility for the preparation of long-chain α-olefins, the above-mentioned catalysts are difficult to break through thermodynamic equilibrium and obtain highly selective α-olefins (Prucker, T., et al., Kinetics of dehydrogenation of n-octane a promoted Pt-catalyst. Chemical Engineering Journal, 2022.442.).
[0004] He Songbo disclosed a Pt-Sn-K / γ-Al2O3 catalyst, which was modified by using an additive K. The modified catalyst was used to catalyze C 16Although the selectivity of alkane dehydrogenation to monoolefins has been improved, the stability of the catalyst is poor, the service life is short, and the deactivation rate is 15% in 24 hours (He Songbo, Bi Wenjun, Lai Yulong, et al. Effect of K additive on dehydrogenation of C16 normal alkane over Pt-Sn-K / γ-Al2O3 catalyst [J]. Journal of Fuel Chemistry, 2010, 038(004): 452-457). One of the difficulties in achieving high selectivity of long-chain alkanes to prepare olefins with dehydrogenation catalysts is the directional activation of the terminal CH bonds of long-chain alkanes. At present, there is still a lack of alkane dehydrogenation catalysts that can take into account both high selectivity for α+β-olefins and long catalytic life. Summary of the invention
[0005] In view of this, the present invention aims to provide a high olefin selectivity C5-C10 alkane dehydrogenation catalyst and its preparation method and application. The catalyst provided by the present invention can achieve C5-C10 alkane dehydrogenation in naphtha. 10 Selective dehydrogenation of alkanes improves the selectivity of α+β-olefin products and prolongs the service life.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a C5-C10 alkane dehydrogenation catalyst with high olefin selectivity, comprising the following steps:
[0008] mixing a platinum source solution and an organic amine ligand to obtain a precursor solution;
[0009] The precursor solution is mixed with ZSM-5 molecular sieve, and exchange treatment, solid-liquid separation and drying are performed in sequence to obtain a powder product;
[0010] The powder product is mixed with NaOH, tetrapropylammonium hydroxide and water, and subjected to aging treatment, recrystallization, solid-liquid separation and first calcination in sequence to obtain a ZSM-5 molecular sieve loaded Pt catalyst;
[0011] A soluble metal salt, water and an organic small molecule complexing agent are mixed and evaporated to obtain a colloidal solid precursor of a metal oxide; the colloidal solid precursor of the metal oxide is subjected to a second calcination to obtain a metal oxide; the metal element in the soluble metal salt is one or more of Mn, Fe, La, Ga, Sn, In, Cu and Zn;
[0012] The ZSM-5 molecular sieve supported Pt catalyst is physically mixed with the metal oxide and subjected to reduction treatment to obtain a C5-C10 alkane dehydrogenation catalyst with high olefin selectivity.
[0013] Preferred organic amine ligands include one or more of ethylenediamine, cyclohexylamine and cyclohexanediamine;
[0014] The molar ratio of the platinum source to the organic amine ligand is 1:30-200.
[0015] Preferably, the precursor solution further comprises an auxiliary metal salt, and the auxiliary metal element in the auxiliary metal salt is one or more of Mn, Fe, La, Ga, Sn, In, Cu and Zn;
[0016] The molar ratio of the auxiliary metal element to the platinum element in the platinum source is ≤10:1.
[0017] Preferably, the concentration of the platinum source in the precursor solution is 1×10 -6 ~1×10 -4 mol / L;
[0018] The mass ratio of the ZSM-5 molecular sieve to the precursor solution is 1:10 to 100;
[0019] The temperature of the exchange treatment is 30-90° C., and the time is 15-720 min.
[0020] Preferably, after the powder product is mixed with NaOH, tetrapropylammonium hydroxide and water, the molar composition of the obtained mixed solution is H2O:Al2O3:Na2O:tetrapropylammonium hydroxide:SiO2=(10-100):(0.00-0.10):(0.02-0.1):(0.1-0.7):1, wherein Al2O3 and SiO2 come from the ZSM-5 molecular sieve in the powder product, and Na2O comes from NaOH;
[0021] The aging treatment time is 2 to 6 hours, the recrystallization temperature is 150 to 200° C., and the time is 24 to 72 hours;
[0022] The temperature of the first calcination is 350-600° C., and the heat preservation time is 3-10 hours.
[0023] Preferably, the organic small molecule complexing agent is one or more of glucose, citric acid, tartaric acid, salicylic acid and adipic acid;
[0024] The molar ratio of the soluble metal salt to the organic small molecule complexing agent is 1:1 to 10;
[0025] The temperature of the second calcination is 350-600° C., and the heat preservation time is 3-10 hours.
[0026] Preferably, the mass ratio of the ZSM-5 molecular sieve supported Pt catalyst to the metal oxide is 1:0.1-3;
[0027] The reduction treatment is carried out in a reducing atmosphere, the temperature of the reduction treatment is 300 to 600° C., and the time is 1 to 10 hours.
[0028] The present invention provides a high olefin selectivity C5-C10 alkane dehydrogenation catalyst prepared by the above preparation method, comprising a ZSM-5 molecular sieve-loaded Pt catalyst and a metal oxide coupled with the ZSM-5 molecular sieve-loaded Pt catalyst; the metal element in the metal oxide comprises one or more of Mn, Fe, La, Ga, Sn, In, Cu and Zn;
[0029] The ZSM-5 molecular sieve loaded Pt catalyst comprises a ZSM-5 molecular sieve and an active component loaded on the surface and internal pores of the ZSM-5 molecular sieve. The ZSM-5 molecular sieve has a hollow structure, and the active component comprises platinum.
[0030] Preferably, the active component further includes an auxiliary metal, and the auxiliary metal element is one or more of Mn, Fe, La, Ga, Sn, In, Cu and Zn.
[0031] The present invention provides the use of the above-mentioned high olefin selectivity C5-C10 alkane dehydrogenation catalyst in catalyzing the dehydrogenation of C5-C10 alkanes to prepare monoolefins.
[0032] The invention provides a preparation method of a C5-C10 alkane dehydrogenation catalyst with high olefin selectivity, comprising the following steps: mixing a platinum source solution and an organic amine ligand to obtain a precursor solution; mixing the precursor solution with a ZSM-5 molecular sieve, and sequentially performing an exchange treatment, solid-liquid separation and drying to obtain a powder product; mixing the powder product with NaOH, tetrapropylammonium hydroxide and water, and sequentially performing an aging treatment, recrystallization, solid-liquid separation and a first calcination to obtain a ZSM-5 molecular sieve-loaded Pt catalyst; mixing a soluble metal salt, water and an organic small molecule complexing agent, and evaporating to obtain a metal oxide colloidal solid precursor; performing a second calcination on the metal oxide colloidal solid precursor to obtain a metal oxide; the metal element in the soluble metal salt is one or more of Mn, Fe, La, Ga, Sn, In, Cu and Zn; physically mixing the ZSM-5 molecular sieve-loaded Pt catalyst with the metal oxide, and performing a reduction treatment to obtain a C5-C10 alkane dehydrogenation catalyst with high olefin selectivity.
[0033] Based on the defect that the traditional oxide carrier only supports the active component and it is difficult to give full play to the role of the carrier and the active component, the present invention adopts ZSM-5 molecular sieve as the carrier, which has a molecular-sized pore structure, rich specific surface area and shape-selective catalytic properties. Compared with the traditional oxide carrier, the Pt can be supported and the dispersion of Pt and C5~C 10The accessibility of alkane molecules enables the selective adsorption and dehydrogenation of the terminal positions of alkane molecules, which can improve the selectivity of α-olefins and β-olefins. The present invention adds organic amine ligand molecules to the precursor solution for exchange. The ligand can serve as a template for the ZSM-5 molecular sieve and can coordinate with metal ions, thereby allowing platinum to participate in the hydrothermal crystallization of the ZSM-5 molecular sieve, stably introducing Pt (or Pt and auxiliary metal Mx) into the molecular sieve, and achieving the coating of Pt (or PtMx) by the ZSM-5 molecular sieve, which significantly improves the dispersion of Pt, inhibits the agglomeration of Pt in the reaction, and improves the dehydrogenation activity and stability of alkane. The present invention adopts the method of recrystallization of the ZSM-5 molecular sieve to obtain a hollow morphology ZSM-5 molecular sieve carrier, which can slow down the carbon deposition rate, improve the stability of the catalyst, and extend the service life. In addition, the hollow structure can also promote the diffusion of products such as α-olefins and β-olefins, reduce the occurrence of side reactions such as isomerization and cyclization, and improve the selectivity of the target product. The present invention adopts a ZSM-5 molecular sieve loaded with a Pt catalyst (abbreviated as PtMx@molecular sieve) coupled with a metal oxide, which can play a synergistic role, promote the forward dehydrogenation of long-chain alkanes, and greatly improve the activity and stability of alkane dehydrogenation.
[0034] The results of the examples show that the catalyst of the present invention is applied to naphtha C5-C 10 In the reaction of alkane dehydrogenation, the life of the catalyst is as high as over 500 hours, the selectivity of α-olefins and β-olefins in the monoolefin products is as high as 99%, and its selectivity for α-olefins is as high as 70%.
[0035] At the same time, the preparation method provided by the present invention is simple to operate, relatively low in cost, and easy to realize industrial mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a diagram showing the evaluation results of the n-octane dehydrogenation reaction catalyzed by catalyst #1 in Example 1;
[0037] Figure 2 This is a diagram showing the evaluation results of the n-octane dehydrogenation reaction catalyzed by catalyst #2 in Example 2;
[0038] Figure 3 This is a diagram showing the evaluation results of the n-octane dehydrogenation reaction catalyzed by catalyst #3 in Example 3;
[0039] Figure 4 This is a diagram showing the evaluation results of the n-octane dehydrogenation reaction catalyzed by catalyst #4 in Example 4;
[0040] Figure 5 This is a diagram showing the evaluation results of the n-octane dehydrogenation reaction catalyzed by the catalyst #5 in Example 5;
[0041] Figure 6This is a diagram showing the evaluation results of the n-octane dehydrogenation reaction catalyzed by the catalyst #6 in Example 6;
[0042] Figure 7 This is a diagram showing the evaluation results of the n-octane dehydrogenation reaction catalyzed by catalyst #7 in Example 7;
[0043] Figure 8 This is a diagram showing the evaluation results of the n-octane dehydrogenation reaction catalyzed by the catalyst #8 in Example 8;
[0044] Fig. 9 This is a diagram showing the evaluation results of the n-octane dehydrogenation reaction catalyzed by the catalyst #9 in Example 9;
[0045] Fig.10 This is a diagram showing the evaluation results of the n-octane dehydrogenation reaction catalyzed by the catalyst #10 in Example 10;
[0046] Fig.11 This is a diagram showing the evaluation results of the n-octane dehydrogenation reaction catalyzed by the catalyst #11 in Example 11;
[0047] Fig.12 This is a diagram showing the evaluation results of the n-octane dehydrogenation reaction catalyzed by the catalyst #11 in Comparative Example 1;
[0048] Fig.13 This is a diagram showing the evaluation results of the n-octane dehydrogenation reaction catalyzed by the catalyst #12 in Comparative Example 2;
[0049] Fig.14 This is a diagram showing the evaluation results of the n-octane dehydrogenation reaction catalyzed by the catalyst #13 in Comparative Example 3;
[0050] Fig.15 This is a diagram showing the evaluation results of the n-octane dehydrogenation reaction catalyzed by catalyst #14 in Comparative Example 4;
[0051] Fig.16 This is a diagram showing the evaluation results of the dehydrogenation reaction of n-pentane catalyzed by catalyst #1 in Example 1;
[0052] Fig.17 This is a diagram showing the evaluation results of the dehydrogenation reaction of n-hexane catalyzed by catalyst #1 in Example 1;
[0053] Fig.18 This is a diagram showing the evaluation results of the dehydrogenation reaction of n-heptane catalyzed by catalyst #1 in Example 1;
[0054] Fig.19 This is a diagram showing the evaluation results of the dehydrogenation reaction of n-nonane catalyzed by catalyst #1 in Example 1;
[0055] Fig. 20 This is a diagram showing the evaluation results of the dehydrogenation reaction of n-decane catalyzed by catalyst #1 in Example 1;
[0056] Fig.21The selectivity curve of the products 1-octene and 2-octene to the total olefin products in the result of the n-octane dehydrogenation reaction evaluated by the catalyst #1 in Example 1 changes with the reaction time;
[0057] Fig. 22 This is the transmission electron microscopy image of catalyst #1. DETAILED DESCRIPTION
[0058] The present invention provides a method for preparing a C5-C10 alkane dehydrogenation catalyst with high olefin selectivity, comprising the following steps:
[0059] mixing a platinum source solution and an organic amine ligand to obtain a precursor solution;
[0060] The precursor solution is mixed with ZSM-5 molecular sieve, and exchange treatment, solid-liquid separation and drying are performed in sequence to obtain a powder product;
[0061] The powder product is mixed with NaOH, tetrapropylammonium hydroxide and water, and subjected to aging treatment, recrystallization, solid-liquid separation and first calcination in sequence to obtain a ZSM-5 molecular sieve loaded Pt catalyst;
[0062] A soluble metal salt, water and an organic small molecule complexing agent are mixed and evaporated to obtain a colloidal solid precursor of a metal oxide; the colloidal solid precursor of the metal oxide is subjected to a second calcination to obtain a metal oxide; the metal element in the soluble metal salt is one or more of Mn, Fe, La, Ga, Sn, In, Cu and Zn;
[0063] The ZSM-5 molecular sieve supported Pt catalyst is physically mixed with the metal oxide and subjected to reduction treatment to obtain a C5-C10 alkane dehydrogenation catalyst with high olefin selectivity.
[0064] Unless otherwise specified, the raw materials used in the present invention are all commercially available.
[0065] The source of the ZSM-5 molecular sieve used in the present invention is preferably prepared by itself. In the present invention, the preparation method of the ZSM-5 molecular sieve preferably includes the following steps:
[0066] Prepare the parent solution according to the initial gel molar composition of 15H2O: (0.00-0.10)Al2O3: (0.05-0.1)lysine: 0.5tetrapropylammonium hydroxide: 1ethyl orthosilicate;
[0067] Performing hydrothermal crystallization on the parent solution and performing solid-liquid separation on the obtained crystallization product to obtain a solid product;
[0068] The solid product is calcined to obtain a ZSM-5 molecular sieve.
[0069] In the present invention, the raw material corresponding to the Al2O3 is preferably aluminum nitrate; the tetrapropylammonium hydroxide (TPAOH) is preferably used in the form of a tetrapropylammonium hydroxide aqueous solution; the mass fraction of the tetrapropylammonium hydroxide aqueous solution is preferably 25%.
[0070] The present invention has no special requirements for the preparation method of the parent solution. The corresponding raw materials can be directly mixed according to the above molar ratio and then aged. The aging time is preferably 2 to 6 hours. As a specific embodiment of the present invention, the preparation method of the ZSM-5 molecular sieve parent solution is: lysine, a 25% TPAOH aqueous solution, and aluminum nitrate are added to H2O in sequence, stirred at 500 rpm until clear, and tetraethyl orthosilicate (TEOS) is slowly added dropwise, and stirred at room temperature for aging for 2 to 6 hours.
[0071] In the present invention, after the TEOS hydrolysis is completed, the present invention preferably heats the water bath at 60° C. to evaporate excess water to form a matrix solution with a gel ratio of 9H2O: (0.00-0.10)Al2O3: (0.05-0.1)lysine: 0.5tetrapropylammonium hydroxide: 1ethyl orthosilicate.
[0072] In the present invention, the hydrothermal crystallization is preferably carried out in a homogeneous reactor; the temperature of the hydrothermal crystallization is preferably 70 to 200° C., more preferably 70 to 170° C.; the time of the hydrothermal crystallization is preferably 2 to 4 days, more preferably 3 days.
[0073] The present invention has no special requirements for the solid-liquid separation method, and any solid-liquid separation method known in the art can be used, such as centrifugation. After the solid-liquid separation, the present invention preferably dries the obtained solid. In the present invention, the drying temperature is preferably 100° C., and the drying time is preferably 6 to 12 hours.
[0074] In the present invention, the calcination is preferably carried out in an air atmosphere, the calcination temperature is preferably 350-600°C, more preferably 400-500°C, the holding time is preferably 3-10h, more preferably 4-8h. In the present invention, the calcination is used to remove the template.
[0075] The present invention mixes a platinum source solution and an organic amine ligand to obtain a precursor solution. In the present invention, the platinum source in the platinum source solution is preferably one or more of chloroplatinic acid, tetraammine platinum chloride, ethylenediamine platinum chloride, sodium hexachloroplatinate or tetrakis(triphenylphosphine)platinum. In the present invention, the organic amine ligand preferably includes one or more of ethylenediamine, cyclohexylamine and cyclohexanediamine. In the present invention, the molar ratio of the platinum source to the organic amine ligand is preferably 1:30 to 200, more preferably 1:60 to 100.
[0076] The present invention has no special requirements for the mixing method, and any mixing method known in the art can be used, such as stirring. In the present invention, the concentration of the platinum source in the precursor solution is preferably 1×10 -6 ~1×10 -4 mol / L, more preferably 1×10 -5 mol / L.
[0077] In the present invention, platinum in the platinum source is used as an active component; the ligand can serve as a template for the ZSM-5 molecular sieve and can coordinate with metal ions, thereby dispersing platinum in the structure of the ZSM-5 molecular sieve, thereby improving the dispersibility and stability of platinum.
[0078] In the present invention, the precursor solution also preferably includes an auxiliary metal salt, and the auxiliary metal element in the auxiliary metal salt is one or more of Mn, Fe, La, Ga, Sn, In, Cu and Zn. The present invention has no special requirements for the specific type of the auxiliary metal salt, and any salt of the above metal that is soluble in water and is well known in the art can be used, specifically one or more of nitrates, chlorides, carbonates and sulfates. In an embodiment of the present invention, the auxiliary metal salt is Mn(NO3)2·6H2O, FeSO4·12H2O, La(NO3)3, Ga(NO3)3, SnCl4·5H2O, In(NO3)3·5H2O, CuSO4·5H2O or Zn(NO3)2.
[0079] In the present invention, the molar ratio of the auxiliary metal element to the platinum element in the platinum source is preferably ≤ 10: 1, more preferably 1 to 10: 1, and more preferably 3 to 8: 1. In the present invention, the auxiliary metal in the auxiliary metal salt acts as an auxiliary agent, generates an electronic effect with platinum, improves the dehydrogenation activity of the catalyst, and improves the dispersibility of platinum.
[0080] In the present invention, when the precursor solution includes an auxiliary metal salt, the method for preparing the precursor solution preferably includes the following steps:
[0081] The platinum source solution, the auxiliary metal salt and the organic amine ligand are mixed to obtain a precursor solution, which is recorded as a PtMx precursor solution. In the present invention, the auxiliary metal salt is preferably added in the form of a solution. The present invention has no special requirements for the concentration of the auxiliary metal salt solution, as long as the auxiliary metal salt can be completely dissolved.
[0082] After obtaining the precursor solution, the present invention mixes the precursor solution with a ZSM-5 molecular sieve, performs exchange treatment, solid-liquid separation and drying in sequence to obtain a powder product. In the present invention, the mass ratio of the ZSM-5 molecular sieve to the precursor solution is preferably 1:10 to 100, more preferably 1:10 to 50, that is, the solid-liquid ratio of the exchange treatment is preferably 1:10 to 100, more preferably 1:10 to 50.
[0083] In the present invention, after the exchange treatment, the mass ratio of ZSM-5 molecular sieve to Pt is 1:0.05-2%, more preferably 1:0.1-1.5%, more preferably 1:0.5-1%.
[0084] In the present invention, the temperature of the exchange treatment is preferably 30 to 90° C., more preferably 30 to 60° C.; the time is preferably 15 to 720 min, more preferably 60 to 600 min, and further preferably 120 to 300 min.
[0085] The present invention has no special requirements for the solid-liquid separation method, and any solid-liquid separation method known in the art can be used, such as centrifugation. In the present invention, the drying temperature is preferably 100° C., and the drying time is preferably 6 to 12 hours. During the exchange treatment, the Pt (or PtMx) metal exists on the surface of the molecular sieve or in the pore size in the form of ions.
[0086] After obtaining the powder product, the present invention mixes the powder product with NaOH, tetrapropylammonium hydroxide and water, and sequentially performs aging treatment, recrystallization, solid-liquid separation and first calcination to obtain a ZSM-5 molecular sieve loaded with Pt catalyst. In the present invention, after the powder product is mixed with NaOH, tetrapropylammonium hydroxide and water, the molar composition of the obtained mixed solution is H2O:Al2O3:Na2O:tetrapropylammonium hydroxide:SiO2=(10-100):(0.00-0.10):(0.02-0.1):(0.1-0.7):1, wherein Al2O3 and SiO2 come from the ZSM-5 molecular sieve in the powder product, and Na2O comes from NaOH. Preferably, the raw material corresponding to the Al2O3 is aluminum nitrate.
[0087] In the present invention, the tetrapropylammonium hydroxide is preferably used in the form of a tetrapropylammonium hydroxide aqueous solution; the mass fraction of the tetrapropylammonium hydroxide aqueous solution is preferably 25%.
[0088] In the present invention, the aging treatment is preferably carried out at room temperature under stirring; the time of the aging treatment is preferably 2 to 6 hours, more preferably 3 to 4 hours.
[0089] In the present invention, the recrystallization is preferably carried out in a homogeneous reactor; the recrystallization temperature is preferably 150-200°C, more preferably 160-180°C; the time is preferably 24-72h, more preferably 36-48h. The present invention, through the recrystallization process, on the one hand, allows platinum to participate in the hydrothermal crystallization of the ZSM-5 molecular sieve, stably introduces Pt (or Pt and auxiliary metal Mx) into the molecular sieve, realizes the coating of Pt (or PtMx) by the ZSM-5 molecular sieve, significantly improves the dispersion of Pt, inhibits the agglomeration of Pt in the reaction, and improves the activity and stability of alkane dehydrogenation; on the other hand, a hollow morphology ZSM-5 molecular sieve carrier can be obtained, which can slow down the carbon deposition rate, improve the catalyst stability, and extend the service life. In addition, the hollow structure can also promote the diffusion of products such as α-olefins and β-olefins, reduce the occurrence of side reactions such as isomerization and cyclization, and improve the selectivity of the target product.
[0090] The present invention has no special requirements for the solid-liquid separation method, and any solid-liquid separation method known in the art can be used, such as centrifugation.
[0091] In the present invention, the first calcination is preferably carried out in an air atmosphere; the temperature of the first calcination is preferably 350-600°C, more preferably 400-500°C; the holding time is preferably 3-10h, more preferably 4-8h. In the present invention, the function of the calcination is to remove the template.
[0092] The present invention mixes a soluble metal salt, water and an organic small molecule complexing agent, evaporates and obtains a colloidal solid precursor of a metal oxide; the colloidal solid precursor of the metal oxide is subjected to a second calcination to obtain a metal oxide. In the present invention, the metal element in the soluble metal salt is one or more of Mn, Fe, La, Ga, Sn, In, Cu and Zn. The present invention has no special requirements for the specific type of the soluble metal salt, and any salt of the above metal that is soluble in water known in the art can be used, specifically one or more of nitrates, chlorides, carbonates and sulfates. In an embodiment of the present invention, the soluble metal salt is Mn(NO3)2·6H2O, FeSO4·12H2O, La(NO3)3, Ga(NO3)3, SnCl4·5H2O, In(NO3)3·5H2O, CuSO4·5H2O or Zn(NO3)2.
[0093] In the present invention, the small molecule complexing agent is preferably one or more of glucose, citric acid, tartaric acid, salicylic acid and adipic acid, and the molar ratio of the soluble metal salt to the organic small molecule complexing agent is preferably 1:1-10, more preferably 1:1-3.
[0094] In the present invention, the temperature of the evaporation is preferably 120° C., and the time is preferably 6 to 12 hours, more preferably 8 to 10 hours. The present invention removes water from the mixture by evaporation.
[0095] In the present invention, the second calcination is preferably carried out in an air atmosphere, the temperature of the second calcination is preferably 350-600°C, more preferably 400-500°C, and the holding time is preferably 3-10h, more preferably 4-8h. The purpose of the second calcination is to remove the complexing agent.
[0096] After obtaining the metal oxide, the present invention physically mixes the ZSM-5 molecular sieve supported Pt catalyst with the metal oxide and performs a reduction treatment to obtain a high olefin selectivity C5-C10 alkane dehydrogenation catalyst. In the present invention, the mass ratio of the ZSM-5 molecular sieve supported Pt catalyst to the metal oxide is 1:0.1 to 3, more preferably 1:1 to 2.
[0097] In the present invention, the physical mixing method preferably includes one or more of powder mixing, granulation mixing, mixing after ball milling and layered mixing. In the present invention, the mesh number of the granulation mixing is preferably 10 to 100 meshes, more preferably 40 to 80 meshes; the number of layers of the layered mixing is preferably 1 to 20 layers, more preferably 5 to 10 layers of filling.
[0098] In the present invention, the reduction treatment is preferably carried out under a reducing atmosphere, and the reducing atmosphere is preferably a carbon monoxide or hydrogen atmosphere. In the present invention, the temperature of the reduction treatment is preferably 300-600°C, more preferably 300-500°C, and further preferably 300-400°C; the time is preferably 1-10h, more preferably 1-5h, and further preferably 2-4h. In the present invention, during the reduction process, the Pt in the ZSM-5 molecular sieve is reduced to a single substance state and / or a positron state, thereby enhancing the catalytic activity of platinum. During the reduction process, Pt can partially form an alloy with the auxiliary metal, and there are electronic effects and geometric effects. The geometric effect increases the dispersion of Pt and prevents Pt from agglomerating; the electronic effect can promote the CH bond activation dehydrogenation process. In addition, during the reduction process, some metals in the metal oxide can be reduced to metal elements.
[0099] The present invention provides a high olefin selectivity C5-C10 alkane dehydrogenation catalyst prepared by the above preparation method, comprising a ZSM-5 molecular sieve-loaded Pt catalyst and a metal oxide coupled with the ZSM-5 molecular sieve-loaded Pt catalyst; the metal element in the metal oxide comprises one or more of Mn, Fe, La, Ga, Sn, In, Cu and Zn;
[0100] The ZSM-5 molecular sieve supported Pt catalyst comprises a ZSM-5 molecular sieve and an active component supported on the surface and internal pores of the ZSM-5 molecular sieve, wherein the ZSM-5 molecular sieve has a hollow structure, and the active component comprises platinum. In the present invention, the active component preferably further comprises a promoter metal, and the promoter metal element is one or more of Mn, Fe, La, Ga, Sn, In, Cu and Zn.
[0101] In the present invention, the mass content of platinum in the high olefin selectivity C5-C10 alkane dehydrogenation catalyst is preferably 0.01-2.00%, more preferably 0.1-1.50%, further preferably 0.5-1.00%; the mass content of the auxiliary metal element is preferably 0.00-2.00%, more preferably 0.01-1.50%, further preferably 0.1-1.00%.
[0102] In the present invention, the high olefin selectivity C5~C 10 The hollow wall thickness of the ZSM-5 molecular sieve of the alkane dehydrogenation catalyst is preferably 10 to 30 nm, and the crystal size of the ZSM-5 molecular sieve is 50 to 450 nm, more preferably 50 to 150 nm. In the present invention, the active component is loaded on the pores and / or surface of the ZSM-5 molecular sieve.
[0103] In the present invention, high olefin selectivity C5~C 10 The mass ratio of the ZSM-5 molecular sieve-supported Pt catalyst to the metal oxide in the alkane dehydrogenation catalyst is preferably 1:0.1 to 3, more preferably 1:1 to 2. The present invention adopts a coupling method of metal oxide and ZSM-5 molecular sieve-supported Pt catalyst to improve the activity of the catalyst, which can consume hydrogen in the catalytic reaction, and coordinates with the molecular sieve supported by PtMx to improve the selectivity of α+β-olefins.
[0104] The present invention adopts ZSM-5 molecular sieve to confine Pt (or PtMx) metal clusters, and constructs a multifunctional catalyst with metal oxides. By regulating the geometric electronic structure of the Pt (or PtMx) metal clusters and the precise placement of the clusters in the ZSM-5 molecular sieve, the alkane molecules can contact the active sites in a specific adsorption manner, and the terminal CH bonds can be efficiently activated. By coupling with the metal oxide, the hydrogen generated by the reaction can be removed in time, the forward thermodynamic equilibrium can be accelerated, the dehydrogenation of the alkanes and the timely diffusion of the products can be promoted, the occurrence of secondary isomerization can be suppressed, and a higher olefin product, especially monoolefins such as α-olefins and β-olefins, can be obtained while maintaining stable conversion.
[0105] The present invention provides the use of the above-mentioned high olefin selectivity C5-C10 alkane dehydrogenation catalyst in catalyzing the dehydrogenation of C5-C10 alkanes to prepare monoolefins. In the present invention, the C5-C10 alkanes preferably include one or more of n-octane, n-pentane, n-hexane, n-heptane, n-nonane and n-decane. In the present invention, the monoolefins preferably include alpha olefins and / or beta olefins, the alpha olefins are terminal olefins, and the beta olefins are diolefins.
[0106] In the present invention, the conditions for catalyzing the dehydrogenation of C5-C10 alkanes to prepare monoolefins preferably include: the temperature is preferably 320-500°C, the mass space velocity is preferably 0.2-12h -1 The reaction atmosphere preferably includes one or more of nitrogen, hydrogen, carbon monoxide and carbon dioxide, and the ratio of the molar amount of the gas providing the reaction atmosphere to the molar amount of the alkane is less than 5. More preferably, the temperature is 350-450°C, and the mass space velocity is 3-10h -1 In the present invention, the ratio of the molar amount of the gas in the reaction atmosphere to the molar amount of the alkane is 1 to 5.
[0107] In the present invention, the C5-C10 alkane is preferably fed at 0.05 mL / min, and the amount of the catalyst used is preferably 0.35 to 2 g, more preferably 0.5 to 1.5 g.
[0108] The high olefin selectivity C5-C10 alkane dehydrogenation catalyst provided by the present invention, its preparation method and application are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0109] Example 1
[0110] 1.1 Synthesis of ZSM-5 molecular sieve
[0111] 0.7g lysine and 17.57g TPAOH aqueous solution (mass fraction of 25%) were added to 12.57g H2O in sequence and stirred at 500rpm until clear, then 10.00g tetraethyl orthosilicate (TEOS) was slowly added dropwise and aged at room temperature for 4h; the corresponding initial gel molar composition was 15H2O: 0.1 lysine: 0.45TPAOH: 1SiO2. After aging, the gel was moved to a 60℃ water bath for evaporation for 4h to remove excess alcohol and water. After reaching a gel ratio of 9H2O: 0.1 lysine: 0.45TPAOH: 1SiO2, it was moved to a homogeneous reactor for crystallization for 72h, with the crystallization temperature of 70℃ for the first 48h and 170℃ for the last 24h. After crystallization, solid-liquid separation was performed to obtain a solid product, which was calcined at 550℃ in a muffle furnace for 6h to obtain a ZSM-5 molecular sieve.
[0112] 1.2 Synthesis of ZSM-5 molecular sieve supported PtMx catalyst
[0113] 1mL 0.0513mol / L chloroplatinic acid solution and 0.61g ethylenediamine were mixed and dissolved in 20mL water at room temperature, and then 1mL 0.0513mol / L Mn(NO3)2·6H2O was added, and then exchanged with 1g of ZSM-5 molecular sieve powder in 1.1 at room temperature of 30℃ for 6h. After centrifugation, the sample was dried at 100℃ for 12 hours to obtain a molecular sieve powder loaded with PtMn. 0.04g NaOH and 1.64g TPAOH aqueous solution (mass fraction of 25%) were added to 8.99g H2O in sequence and stirred at 500rpm until clear, and then 1g of the above powder was added and stirred at room temperature for aging for 4h. After being transferred to a homogeneous reactor for recrystallization at 170℃ for 36h, the obtained crystallized product was subjected to solid-liquid separation to obtain a solid product. The obtained solid product was calcined at 550℃ in an air atmosphere in a muffle furnace for 5 hours to obtain a calcined product. A ZSM-5 molecular sieve-supported PtMn catalyst was obtained.
[0114] 1.3Mn2O3 oxide synthesis
[0115] 6.0g of Mn(NO3)2·6H2O aqueous solution (50wt.%) was added to 100ml of H2O and stirred evenly, and 10.0g of glucose was added. After the solution was stirred evenly, it was moved to a water bath at 80℃ for 4h to obtain a colloidal solid precursor of metal oxide. After the solid was dried in an oven at 120℃ for 12h, it was calcined in a muffle furnace at 500℃ for 6h to obtain a metal oxide.
[0116] The sample was tableted, crushed, and sieved to 40-60 mesh. The molecular sieve and oxide particles were mixed evenly in a mass ratio of 1:1, and then reduced at 500°C in a hydrogen atmosphere for 2 hours. It was recorded as catalyst #1, abbreviated as Pt-Mn@ZSM-5+Mn2O3 catalyst (the Pt loading in the ZSM-5 molecular sieve is 0.2wt%, and the Mn loading is 0.2wt%).
[0117] Example 2
[0118] 1mL 0.0513mol / L chloroplatinic acid solution and 0.61g ethylenediamine were mixed and dissolved in 20mL water at room temperature, and then 1mL 0.0513mol / L FeSO4·12H2O was added, and then exchanged with 1g ZSM-5 molecular sieve powder prepared in Example 1 at room temperature of 30℃ for 6h. After centrifugation, the sample was dried at 100℃ for 12 hours to obtain a molecular sieve powder loaded with PtMx. 0.04g NaOH and 1.64g TPAOH aqueous solution (mass fraction of 25%) were added to 8.99g H2O in sequence and stirred at 500rpm until clear, and then 1g of the above powder was added and stirred at room temperature for aging for 4h. After being transferred to a homogeneous reactor for recrystallization at 170℃ for 36h, the obtained crystallized product was subjected to solid-liquid separation to obtain a solid product. The obtained solid product was calcined at 550° C. for 5 hours in an air atmosphere in a muffle furnace to obtain a calcined product, thereby obtaining a ZSM-5 molecular sieve-supported PtFe catalyst.
[0119] Synthesis of Fe2O3 oxide
[0120] 6.0g FeSO4·12H2O aqueous solution (50wt.%) was added to 100ml H2O and stirred evenly, and 10.0g glucose was added. After the solution was stirred evenly, it was moved to a water bath at 80℃ for 4h to obtain a colloidal solid precursor of metal oxide. After the solid was dried in an oven at 120℃ for 12h, it was calcined in a muffle furnace at 500℃ for 6h to obtain a metal oxide.
[0121] The sample was tableted, crushed, and sieved to 20-40 mesh. The molecular sieve and oxide particles were mixed evenly in a mass ratio of 1:1, and then reduced at 500°C in a hydrogen atmosphere for 2 hours. It was recorded as catalyst #2, abbreviated as Pt-Fe@ZSM-5+Fe2O3 catalyst (the Pt loading in the ZSM-5 molecular sieve is 0.2wt%, and the Fe loading is 0.2wt%).
[0122] Example 3
[0123] 1mL 0.0513mol / L chloroplatinic acid solution and 0.61g ethylenediamine were mixed and dissolved in 20mL water at room temperature, and then 1mL 0.0513mol / L La(NO3)3 was added, and then exchanged with 1g ZSM-5 molecular sieve powder prepared in Example 1 at room temperature of 30°C for 6h. After centrifugation, the sample was dried at 100°C for 12 hours to obtain a molecular sieve powder loaded with PtMx. 0.04g NaOH and 1.64g TPAOH aqueous solution (mass fraction of 25%) were added to 8.99g H2O in sequence and stirred at 500rpm until clear, and then 1g of the above powder was added and stirred at room temperature for aging for 4h. After being transferred to a homogeneous reactor for recrystallization at 170°C for 36h, the obtained crystallized product was subjected to solid-liquid separation to obtain a solid product. The obtained solid product was roasted at 550°C in an air atmosphere in a muffle furnace for 5 hours to obtain a roasted product. A ZSM-5 molecular sieve loaded with PtLa catalyst was obtained.
[0124] Synthesis of La2O3 Oxide
[0125] 6.0g La(NO3)3 aqueous solution (50wt.%) was added to 100ml H2O and stirred evenly, and 10.0g glucose was added. After the solution was stirred evenly, it was moved to a water bath at 80℃ for 4h to obtain a colloidal solid precursor of metal oxide. After the solid was dried in an oven at 120℃ for 12h, it was calcined in a muffle furnace at 500℃ for 6h to obtain a metal oxide.
[0126] The sample was tableted, crushed, and the molecular sieve and oxide powder were mixed in a mass ratio of 1:1, sieved to 20-40 mesh, and reduced at 500°C in a hydrogen atmosphere for 2 hours. It was recorded as catalyst #3, abbreviated as Pt-La@ZSM-5+La2O3 (the Pt loading in the ZSM-5 molecular sieve is 0.2wt%, and the La loading is 0.2wt%).
[0127] Example 4
[0128] 1mL 0.0513mol / L chloroplatinic acid solution and 0.61g ethylenediamine were mixed and dissolved in 20mL water at room temperature, and then 1mL 0.0513mol / L Ga(NO3)3 was added, and then exchanged with 1g ZSM-5 molecular sieve powder prepared in Example 1 at room temperature of 30°C for 6h. After centrifugation, the sample was dried at 100°C for 12 hours to obtain a molecular sieve powder loaded with PtMx. 0.04g NaOH and 1.64g TPAOH aqueous solution (mass fraction of 25%) were added to 8.99g H2O in sequence and stirred at 500rpm until clear, and then 1g of the above powder was added and stirred at room temperature for aging for 4h. After being transferred to a homogeneous reactor for recrystallization at 170°C for 36h, the obtained crystallized product was subjected to solid-liquid separation to obtain a solid product. The obtained solid product was calcined at 550°C in an air atmosphere in a muffle furnace for 5 hours to obtain a calcined product. A ZSM-5 molecular sieve loaded with PtGa catalyst was obtained.
[0129] Synthesis of Ga2O3 Oxide
[0130] 6.0g of Ga(NO3)3 aqueous solution (50wt.%) was added to 100ml of H2O and stirred evenly, and 10.0g of glucose was added. After the solution was stirred evenly, it was moved to a water bath at 80℃ for 4h to obtain a colloidal solid precursor of metal oxide. After the solid was dried in an oven at 120℃ for 12h, it was calcined in a muffle furnace at 500℃ for 6h to obtain a metal oxide.
[0131] The sample was tableted, crushed, and sieved to 20-40 mesh. The mass ratio of molecular sieve to oxide particles was 1:1. The molecular sieve and the oxide were divided into 5 parts of equal mass, loaded layer by layer into a fixed bed, and reduced at 500°C in a hydrogen atmosphere for 2 hours. It was recorded as catalyst #4, abbreviated as Pt-Ga@ZSM-5+Ga2O3 catalyst (the Pt loading in the ZSM-5 molecular sieve was 0.2wt%, and the Ga loading was 0.2wt%).
[0132] Example 5
[0133] 1mL 0.0513mol / L chloroplatinic acid solution and 0.61g ethylenediamine were mixed and dissolved in 20mL water at room temperature, and then 1mL 0.0513mol / L SnCl4·5H2O was added, and then exchanged with 1g ZSM-5 molecular sieve powder prepared in Example 1 at room temperature of 30℃ for 6h. After centrifugation, the sample was dried at 100℃ for 12 hours to obtain a molecular sieve powder loaded with PtMx. 0.04g NaOH and 1.64g TPAOH aqueous solution (mass fraction of 25%) were added to 8.99g H2O in sequence and stirred at 500rpm until clear, and then 1g of the above powder was added and stirred at room temperature for aging for 4h. After being transferred to a homogeneous reactor for recrystallization at 170℃ for 36h, the obtained crystallized product was subjected to solid-liquid separation to obtain a solid product. The obtained solid product was roasted at 550℃ in an air atmosphere in a muffle furnace for 5 hours to obtain a roasted product. The ZSM-5 molecular sieve supported PtSn catalyst was obtained.
[0134] SnO2 Oxide Synthesis
[0135] 6.0g SnCl4·5H2O aqueous solution (50wt.%) was added to 100ml H2O and stirred evenly, and 10.0g glucose was added. After the solution was stirred evenly, it was moved to a water bath at 80℃ for 4h to obtain a colloidal solid precursor of metal oxide. After the solid was dried in an oven at 120℃ for 12h, it was calcined in a muffle furnace at 500℃ for 6h to obtain a metal oxide.
[0136] The sample was tableted, crushed, and sieved to 20-40 mesh. The molecular sieve and oxide particles were mixed evenly in a mass ratio of 1:1, and then reduced at 500°C in a hydrogen atmosphere for 2 hours. It was recorded as catalyst #5, abbreviated as Pt-Sn@ZSM-5+SnO2 catalyst (the Pt loading in the ZSM-5 molecular sieve is 0.2wt%, and the Sn loading is 0.2wt%).
[0137] Example 6
[0138] 1mL 0.0513mol / L chloroplatinic acid solution and 0.61g ethylenediamine were mixed and dissolved in 20mL water at room temperature, and then 1mL 0.0513mol / L In(NO3)3·5H2O was added, and then exchanged with 1g ZSM-5 molecular sieve powder prepared in Example 1 at room temperature of 30°C for 6h. After centrifugation, the sample was dried at 100°C for 12 hours to obtain a molecular sieve powder loaded with PtMx. 0.04g NaOH and 1.64g TPAOH aqueous solution (mass fraction of 25%) were added to 8.99g H2O in sequence and stirred at 500rpm until clear, and then 1g of the above powder was added and stirred at room temperature for aging for 4h. After being transferred to a homogeneous reactor for recrystallization at 170°C for 36h, the obtained crystallized product was subjected to solid-liquid separation to obtain a solid product. The obtained solid product was calcined at 550°C in an air atmosphere in a muffle furnace for 5 hours to obtain a calcined product. A ZSM-5 molecular sieve loaded PtIn catalyst was obtained.
[0139] In2O3 Oxide Synthesis
[0140] 6.0g In(NO3)3·5H2O aqueous solution (50wt.%) was added to 100ml H2O and stirred evenly, and 10.0g glucose was added. After the solution was stirred evenly, it was moved to a water bath at 80℃ for 4h to obtain a colloidal solid precursor of metal oxide. After the solid was dried in an oven at 120℃ for 12h, it was calcined in a muffle furnace at 500℃ for 6h to obtain a metal oxide.
[0141] The sample was tableted, crushed, and sieved to 20-40 mesh. The molecular sieve and oxide particles were mixed evenly in a mass ratio of 1:1, and then reduced at 500°C in a hydrogen atmosphere for 2 hours. It was recorded as catalyst #6, abbreviated as Pt-In@ZSM-5+In2O3 catalyst (the Pt loading in the ZSM-5 molecular sieve is 0.2wt%, and the In loading is 0.2wt%).
[0142] Example 7
[0143] 1mL 0.0513mol / L chloroplatinic acid solution and 0.61g ethylenediamine were mixed and dissolved in 20mL water at room temperature, and then 1mL 0.0513mol / L CuSO4·5H2O was added, and then exchanged with 1g ZSM-5 molecular sieve powder prepared in Example 1 at room temperature of 30℃ for 6h. After centrifugation, the sample was dried at 100℃ for 12 hours to obtain a molecular sieve powder loaded with PtMx. 0.04g NaOH and 1.64g TPAOH aqueous solution (mass fraction of 25%) were added to 8.99g H2O in sequence and stirred at 500rpm until clear, and then 1g of the above powder was added and stirred at room temperature for aging for 4h. After being transferred to a homogeneous reactor and recrystallized at 170℃ for 36h, the obtained crystallized product was separated into solid and liquid to obtain a solid product. The obtained solid product was roasted at 550℃ in an air atmosphere in a muffle furnace for 5 hours to obtain a roasted product. A ZSM-5 molecular sieve loaded with PtCu catalyst was obtained.
[0144] CuO Oxide Synthesis
[0145] 6.0g CuSO4·5H2O aqueous solution (50wt.%) was added to 100ml H2O and stirred evenly, and 10.0g glucose was added. After the solution was stirred evenly, it was moved to a water bath at 80℃ for 4h to obtain a colloidal solid precursor of metal oxide. After the solid was dried in an oven at 120℃ for 12h, it was calcined in a muffle furnace at 500℃ for 6h to obtain a metal oxide.
[0146] The sample was tableted, crushed, and sieved to 20-40 mesh. The molecular sieve and oxide particles were mixed evenly in a mass ratio of 1:1, and then reduced at 500°C in a hydrogen atmosphere for 2 hours. It was recorded as catalyst #7, abbreviated as Pt-Cu@ZSM-5+CuO catalyst (the Pt loading in the ZSM-5 molecular sieve is 0.2wt%, and the Cu loading is 0.2wt%).
[0147] Example 8
[0148] 1mL 0.0513mol / L chloroplatinic acid solution and 0.61g ethylenediamine were mixed and dissolved in 20mL water at room temperature, and then 1mL 0.0513mol / L Zn(NO3)2 solution was added, and then exchanged with 1g ZSM-5 molecular sieve powder prepared in Example 1 at room temperature of 30°C for 6h. After centrifugation, the sample was dried at 100°C for 12 hours to obtain a molecular sieve powder loaded with PtMx. 0.04g NaOH and 1.64g TPAOH aqueous solution (mass fraction of 25%) were added to 8.99g H2O in sequence and stirred at 500rpm until clear, and then 1g of the above powder was added and stirred at room temperature for aging for 4h. After being transferred to a homogeneous reactor for recrystallization at 170°C for 36h, the obtained crystallized product was subjected to solid-liquid separation to obtain a solid product. The obtained solid product was roasted at 550°C in an air atmosphere in a muffle furnace for 5 hours to obtain a roasted product. A ZSM-5 molecular sieve supported PtZn catalyst was obtained.
[0149] ZnO Oxide Synthesis
[0150] Add 6.0g Zn(NO3)2 aqueous solution to 100ml H2O and stir evenly, then add 10.0g glucose. After stirring evenly, move the solution to a 80℃ water bath for 4h to obtain a colloidal solid precursor of metal oxide. After drying the solid in a 120℃ oven for 12h, calcine it in a muffle furnace at 500℃ for 6h to obtain a metal oxide.
[0151] The sample was tableted, crushed, and sieved to 20-40 mesh. The molecular sieve and oxide particles were mixed evenly in a mass ratio of 1:1, and then reduced at 500°C in a hydrogen atmosphere for 2 hours for activity testing. It was recorded as catalyst #8, abbreviated as Pt-Zn@ZSM-5+ZnO catalyst (the Pt loading in the ZSM-5 molecular sieve is 0.2wt%, and the Zn loading is 0.2wt%).
[0152] Example 9
[0153] 1mL 0.0513mol / L chloroplatinic acid solution and 0.61g ethylenediamine were mixed and dissolved in 20mL water at room temperature, and then 1mL 0.0513mol / L Mn(NO3)2·6H2O solution was added, and then exchanged with 1g ZSM-5 molecular sieve powder prepared in Example 1 at room temperature of 30℃ for 6h. After centrifugation, the sample was dried at 100℃ for 12 hours to obtain a molecular sieve powder loaded with PtMx. 0.04g NaOH and 1.64g TPAOH aqueous solution (mass fraction of 25%) were added to 8.99g H2O in sequence and stirred at 500rpm until clear, and then 1g of the above powder was added and stirred at room temperature for aging for 4h. After being transferred to a homogeneous reactor for recrystallization at 170℃ for 36h, the obtained crystallized product was subjected to solid-liquid separation to obtain a solid product. The obtained solid product was calcined at 550℃ in an air atmosphere in a muffle furnace for 5 hours to obtain a calcined product. A ZSM-5 molecular sieve-supported PtMn catalyst was obtained.
[0154] ZnO Oxide Synthesis
[0155] Add 6.0g Zn(NO3)2 aqueous solution to 100ml H2O and stir evenly, then add 10.0g glucose. After stirring evenly, transfer the solution to a water bath at 80℃ for 4h to obtain a colloidal solid precursor of metal oxide. Dry the solid in an oven at 120℃ for 12h, and then calcine it in a muffle furnace at 500℃ for 6h to obtain a metal oxide.
[0156] The sample was tableted, crushed, sieved to 20-40 mesh, and the molecular sieve and oxide particles were mixed uniformly in a mass ratio of 1:1. The mixture was then reduced at 500°C in a hydrogen atmosphere for 2 h and recorded as catalyst #9, abbreviated as Pt-Mn@ZSM-5+ZnO catalyst (the Pt loading in the ZSM-5 molecular sieve was 0.2wt%, and the Mn loading was 0.2wt%).
[0157] Example 10
[0158] 1mL 0.0513mol / L chloroplatinic acid solution and 0.61g ethylenediamine were mixed and dissolved in 20mL water at room temperature, and then 1mL 0.0513mol / L Zn(NO3)2 solution was added, and then exchanged with 1g ZSM-5 molecular sieve powder prepared in Example 1 at room temperature of 30°C for 6h. After centrifugation, the sample was dried at 100°C for 12 hours to obtain a molecular sieve powder loaded with PtMx. 0.04g NaOH and 1.64g TPAOH aqueous solution (mass fraction of 25%) were added to 8.99g H2O in sequence and stirred at 500rpm until clear, and then 1g of the above powder was added and stirred at room temperature for aging for 4h. After being transferred to a homogeneous reactor for recrystallization at 170°C for 36h, the obtained crystallized product was subjected to solid-liquid separation to obtain a solid product. The obtained solid product was roasted at 550°C in an air atmosphere in a muffle furnace for 5 hours to obtain a roasted product. A ZSM-5 molecular sieve supported PtZn catalyst was obtained.
[0159] Synthesis of Mn2O3 oxide
[0160] Add 6.0g of Mn(NO3)2·6H2O aqueous solution to 100ml of H2O and stir evenly, then add 10.0g of glucose. After stirring evenly, move the solution to a water bath at 80℃ for 4h to obtain a colloidal solid precursor of metal oxide. Dry the solid in an oven at 120℃ for 12h, and then calcine it in a muffle furnace at 500℃ for 6h to obtain a metal oxide.
[0161] The sample was tableted, crushed, and sieved to 20-40 mesh. The molecular sieve and oxide particles were mixed evenly in a mass ratio of 1:1, and then reduced at 500°C in a hydrogen atmosphere for 2 hours. It was recorded as catalyst #10, abbreviated as Pt-Zn@ZSM-5+Mn2O3 catalyst (the Pt loading in the ZSM-5 molecular sieve is 0.2wt%, and the Zn loading is 0.2wt%).
[0162] Embodiment 11
[0163] 1mL 0.0513mol / L chloroplatinic acid solution and 0.61g ethylenediamine were mixed and dissolved in 20mL water at room temperature, and then exchanged with 1g ZSM-5 molecular sieve powder prepared in Example 1 at room temperature of 30°C for 6h. After centrifugation, the sample was dried at 100°C for 12 hours to obtain a molecular sieve powder loaded with PtMx. 0.04g NaOH and 1.64g TPAOH aqueous solution (mass fraction of 25%) were added to 8.99g H2O in sequence and stirred at 500rpm until clear, then 1g of the above powder was added and stirred at room temperature for aging for 4h. After being transferred to a homogeneous reactor for recrystallization at 170°C for 36h, the obtained crystallized product was subjected to solid-liquid separation to obtain a solid product. The obtained solid product was calcined at 550°C in an air atmosphere in a muffle furnace for 5 hours to obtain a calcined product. A ZSM-5 molecular sieve loaded with Pt catalyst was obtained.
[0164] Synthesis of Mn2O3 oxide
[0165] Add 6.0g of Mn(NO3)2·6H2O aqueous solution to 100ml of H2O and stir evenly, then add 10.0g of glucose. After stirring evenly, move the solution to a water bath at 80℃ for 4h to obtain a colloidal solid precursor of metal oxide. Dry the solid in an oven at 120℃ for 12h, and then calcine it in a muffle furnace at 500℃ for 6h to obtain a metal oxide.
[0166] The sample was tableted, crushed, and sieved to 20-40 mesh. The molecular sieve and oxide particles were mixed evenly in a mass ratio of 1:1, and then reduced at 500°C in a hydrogen atmosphere for 2 hours. It was recorded as catalyst #11, abbreviated as Pt@ZSM-5+Mn2O3 catalyst (the Pt loading in the ZSM-5 molecular sieve was 0.2wt%).
[0167] Comparative Example 1 Non-hollow morphology catalyst
[0168] 1mL 0.0513mol / L chloroplatinic acid solution and 0.61g ethylenediamine were mixed and dissolved in 20mL water at room temperature, and then 1mL 0.0513mol / L Mn(NO3)2·6H2O was added, and then exchanged with 1g ZSM-5 molecular sieve powder prepared in Example 1 at room temperature of 30°C for 6h. After centrifugation, the sample was dried at 100°C for 12 hours to obtain a molecular sieve powder loaded with PtMn. The obtained powder product was calcined at 550°C in an air atmosphere in a muffle furnace for 5 hours to obtain a calcined product. A ZSM-5 molecular sieve loaded with PtMn catalyst (without hollow structure) was obtained.
[0169] Synthesis of Mn2O3 oxide
[0170] Add 6.0g of Mn(NO3)2·6H2O aqueous solution to 100ml of H2O and stir evenly, then add 10.0g of glucose. After stirring evenly, move the solution to a water bath at 80℃ for 4h to obtain a colloidal solid precursor of metal oxide. Dry the solid in an oven at 120℃ for 12h, and then calcine it in a muffle furnace at 500℃ for 6h to obtain a metal oxide.
[0171] The sample was tableted, crushed, and sieved to 20-40 mesh. The molecular sieve and oxide particles were mixed uniformly in a mass ratio of 1:1, and then reduced at 500°C in a hydrogen atmosphere for 2 hours. It was recorded as catalyst #12 (the Pt loading in the ZSM-5 molecular sieve was 0.2wt%, and the Mn loading was 0.2wt%).
[0172] Comparative Example 2 In-situ encapsulation type hollow morphology catalyst (metal is added directly during the in-situ encapsulation process)
[0173] 1 mL of 0.0513 mol / L chloroplatinic acid solution and 0.61 g of ethylenediamine were mixed at room temperature, and then 1 mL of 0.0513 mol / L mn(NO3)2·6H2O was added to obtain a metal precursor solution.
[0174] 0.7g lysine and 17.57g TPAOH aqueous solution (mass fraction of 25%) were added to 12.57g H2O in sequence and stirred at 500rpm until clear, then 10.00g tetraethyl orthosilicate (TEOS) was slowly added dropwise and aged at room temperature for 4h; the corresponding initial gel molar composition was 15H2O: 0.1 lysine: 0.45TPAOH: 1SiO2. After aging, the mixture was moved to a 60℃ water bath for evaporation for 4h, and the excess alcohol and water were removed. After reaching a gel ratio of 9H2O: 0.1 lysine: 0.45TPAOH: 1SiO2, the above metal precursor solution was added and moved to a homogeneous reactor for crystallization for 72h. The crystallization temperature for the first 48h was 70℃, and the crystallization temperature for the last 24h was 170℃. After crystallization, solid-liquid separation was performed to obtain a solid product, which was calcined at 550℃ in a muffle furnace for 6h.
[0175] 0.04g NaOH and 1.64g TPAOH aqueous solution (mass fraction of 25%) were added to 8.99g H2O in sequence and stirred at 500rpm until clear, then 1g of the above powder was added and stirred at room temperature for aging for 4h. After being transferred to a homogeneous reactor for recrystallization at 170°C for 36h, the obtained crystallized product was subjected to solid-liquid separation to obtain a solid product. The obtained solid product was calcined at 550°C in an air atmosphere in a muffle furnace for 5 hours to obtain a calcined product. A ZSM-5 molecular sieve encapsulated PtMn catalyst was obtained.
[0176] Synthesis of Mn2O3 oxide
[0177] Add 6.0g of Mn(NO3)2·6H2O aqueous solution to 100ml of H2O and stir evenly, then add 10.0g of glucose. After stirring evenly, move the solution to a water bath at 80℃ for 4h to obtain a colloidal solid precursor of metal oxide. Dry the solid in an oven at 120℃ for 12h, and then calcine it in a muffle furnace at 500℃ for 6h to obtain a metal oxide.
[0178] The sample was tableted, crushed, and sieved to 20-40 mesh. The molecular sieve and oxide particles were mixed uniformly in a mass ratio of 1:1, and then reduced at 500°C in a hydrogen atmosphere for 2 hours. It was recorded as catalyst #13 (the Pt loading in the ZSM-5 molecular sieve was 0.2wt%, and the Mn loading was 0.2wt%).
[0179] Comparative Example 3: Uncoupled Metal Oxide
[0180] 1mL 0.0513mol / L chloroplatinic acid solution and 0.61g ethylenediamine were mixed and dissolved in 20mL water at room temperature, and then 1mL 0.0513mol / L Mn(NO3)2·6H2O solution was added, and then exchanged with 1g ZSM-5 molecular sieve powder prepared in Example 1 at room temperature of 30℃ for 6h. After centrifugation, the sample was dried at 100℃ for 12 hours to obtain a molecular sieve powder loaded with PtMx. 0.04g NaOH and 1.64g TPAOH aqueous solution (mass fraction of 25%) were added to 8.99g H2O in sequence and stirred at 500rpm until clear, and then 1g of the above powder was added and stirred at room temperature for aging for 4h. After being transferred to a homogeneous reactor for recrystallization at 170℃ for 36h, the obtained crystallized product was subjected to solid-liquid separation to obtain a solid product. The obtained solid product was calcined at 550℃ in an air atmosphere in a muffle furnace for 5 hours to obtain a calcined product. A ZSM-5 molecular sieve-supported PtMn catalyst was obtained.
[0181] The sample was tableted, crushed, sieved to 20-40 mesh, and evenly mixed with molecular sieve and quartz sand particles in a mass ratio of 1:1. It was then reduced at 500°C in a hydrogen atmosphere for 2 hours and recorded as catalyst #14 (the Pt loading in the ZSM-5 molecular sieve was 0.2%, and the Mn loading was 0.2%).
[0182] Comparative Example 4
[0183] 1mL 0.0513mol / L chloroplatinic acid solution and 0.61g ethylenediamine were mixed and dissolved in 20mL water at room temperature, and then 1mL 0.0513mol / L Mn(NO3)2·6H2O solution was added, and then exchanged with 1g ZSM-5 molecular sieve powder prepared in Example 1 at room temperature of 30℃ for 6h. After centrifugation, the sample was dried at 100℃ for 12 hours to obtain a molecular sieve powder loaded with PtMx. 0.04g NaOH and 1.64g TPAOH aqueous solution (mass fraction of 25%) were added to 8.99g H2O in sequence and stirred at 500rpm until clear, and then 1g of the above powder was added and stirred at room temperature for aging for 4h. After being transferred to a homogeneous reactor for recrystallization at 170℃ for 36h, the obtained crystallized product was subjected to solid-liquid separation to obtain a solid product. The obtained solid product was calcined at 550℃ in an air atmosphere in a muffle furnace for 5 hours to obtain a calcined product. A ZSM-5 molecular sieve-supported PtMn catalyst was obtained.
[0184] The sample was tableted, crushed, and sieved to 20-40 mesh. The molecular sieve and commercially available oxide (Mn2O3) were mixed in a mass ratio of 1:1, and then reduced at 500°C in a hydrogen atmosphere for 2 hours. It was recorded as catalyst #15 (the Pt loading in the ZSM-5 molecular sieve was 0.2%, and the Mn loading was 0.2%).
[0185] Evaluation of fixed bed reaction in application examples 1 to 11 and comparative application examples 1 to 4
[0186] The dehydrogenation reaction of n-octane was carried out in a continuous flow fixed bed microreactor using fourteen catalysts: #1, #2, #3, #4, #5, #6, #7, #8, #9, #10, #11, #12, #13, #14 and #15.
[0187] Application Example 1 The reaction conditions are: normal pressure, temperature 420°C, mass space velocity of n-octane 6h -1 , the molar ratio of nitrogen to n-octane is 1.33.
[0188] Application Example 2 The reaction conditions are normal pressure, temperature 420°C, and mass space velocity of n-octane 6h -1 , the molar ratio of carbon monoxide to n-octane is 1.33.
[0189] Application Example 3 The reaction conditions are normal pressure, temperature 420°C, and mass space velocity of n-octane 6h -1 , the molar ratio of carbon dioxide to n-octane is 1.33.
[0190] Application Example 4 The reaction conditions are: normal pressure, temperature 420°C, mass space velocity of n-octane 6h -1 , the molar ratio of nitrogen to n-octane is 1.33.
[0191] Application Example 5 The reaction conditions are: normal pressure, temperature 420°C, mass space velocity of n-octane 6h -1 , the molar ratio of nitrogen to n-octane is 1.33.
[0192] Application Example 6 The reaction conditions are: normal pressure, temperature 420°C, mass space velocity of n-octane 6h -1 , the molar ratio of nitrogen to n-octane is 1.33.
[0193] Application Example 7 The reaction conditions are: normal pressure, temperature 420°C, mass space velocity of n-octane 6h -1 , the molar ratio of nitrogen to n-octane is 1.33.
[0194] Application Example 8 The reaction conditions are: normal pressure, temperature 420°C, mass space velocity of n-octane 6h -1 , the molar ratio of hydrogen to n-octane is 1.33.
[0195] Application Example 9 The reaction conditions are: normal pressure, temperature 420°C, mass space velocity of n-octane 6h -1 , the molar ratio of nitrogen to n-octane is 1.33.
[0196] Application Example 10 The reaction conditions are: normal pressure, temperature 420°C, mass space velocity of n-octane 6h -1 , the molar ratio of nitrogen to n-octane is 1.33.
[0197] Application Example 11 The reaction conditions are: normal pressure, temperature 420°C, mass space velocity of n-octane 6h -1 , the molar ratio of nitrogen to n-octane is 1.33.
[0198] Comparative Application Example 1 The reaction conditions are: normal pressure, temperature 420°C, mass space velocity of n-octane 6h -1 , the molar ratio of nitrogen to n-octane is 1.33.
[0199] Comparative Application Example 2 The reaction conditions are: normal pressure, temperature 420°C, mass space velocity of n-octane 6h -1 , the molar ratio of nitrogen to n-octane is 1.33.
[0200] Comparative Application Example 3 The reaction conditions are: normal pressure, temperature 420°C, mass space velocity of n-octane 6h -1 , the molar ratio of nitrogen to n-octane is 1.33.
[0201] Comparative Application Example 4 The reaction conditions are: normal pressure, temperature 420°C, mass space velocity of n-octane 6h -1 , the molar ratio of nitrogen to n-octane is 1.33.
[0202] The products were analyzed by Agilent 7890B gas chromatography and Agilent 7890A oil chromatography. The reaction evaluation results are shown in Figures 1 to 15 , the comparison results are shown in Table 1.
[0203] Table 1 Application examples and comparative application examples Reactant conversion rate and product selectivity results (%) after 30 hours of reaction
[0204]
[0205]
[0206] From the results of application examples 1 to 11 in Table 1, it can be seen that the coupling process of metal additives and metal oxides can greatly improve the activity of the reaction, especially the dehydrogenation ability of α+β-olefins. Compared with the hollow structure carrier that is not formed in comparative application example 1, the diffusion of the product is promoted, the secondary reaction of monoolefins is inhibited, and the selectivity of α+β-olefins is improved. Compared with the in-situ encapsulation method of comparative application example 2, the present invention first uses ion exchange to prepare the catalyst to achieve the coating of Pt particles by ZSM-5 molecular sieve, which significantly improves the dispersion of Pt, inhibits the agglomeration of Pt in the reaction, and improves the dehydrogenation activity and stability of alkanes. Compared with comparative application example 3, it can be seen that in the case of coupling metal oxides, the forward dehydrogenation equilibrium can be promoted, and the activity of alkane reactions can be improved. Compared with comparative application example 4, the catalyst activity of commercially available manganese oxide coupled with molecular sieve is lower than that of the oxide prepared by the present invention, and the oxide prepared by the present invention has better stability.
[0207] Application Examples 16-20
[0208] The difference from Application Example 1 is that the reaction raw materials are changed, and n-pentane, n-hexane, n-heptane, n-nonane and n-decane are used as the raw materials of the dehydrogenation catalyst. Using catalyst #1, the reaction conditions of Application Examples 15-19 are the same as those of Application Example 1. The products are analyzed by Agilent 7890B gas chromatography and Agilent 7890A oil chromatography. The reaction evaluation results are shown in Figures 16-20 The results of the comparison of the reactant conversion rate and product selectivity after 30 hours of reaction are shown in Table 2
[0209] Table 2 Results of reactant conversion and product selectivity in application examples 16 to 20 for 30 hours (%)
[0210]
[0211] As shown in Table 2, the catalyst of the present invention can be applied to C5~C 10 Dehydrogenation is universal and can obtain terminal olefins, so it has a wide range of applications.
[0212] Application Example 21
[0213] The life test of n-octane dehydrogenation reaction was carried out in a continuous flow fixed bed microreactor. The reaction conditions were: atmospheric pressure, temperature 420℃, mass space velocity of n-octane 6h -1 The molar ratio of nitrogen to n-heptane was 1.33. Using catalyst #1, the product was analyzed by Agilent 7890B gas chromatography and Agilent 7890A oil chromatography. The reaction evaluation results are shown in Fig.21 . Fig.21 The corresponding specific data are shown in Table 3.
[0214] Table 3 Results of reactant conversion and product selectivity in Application Example 21 after 120 hours of reaction (%)
[0215]
[0216] Depend on Fig.21 As can be seen from Table 3, the dehydrogenation catalyst of the present invention has good stability, a long service life, and can operate stably for 500 hours.
[0217] Fig. 22 This is the transmission electron microscope image of catalyst #1. Fig. 22 It can be seen that the high olefin selectivity C5-C10 alkane dehydrogenation catalyst obtained by the present invention has no Pt particle aggregation and does not form large particle Pt clusters.
[0218] It can be seen from the above examples and comparative examples that the present invention greatly improves the service life of the catalyst, and the obtained high olefin selectivity C5-C10 alkane dehydrogenation catalyst has high dehydrogenation activity and high α+β-olefin selectivity for alkane dehydrogenation reaction.
[0219] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a C5-C10 alkane dehydrogenation catalyst with high olefin selectivity, characterized in that: The following steps are involved: mixing a platinum source solution and an organic amine ligand to obtain a precursor solution; The precursor solution is mixed with ZSM-5 molecular sieve, and exchange treatment, solid-liquid separation and drying are performed in sequence to obtain a powder product; The powder product is mixed with NaOH, tetrapropylammonium hydroxide and water, and subjected to aging treatment, recrystallization, solid-liquid separation and first calcination in sequence to obtain a ZSM-5 molecular sieve loaded Pt catalyst; A soluble metal salt, water and an organic small molecule complexing agent are mixed and evaporated to obtain a colloidal solid precursor of a metal oxide; the colloidal solid precursor of the metal oxide is subjected to a second calcination to obtain a metal oxide; the metal element in the soluble metal salt is one or more of Mn, Fe, La, Ga, Sn, In, Cu and Zn; The ZSM-5 molecular sieve supported Pt catalyst is physically mixed with the metal oxide and subjected to reduction treatment to obtain a C5-C10 alkane dehydrogenation catalyst with high olefin selectivity.
2. The preparation method according to claim 1, characterized in that: The organic amine ligand includes one or more of ethylenediamine, cyclohexylamine and cyclohexanediamine; The molar ratio of the platinum source to the organic amine ligand is 1:30-200.
3. The preparation method according to claim 1, characterized in that: The precursor solution also includes an auxiliary metal salt, wherein the auxiliary metal element in the auxiliary metal salt is one or more of Mn, Fe, La, Ga, Sn, In, Cu and Zn; The molar ratio of the auxiliary metal element to the platinum element in the platinum source is ≤10:
1.
4. The preparation method according to claim 1 or 3, characterized in that: The concentration of the platinum source in the precursor solution is 1×10 -6 ~1×10 -4 mol / L; The mass ratio of the ZSM-5 molecular sieve to the precursor solution is 1:10 to 100; The temperature of the exchange treatment is 30-90° C., and the time is 15-720 min.
5. The preparation method according to claim 1 or 3, characterized in that: After the powder product is mixed with NaOH, tetrapropylammonium hydroxide and water, the molar composition of the obtained mixed solution is H2O:Al2O3:Na2O:tetrapropylammonium hydroxide:SiO2=(10-100):(0.00-0.10):(0.02-0.1):(0.1-0.7):1, wherein Al2O3 and SiO2 come from the ZSM-5 molecular sieve in the powder product, and Na2O comes from NaOH; The aging treatment time is 2 to 6 hours, the recrystallization temperature is 150 to 200° C., and the time is 24 to 72 hours; The temperature of the first calcination is 350-600° C., and the heat preservation time is 3-10 hours.
6. The preparation method according to claim 1, characterized in that: The organic small molecule complexing agent is one or more of glucose, citric acid, tartaric acid, salicylic acid and adipic acid; The molar ratio of the soluble metal salt to the organic small molecule complexing agent is 1:1 to 10; The temperature of the second calcination is 350-600° C., and the heat preservation time is 3-10 hours.
7. The preparation method according to claim 1 or 3, characterized in that: The mass ratio of the ZSM-5 molecular sieve supported Pt catalyst to the metal oxide is 1:0.1-3; The reduction treatment is carried out in a reducing atmosphere, the temperature of the reduction treatment is 300 to 600° C., and the time is 1 to 10 hours.
8. The high olefin selectivity C5-C10 alkane dehydrogenation catalyst prepared by the preparation method according to any one of claims 1 to 7, comprising a ZSM-5 molecular sieve supported Pt catalyst and a metal oxide coupled with the ZSM-5 molecular sieve supported Pt catalyst; the metal element in the metal oxide comprises one or more of Mn, Fe, La, Ga, Sn, In, Cu and Zn; The ZSM-5 molecular sieve loaded Pt catalyst comprises a ZSM-5 molecular sieve and an active component loaded on the surface and internal pores of the ZSM-5 molecular sieve. The ZSM-5 molecular sieve has a hollow structure, and the active component comprises platinum.
9. The high olefin selectivity C5-C10 alkane dehydrogenation catalyst according to claim 8, characterized in that: The active component also includes an auxiliary metal, and the auxiliary metal element is one or more of Mn, Fe, La, Ga, Sn, In, Cu and Zn.
10. Use of the high olefin selectivity C5-C10 alkane dehydrogenation catalyst according to claim 8 or 9 in catalyzing the dehydrogenation of C5-C10 alkanes to produce monoolefins.
Citation Information
Patent Citations
Catalyst used for preparing low-carbon olefin through low-carbon alkane dehydrogenation and using method thereof
CN105363443A
Metal modified ZSM-5 molecular sieve catalyst, preparation method and applications thereof
CN109663613A
Dehydrogenation catalyst as well as preparation method and application thereof
CN113908880A
C5-C10 alkane dehydrogenation catalyst as well as preparation method and application thereof
CN114749206A
Pt-based catalyst for preparing propylene through low-temperature dehydrogenation of propane and preparation method of Pt-based catalyst
CN116673065A
Cited By
Catalyst for inhibiting dehydrogenation isomerization of n-butane as well as preparation method and application of catalyst
CN119565601A
Low-carbon alkane dehydrogenation catalyst as well as preparation method and application thereof
CN121927664A