Method for sorting non-ferrous metal sulfide ore by using high-calcium waste residue emulsion

By using high-calcium waste residue emulsion to replace lime in the non-ferrous metal sulfide ore ore dressing process, the high carbon emission and pollution problems caused by the use of lime are solved, the concentrate grade and recovery rate are improved, and the effective utilization and environmental protection of calcium carbide slag is achieved.

CN118874688APending Publication Date: 2024-11-01INST OF MULTIPURPOSE UTILIZATION OF MINERAL RESOURCES CHINESE ACAD OF GEOLOGICAL SCI
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410754443.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The use of lime in the existing non-ferrous metal sulfide ore ore treatment process leads to high carbon emission intensity, high energy consumption, serious pollution, and difficulty in effectively recycling low-grade sulfur concentrate, and the problem of storage and utilization of calcium carbide slag has not been effectively solved.

Method used

High-calcium waste residue emulsion is used to replace quicklime, limestone, ripe lime, lime milk and calcium hydroxide, and is used for grinding, flotation, coagulation settlement, pressure filtration, regeneration purification and wastewater neutralization of non-ferrous metal sulfide ore to prepare calcium carbide residue emulsion And pretreatment is performed to remove impurities for use in the entire sorting process.

Benefits of technology

Reduced limestone resource consumption and carbon dioxide emissions, reduced energy consumption and dust emissions, improved concentrate grade and recovery rate, simplified operation, solved the storage and environmental pollution problems of calcium carbide slag, and achieved the green improvement of non-ferrous metal sulfide ore Quality and waste resource utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874688A_ABST
    Figure CN118874688A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of resource beneficiation, and provides a method for separating non-ferrous metal sulfide ore by using high-calcium waste residue emulsion, and the separation comprises the steps of ore grinding, flotation, coagulating sedimentation, filter pressing, regeneration purification and wastewater neutralization. The method comprises the following steps: replacing at least one of quick lime, limestone, slaked lime, lime milk and calcium hydroxide with a high-calcium waste residue emulsion for at least one of ore grinding, flotation, coagulating sedimentation, filter pressing, regeneration purification and wastewater neutralization, and the high-calcium waste residue emulsion comprises carbide slag emulsion. The method provided by the invention solves the problems of difficult storage of the carbide slag, environmental pollution, difficult comprehensive utilization and the like, reduces the carbon emission intensity of separation of the non-ferrous metal sulfide ore, also greatly reduces the consumption of lime, accords with the national advocated requirements of mineral resource conservation and comprehensive utilization policies, is a specific embodiment of developing low-carbon mineral products, and has a wide application prospect. And green quality improvement and waste resource utilization of the non-ferrous metal sulfide ore are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of resource-based mineral processing, for example, to a method for using high-calcium waste slag emulsion to separate non-ferrous metal sulfide ores. Background Art

[0002] As an important chemical raw material, calcium carbide is widely used in the production of polyvinyl chloride (PVC), vinylon, lime nitrogen, dicyandiamide, carbon black, dissolved acetylene and other products. The storage of waste calcium carbide slag produced by chemical plants not only occupies land and is very expensive, but also has a serious adverse impact on the surrounding environment, especially groundwater and surrounding villages if the anti-seepage and dust prevention treatment is not good. Therefore, it is a major safety hazard point and major source of danger in chemical production. Therefore, the storage of calcium carbide slag has always been a problem that plagues chemical plants, and how to recycle it is imminent.

[0003] In the acetylene process of producing PVC, acetylene is produced from calcium carbide, and a large amount of by-product carbide slag is discharged, whether it is a wet process or a dry process (wet process slag slurry generally contains 85% to 95% water, and dry process slag slurry generally contains 3% to 6% water). Every ton of PVC produced consumes about 1.8 tons of calcium carbide, and about 14 tons of carbide slag containing about 85% water can be discharged. At present, a large amount of calcium carbide slag is used as part of the raw materials for cement production in China, and some manufacturers use it as a substitute for building materials to make comprehensive use of waste slag, thereby achieving the purpose of turning waste into treasure. However, more and better ways have not yet been found for how to deal with a large amount of calcium carbide slag. As a large-scale industrial solid waste, calcium carbide slag urgently needs to replace primary minerals with waste to generate circular economic benefits of comprehensive resource utilization.

[0004] Lime is widely used in the beneficiation process of non-ferrous metal sulfide ores, especially in flotation operations, where it can be used as an adjuster, inhibitor, coagulant, activator, and mud dispersant. In addition, lime can also be used in combination with other agents in a certain proportion, with the characteristics of low cost and easy availability. In this regard, the main domestic users include Jiangxi Copper Co., Ltd., Northern Copper Co., Ltd., Zhongjin Lingnan Fankou Lead-Zinc Mine, Zijin Mining Group Co., Ltd., Chifeng Yuntong Nonferrous Metals Co., Ltd., Tongling Nonferrous Metals Co., Ltd., and Lala Copper Mine.

[0005] Lime used in the beneficiation of non-ferrous metal sulfide ores mainly includes limestone as the main raw material, calcined at a temperature lower than the sintering temperature to form block and powder lime and milky lime formed by reacting with water. However, the carbon emission intensity of the entire production process is high, the energy consumption is high, and the air pollution is serious. With the expansion of the beneficiation production scale of non-ferrous metal sulfide ores, the amount of lime used has gradually increased, resulting in a significant change in the demand for lime substitution by the user unit. At the same time, with the increase in social attention to low-carbon resources, the requirements for the green supply chain of mineral raw materials have also been further improved; at the same time, with the decline of the mining steps of non-ferrous metal sulfide mines, the grade of sulfur in medium and deep deposits has also increased year by year. If the existing lime priority flotation process is still used for production, the recovery rate and grade of sulfur concentrate are low and the sulfur content in tailings is high. The problem cannot be solved, and the enterprise's requirements for resource utilization and reduction of tailings cannot be met; in addition, due to the increase of copper pyrite in the raw ore of medium and deep nickel-cobalt-copper deposits in the future, the grade and recovery rate of nickel-cobalt-copper concentrate will also be affected.

[0006] In summary, non-ferrous metal sulfide ores still face process problems and potential tailings environmental hazards that need to be addressed. Summary of the invention

[0007] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a method for using high-calcium waste slag emulsion for the separation of non-ferrous metal sulfide ores.

[0008] The purpose of this disclosure is achieved through the following technical solutions:

[0009] On the one hand, a method for using high-calcium waste residue emulsion for sorting non-ferrous metal sulfide ores is provided. The sorting includes grinding, flotation, coagulation sedimentation, filter pressing, regeneration purification and wastewater neutralization. The method includes: using the high-calcium waste residue emulsion to replace at least one of quicklime, limestone, slaked lime, lime milk and calcium hydroxide for at least one of the grinding, flotation, coagulation sedimentation, filter pressing, regeneration purification and wastewater neutralization, wherein the high-calcium waste residue emulsion includes carbide slag emulsion.

[0010] It should be understood that limestone (CaCO3) is calcined under high temperature conditions to decompose into quicklime (CaO) and carbon dioxide. Quicklime easily absorbs water to become slaked lime (Ca(OH)2). Slaked lime is a white powdery substance that is not easily soluble in water. Therefore, in flotation operations, quicklime is usually added directly or lime milk is prepared by mixing it with water. Calcium hydroxide (Ca(OH)2) is a strong base that is completely ionized when dissolved in water, making the solution strongly alkaline.

[0011] In some embodiments, the non-ferrous metal sulfide ore includes a copper-containing sulfide ore.

[0012] It should be noted that cobalt is often associated in small amounts in copper sulfide ores, especially copper and nickel sulfide ores.

[0013] On this basis, in some embodiments, the copper-containing sulfide ore includes nickel-cobalt-containing copper sulfide ore.

[0014] In some embodiments, the method for preparing the carbide slag emulsion includes: pretreating carbide slag to obtain the carbide slag emulsion; wherein the particle size of the carbide slag emulsion is -0.074mm; in the carbide slag emulsion, the mass percentage of iron is less than or equal to 0.1%, and the mass percentage of calcium hydroxide is 20% to 36%.

[0015] In some embodiments, in the carbide slag, the water content is 23% to 55%, and the mass percentage of calcium hydroxide is greater than or equal to 40%.

[0016] In some examples, the carbide slag includes carbide slag which is a byproduct of producing polyvinyl chloride (PVC) by the acetylene process.

[0017] In some examples, in the carbide slag, the mass percentage of calcium carbonate in the total calcium is less than 10%.

[0018] In some embodiments, the pretreatment includes removing at least one of large particles of carbide slag and ferrosilicon particles.

[0019] In some examples, the pretreatment includes at least one of screening and high gradient magnetic separation.

[0020] In some of the above examples, the screening is used to remove the large particles of carbide slag to avoid blockage in the liquid transmission, and the high gradient magnetic separation is used to remove the ferrosilicon particles to reduce the wear and consumption of the transmission material; wherein, the screening can, for example, be through a 100-200 mesh sieve, and the magnetic field strength of the high gradient magnetic separation can, for example, be 0.3-1.8T.

[0021] In some examples, the carbide slag milk is subjected to cyclone classification to obtain underflow slurry and overflow slurry; wherein the underflow slurry is used for the grinding, and the overflow slurry is used for at least one of the flotation, the coagulation sedimentation, the filter press, the regeneration purification and the wastewater neutralization.

[0022] Exemplarily, before the underflow slurry is used for the ore grinding, the underflow slurry is prepared into a high-concentration carbide slag emulsion with a mass percentage of 20% to 60% of calcium hydroxide using warm water.

[0023] Exemplarily, before the overflow slurry is used for at least one of the flotation, the coagulation and sedimentation, the filter press, the regeneration and purification, and the wastewater neutralization, the overflow slurry is prepared into a low-concentration carbide slag milk with a mass percentage of 3% to 15% of calcium hydroxide using warm water.

[0024] It should be noted that the warm water may include, for example, at least one of production sedimentation return water in the separation, mining tailings yard return water in the separation, warmed surface water and warmed groundwater.

[0025] In some embodiments, the grinding comprises primary grinding.

[0026] In some embodiments, when the carbide slag milk is used for the ore grinding, the carbide slag milk is subjected to the ore grinding with the mineral.

[0027] It should be noted that, in the primary grinding, the mineral may be a crushed mineral obtained by crushing the original ore, or may be a coarse concentrate obtained by preliminary sorting of the original ore.

[0028] Exemplarily, in the primary grinding, the amount of carbide slag milk is expressed as 0.3 to 42 kg / t·dry weight of ore on a dry basis.

[0029] In some embodiments, when the carbide slag milk is used for the flotation, the flotation agent, the carbide slag milk and the ore pulp obtained by the primary grinding are subjected to the flotation; wherein the flotation agent includes dimethyl sulfoxide and amyl xanthate.

[0030] In some examples, the amount of dimethyl sulfoxide used is 30-100 g / t·dry weight of ore, and the amount of amyl xanthate used is 100-200 g / t·dry weight of ore.

[0031] In some embodiments, at least part of the flotation pulp obtained by the flotation is concentrated to obtain concentrated water and concentrated pulp respectively; wherein the flotation pulp includes concentrate pulp and tailings pulp. In the case where the carbide slag milk is used for the coagulation and sedimentation, the carbide slag milk and the concentrated water are subjected to the coagulation and sedimentation to precipitate heavy metal ions; and / or, in the case where the carbide slag milk is used for the filter press, the carbide slag milk and at least part of the concentrated pulp are subjected to the filter press.

[0032] In some examples, when the non-ferrous metal sulfide ore is the copper-containing sulfide ore, the concentrate slurry includes copper concentrate slurry and sulphur concentrate slurry.

[0033] In this case, the sources of the concentrate slurry and the tailings slurry include: the slurry obtained by the primary grinding is subjected to the first flotation to obtain copper tailings slurry and a higher-grade mixed concentrate slurry, the mixed concentrate slurry is subjected to the second flotation to obtain the copper concentrate slurry, and the copper tailings slurry is subjected to the third flotation to obtain the sulfur concentrate slurry and the tailings slurry.

[0034] Exemplarily, the grinding further comprises regrinding before the second flotation.

[0035] For example, in the regrinding, the amount of carbide slag milk is expressed as 0.3-20 kg / t·dry weight of ore on a dry basis.

[0036] Exemplarily, in the case where the copper-containing sulfide ore is the nickel-cobalt-containing copper sulfide ore, the concentrate slurry also includes nickel-cobalt concentrate slurry.

[0037] In this case, the mixed concentrate slurry is subjected to the second flotation to obtain the nickel-cobalt concentrate slurry.

[0038] It should be understood that the nickel-cobalt concentrate slurry can be further sorted to obtain nickel concentrate slurry and cobalt concentrate slurry.

[0039] It should be noted that each type of slurry in at least a part of the flotation slurry is independently concentrated to obtain concentrated water and concentrated slurry corresponding to each other; wherein the concentrated water is obtained by merging the concentrated water corresponding to each type of slurry, and the concentrated slurry is the concentrated slurry corresponding to each independent slurry (that is, the concentrated slurry corresponding to each type of slurry does not need to be merged).

[0040] In addition, it should be noted that each type of slurry in at least a portion of the concentrated slurry is independently subjected to the filter press with the carbide slag milk to obtain the corresponding filter press water and minerals; wherein the filter press water corresponding to each slurry is combined to obtain the filter press water obtained by the filter press.

[0041] For example, in the case where at least part of the flotation slurry includes the copper concentrate slurry and the sulfur concentrate slurry, the copper concentrate slurry is concentrated to obtain copper concentrate concentrated water and copper concentrate concentrated slurry, and the sulfur concentrate slurry is concentrated to obtain sulfur concentrate concentrated water and sulfur concentrate concentrated slurry; wherein the concentrated water is obtained by combining the copper concentrate concentrated water and the sulfur concentrate concentrated water, and the concentrated slurries are the respectively independent copper concentrate concentrated slurry and the sulfur concentrate concentrated slurry.

[0042] On this basis, the carbide slag milk and the concentrated water are subjected to the coagulation sedimentation to precipitate heavy metal ions, the copper concentrate concentrated slurry and the carbide slag milk are subjected to the filter pressing to obtain copper concentrate and copper concentrate filter press water, and the sulfur concentrate concentrated slurry and the carbide slag milk are subjected to the filter pressing to obtain sulfur concentrate and sulfur concentrate filter press water; wherein the copper concentrate filter press water and the sulfur concentrate filter press water are combined to obtain the filter press water obtained by the filter pressing.

[0043] In some examples, when at least a portion of the concentrated slurry includes tailings concentrated slurry obtained by the concentration of the tailings slurry, the carbide slag emulsion and the tailings concentrated slurry are subjected to the filter pressing.

[0044] In this case, the carbide slag emulsion can promote the sludge in the tailings concentrated slurry to agglomerate into larger aggregates.

[0045] In some embodiments, when the carbide slag emulsion is used for the regeneration and purification, an inorganic polymer flocculant, the carbide slag emulsion and the filter press water obtained by the filter press are subjected to the regeneration and purification.

[0046] In some examples, the inorganic polymeric flocculant includes polymeric ferric sulfate.

[0047] In some examples, in the regeneration purification, the amount of the carbide slag milk is 0.5% to 1.3% of the mass of the filter press slurry.

[0048] Exemplarily, the reclaimed water obtained through the regeneration and purification is reused as production water.

[0049] In some embodiments, when the carbide slag milk is used for neutralizing the wastewater, the carbide slag milk is treated with acidic wastewater to neutralize the wastewater.

[0050] In some examples, the consumption of calcium hydroxide in the neutralization of the carbide slag emulsion in the wastewater is maintained at 105% to 120% of the molar mass of the acidic medium.

[0051] In some examples, the acidic wastewater includes acidic cleaning wastewater generated during maintenance and / or cleaning of equipment performed during the separation.

[0052] It should be understood that carbide slag has fewer impurities and more flotation-use components. Compared with lime (e.g., lime milk) used for the beneficiation of non-ferrous metal sulfide ores, it has coarse particle size, more high-hardness minerals such as ferrosilicon, and more large-particle coke. There are few processes and equipment for the direct replacement of lime by carbide slag milk for the beneficiation of non-ferrous metal sulfide ores (especially nickel-cobalt-copper sulfide ores) at home and abroad. In this regard, patent CN117599960A reported the use of carbide slag as a slurry regulator for the flotation of nickel-cobalt-copper sulfide ores, and the document "Experimental Study on the Use of Carbide Slag as a Depressant for Copper-Sulfur Flotation Separation" reported that the copper grade and yield obtained by replacing lime as a depressant for pyrite with carbide slag were equivalent to those of lime. However, the above documents are for copper-pyrite ores and are not applicable to nickel-cobalt copper sulfide ores, and the above patents and documents only use carbide slag for flotation, while the method provided by the present disclosure can use carbide slag milk instead of lime for the entire process of sorting non-ferrous metal sulfide ores (grinding, flotation, coagulation and sedimentation, filter pressing, regeneration and purification, and neutralization of wastewater) to achieve an effect superior to lime. Therefore, the above patents and documents cannot bring technical inspiration to the method provided by the present disclosure.

[0053] It should be emphasized that the use of carbide slag to replace lime has many advantages in the field of non-ferrous metal sulfide ore beneficiation: First, it can replace limestone raw materials in a large proportion, reduce the consumption of limestone resources and the emission of carbon dioxide gas. Reducing the use of each ton of quicklime can save 1.8 tons of limestone resources and reduce the emission of 0.79 tons of carbon dioxide gas. Second, it can greatly reduce the purchase cost of raw materials, energy consumption and dust emissions at the production site. The heat consumption of preparing carbide slag milk is lower than that of preparing lime milk with limestone as raw material, which is convenient for precise control of slurry pH and slurry ORP to greatly improve the physical separation efficiency of non-ferrous metal sulfide ores, and the broad-spectrum coupling with green beneficiation agents can ensure the stable production of beneficiation manufacturers. Third, the production process is becoming more mature, advanced and environmentally friendly, which can greatly reduce dust emissions and labor intensity at the production site, with obvious competitive advantages, which is conducive to improving the high-value comprehensive utilization level of non-ferrous metal sulfide ores (for example, difficult-to-smelt and low-grade nickel, cobalt and copper sulfide ores).

[0054] It is worth noting that the method provided by the present disclosure uses carbide slag milk to replace at least one of quicklime, limestone, slaked lime, lime milk and calcium hydroxide for at least one of grinding, flotation, coagulation sedimentation, filter pressing, regeneration purification and wastewater neutralization. Among them, carbide slag milk (for example, high-concentration carbide slag milk) has a stable effect in the process of grinding, does not affect the normal production of concentrate, and does not destroy the properties of the concentrate itself; at the same time, carbide slag milk (for example, low-concentration carbide slag milk) can not only finely adjust the pH and ORP of the pulp during flotation, but also activate the minerals, thereby improving the grade of the resulting concentrate; in addition, the amount of carbide slag milk added in flotation, coagulation sedimentation, filter pressing, regeneration purification and wastewater neutralization is basically the same as the theoretical amount of lime added, the indicators meet the production requirements, and the liquid-passing capacity of concentrate, tailings and sludge is improved. On the one hand, the problems of carbide slag storage difficulty, environmental pollution and comprehensive utilization difficulty are solved, and on the other hand, the carbon emission intensity of the entire sorting is reduced, and the consumption of lime raw materials is greatly reduced. Therefore, the method provided by the present invention complies with the policy requirements of mineral resource conservation and comprehensive utilization advocated by the state, is a concrete manifestation of the development of low-carbon mineral products, and realizes the green quality improvement of non-ferrous metal sulfide ores and waste resource utilization.

[0055] The beneficial effects of the present disclosure are:

[0056] 1. The carbide slag milk used in the method provided by the present invention contains a large amount of Ca(OH)2, which has a fine particle size and a concentration close to that of lime milk; when used, it only needs to be slightly diluted and emulsified, which shortens the digestion time and simplifies the operation process.

[0057] 2. The carbide slag milk used in the method provided by the present invention contains fewer impurities, more beneficial components, fine particle size, and does not require special equipment for emulsification, thus avoiding the problems existing in the preparation and addition of lime milk.

[0058] 3. The method provided by the present disclosure does not affect the normal production of the concentrate and does not destroy the properties of the concentrate itself when calcium carbide slag milk is used to replace at least one of quicklime, limestone, slaked lime, lime milk and calcium hydroxide for grinding.

[0059] 4. The method provided by the present invention can not only finely adjust the pH and ORP of the slurry, but also activate the minerals when carbide slag milk is used to replace at least one of quicklime, limestone, slaked lime, lime milk and calcium hydroxide for flotation. At the same time, the method is used in combination with high-efficiency flotation reagents such as dimethyl sulfoxide and amyl xanthate to obtain a stable flotation separation effect under weakly alkaline conditions, with excellent sorting indicators, and is a relatively ideal comprehensive recovery method.

[0060] 5. The amount of calcium carbide slag emulsion provided by the present invention added in flotation, coagulation sedimentation, filter press, regeneration purification and wastewater neutralization is basically the same as the theoretical amount of lime added, and the indicators meet the production requirements. It improves the liquid passing capacity of concentrate, tailings and sludge, and on the one hand solves the problems of difficult storage of calcium carbide slag, environmental pollution and difficulty in comprehensive utilization. On the other hand, it reduces the carbon emission intensity of the entire sorting, and also greatly reduces the consumption of lime raw materials.

[0061] 6. The method provided by the present invention is stable and reliable, and can solve the problems of large amount of lime used in traditional methods, which affects the recovery of associated precious metals and easily forms scale on the inner wall of slurry storage equipment and transportation pipelines.

[0062] 7. The method disclosed herein complies with the national policy requirements for conservation and comprehensive utilization of mineral resources, is a concrete manifestation of the development of low-carbon mineral products, and realizes the green quality improvement of non-ferrous metal sulfide ores and the resource utilization of waste. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] In order to more clearly illustrate the technical solutions in the present disclosure, the following briefly introduces the drawings required to be used in some embodiments of the present disclosure. Obviously, the drawings described below are only drawings of some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can also be obtained based on these drawings. In addition, the drawings described below can be regarded as schematic diagrams, and are not limitations on the actual process of the method involved in the embodiments of the present disclosure.

[0064] Figure 1 A method for separating nonferrous metal sulfide ores provided in an embodiment of the present disclosure;

[0065] Figure 2 The invention discloses a method for separating nonferrous metal sulfide ores provided by the prior art. DETAILED DESCRIPTION

[0066] The technical solutions in some embodiments of the present disclosure are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments provided by the present disclosure, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present disclosure.

[0067] When describing some embodiments, the expression "A and / or B" may be used. It is easy to understand that "A and / or B" includes the following three combinations: only A, only B, and a combination of A and B.

[0068] When describing some embodiments, the expressions "at least one of A, B and C" and "at least one of A, B or C" may be used, both of which have the same meaning and include the following combinations of A, B and C: A only, B only, C only, the combination of A and B, the combination of A and C, the combination of B and C, and the combination of A, B and C.

[0069] It should be noted that when describing some embodiments, the expression "percentage (%)" may be used. It is easy to understand that the "percentage (%)" involved in the embodiments of the present disclosure refers to mass percentage.

[0070] Example 1

[0071] A nickel-cobalt-copper rough concentrate (Cu 3.60%, Ni 7.91%, Co 0.31%) in Panxi, Sichuan was taken as the research object. The nickel-cobalt-copper rough concentrate was obtained by preliminary sorting of nickel-cobalt-copper sulfide ore. Carbide slag was used for sorting the nickel-cobalt-copper rough concentrate, which included the following steps:

[0072] S1. Carbide slag (water content 43.2%, effective calcium hydroxide 51.8%) from a certain place in Sichuan is sent to a pulping tank, washed with a high-pressure water gun and then screened. The slurry after screening is subjected to 1.2T high-gradient magnetic separation to obtain carbide slag milk (Fe≤0.1%, -0.074mm≥100%, calcium hydroxide 31.5%) and ferrosilicon magnetic products with a concentration of 4.36%; the carbide slag milk is subjected to cyclone classification to obtain underflow slurry and overflow slurry, and the underflow slurry and overflow slurry are respectively prepared with warm water to obtain high-concentration carbide slag milk (calcium hydroxide 42%) and low-concentration carbide slag milk (calcium hydroxide 7%);

[0073] S2. High-concentration carbide slag milk is sent to the carbide slag milk buffer tank through a slurry pump and then to the grinding process; low-concentration carbide slag milk is sent to the dosing points for flotation, coagulation sedimentation, filter press, regeneration purification and wastewater neutralization, and low-concentration carbide slag milk is added to each dosing point by a metering pump according to production needs;

[0074] S3. The coarse concentrate and high-concentration carbide slag milk are put into the raw material mill for wet grinding and pulping. The amount of high-concentration carbide slag milk is expressed as the amount of carbide slag added on a dry basis of 0.8kg / t· dry ore to form a pH of 10.8 qualified pulp for flotation process;

[0075] S4. The slurry obtained in S3 is put into the pre-flotation buffer stirring tank together with low-concentration carbide slag milk (50 g / t· ore dry weight) and flotation reagents (dimethyl sulfoxide and amyl xanthate, with amounts of 50 g / t· ore dry weight and 150 g / t· ore dry weight, respectively) to complete the de-drug pretreatment;

[0076] S5. After the ore pulp is subjected to multiple flotation processes, a concentrate slurry and a tailings slurry are obtained; wherein the concentrate slurry is a high-grade copper concentrate slurry (copper grade 27.8%, copper recovery rate 85.12%), a nickel concentrate slurry (nickel grade 9.95%, nickel recovery rate 90.56%) and a cobalt concentrate slurry (cobalt grade 0.61%, cobalt recovery rate 61.43%); the copper concentrate slurry is concentrated to obtain copper concentrate concentrated water and copper concentrate concentrated slurry; the nickel concentrate slurry is concentrated to obtain nickel concentrate concentrated water and nickel concentrate concentrated slurry; the cobalt concentrate slurry is concentrated to obtain cobalt concentrate concentrated water and cobalt concentrate concentrated slurry; the tailings slurry is concentrated to obtain tailings concentrated water and tailings concentrated slurry; wherein the copper concentrate concentrated water, the nickel concentrate concentrated water, the cobalt concentrate concentrated water and the tailings concentrated water are combined into concentrated water;

[0077] S6. Concentrated water at 1.2kg / M 3 Add low-concentration carbide slag milk and stir to perform coagulation and sedimentation for 30 minutes to precipitate harmful heavy metal ions in the slurry;

[0078] S7. The copper concentrate slurry is concentrated and filtered to obtain copper concentrate and copper concentrate concentrated filter water; the nickel concentrate slurry is concentrated and filtered to obtain nickel concentrate and nickel concentrate concentrated filter water; the cobalt concentrate slurry is concentrated and filtered to obtain cobalt concentrate and cobalt concentrate concentrated filter water; the tailings concentrated slurry is concentrated and filtered to obtain 50kg / M 3 The tailings and tailings concentrated filter press water were obtained by adding low-concentration carbide slag milk and stirring for 15 minutes to promote the tailings mud to coagulate into larger aggregates, and then concentrated filter press water was obtained. It should be noted that compared with the case where the tailings were not added with carbide slag milk, the time required for concentrated filter press water with the addition of low-concentration carbide slag milk was shortened by 1 / 3; wherein, the concentrated filter press water of copper concentrate, the concentrated filter press water of nickel concentrate, the concentrated filter press water of cobalt concentrate and the concentrated filter press water of tailings were combined into concentrated filter press water;

[0079] S8. Concentrated filter water at 11kg / M 3 Add low-concentration carbide slag emulsion and polyferric sulfate for precipitation, drug removal, regeneration and purification, remove heavy metals and mineral processing agents and other harmful substances in concentrated filter press water to make them enter the sludge, and reuse the purified water as production water;

[0080] S9. The pH of the acidic cleaning wastewater generated during equipment maintenance is 0.5, and the pH value is 328 kg / M 3 Low-concentration carbide slag emulsion is added for neutralization, and the neutralized wastewater is discharged in compliance with the standards.

[0081] Example 2

[0082] A copper-containing sulfide ore (Cu 0.737%, S11.40%) in western Sichuan was taken as the research object, and carbide slag emulsion was used for the separation of the copper-containing sulfide ore, including the following steps:

[0083] S1. Carbide slag (water content 53.8%, effective calcium hydroxide 42.5%) from a certain place in Sichuan is sent to a pulping tank, washed with a high-pressure water gun and then screened. The slurry after screening is subjected to 1.5T high-gradient magnetic separation to obtain carbide slag emulsion (Fe≤0.1%, -0.074mm≥100%, calcium hydroxide 20.3%) and ferrosilicon magnetic product with a concentration of 5.75%; the carbide slag emulsion is subjected to cyclone classification to obtain underflow slurry and overflow slurry, and the underflow slurry and overflow slurry are respectively prepared with warm water to obtain high-concentration carbide slag emulsion (calcium hydroxide 28.7%) and low-concentration carbide slag emulsion (calcium hydroxide 4.7%);

[0084] S2. High-concentration carbide slag milk is sent to the carbide slag milk buffer tank through a slurry pump, part of which is sent to the primary grinding process and part to the regrinding process; low-concentration carbide slag milk is sent to the dosing points of flotation, coagulation sedimentation, filter press, regeneration purification and wastewater neutralization production operations, and low-concentration carbide slag milk is added to each dosing point by digital control using a metering pump according to production needs;

[0085] S3. The crushed ore and high-concentration carbide slag milk are fed into the raw mill together with wet grinding pulping (primary grinding), the amount of high-concentration carbide slag milk is expressed as the amount of carbide slag added on a dry basis is 41.44kg / t· ore dry weight, and a pH of 12.1 is prepared to be a qualified slurry for flotation process, and the mixed concentrate obtained by flotation and the high-concentration carbide slag milk are fed into the raw mill with wet grinding pulping (regrinding), the amount of high-concentration carbide slag milk is expressed as the amount of carbide slag added on a dry basis is 9.21kg / t· ore dry weight, and a pH of 11.2 is prepared to be a qualified slurry for flotation process;

[0086] S4. The slurry obtained in S3 is put into the pre-flotation buffer stirring tank together with low-concentration carbide slag emulsion (180 g / t· ore dry weight) and flotation reagents (dimethyl sulfoxide and amyl xanthate, with the dosages of 100 g / t· ore dry weight and 200 g / t· ore dry weight, respectively) to complete the de-drug pretreatment;

[0087] S5. After the two slurries are subjected to multiple flotation processes, concentrate slurry and tailings slurry (copper grade 0.14%, sulfur grade 2.6%, copper recovery rate 17.12%) are obtained; wherein, the concentrate slurry is high-grade copper concentrate slurry (copper grade 20.71%, sulfur grade 30.23%, copper recovery rate 80.1%) and sulfur concentrate slurry (copper grade 0.21%, sulfur grade 36.16%, copper recovery rate 2.78%); the copper concentrate slurry is concentrated to obtain copper concentrate concentrated water and copper concentrate concentrated slurry; the sulfur concentrate slurry is concentrated to obtain sulfur concentrate concentrated water and sulfur concentrate concentrated slurry; the tailings slurry is concentrated to obtain tailings concentrated water and tailings concentrated slurry; wherein, the copper concentrate concentrated water, the sulfur concentrate concentrated water and the tailings concentrated water are combined into concentrated water;

[0088] S6. Concentrated water at 2.8kg / M 3Add low-concentration carbide slag milk and stir to perform coagulation and sedimentation for 30 minutes to precipitate harmful heavy metal ions in the slurry;

[0089] S7. The concentrated slurry of copper concentrate is concentrated and filtered to obtain copper concentrate and concentrated filter water of copper concentrate; the concentrated slurry of sulfur concentrate is concentrated and filtered to obtain sulfur concentrate and concentrated filter water of sulfur concentrate; the concentrated slurry of tailings is concentrated and filtered to obtain sulfur concentrate and concentrated filter water of sulfur concentrate; 3 The tailings and tailings concentrated filter press water were obtained by adding low-concentration carbide slag milk and stirring for 15 minutes to promote the tailings mud to coagulate into larger aggregates, and then concentrated filter press water was obtained. It should be noted that compared with the case where the tailings were not added with carbide slag milk, the concentrated filter press water with the addition of low-concentration carbide slag milk was improved; wherein, the concentrated filter press water of copper concentrate, the concentrated filter press water of sulfur concentrate and the concentrated filter press water of tailings were combined into concentrated filter press water;

[0090] S8. Concentrated filter water at 5kg / M 3 Add low-concentration carbide slag emulsion and polyferric sulfate for precipitation, drug removal, regeneration and purification, remove heavy metals and mineral processing agents and other harmful substances in concentrated filter press water to make them enter the sludge, and reuse the purified water as production water;

[0091] S9. The pH of the acidic cleaning wastewater generated during equipment maintenance is 1.5, and the pH value is 14.3 kg / M 3 Low-concentration carbide slag emulsion is added for neutralization, and the neutralized wastewater is discharged in compliance with the standards.

[0092] Example 3

[0093] A nickel-cobalt-copper rough concentrate (Cu 9.56%, Ni 11.38%, Co 0.41%) in Gansu was taken as the research object. The nickel-cobalt-copper rough concentrate was obtained by preliminary sorting of nickel-cobalt-copper sulfide ore. Carbide slag was used for sorting the nickel-cobalt-copper rough concentrate, which included the following steps:

[0094] S1. Carbide slag (water content 23.56%, effective calcium hydroxide 68.8%) from a certain place in Gansu was sent to a pulping tank, washed with a high-pressure water gun and then screened. The slurry after screening was subjected to 1.2T high-gradient magnetic separation to obtain carbide slag milk (Fe≤0.1%, -0.074mm≥100%, calcium hydroxide 35.7%) and ferrosilicon magnetic products with a concentration of 6.14%; the carbide slag milk was subjected to cyclone classification to obtain underflow slurry and overflow slurry, and the underflow slurry and overflow slurry were respectively prepared with warm water to obtain high-concentration carbide slag milk (calcium hydroxide 48%) and low-concentration carbide slag milk (calcium hydroxide 8%);

[0095] S2. High-concentration carbide slag milk is sent to the carbide slag milk buffer tank through a slurry pump and then to the grinding process; low-concentration carbide slag milk is sent to the dosing points for flotation, coagulation sedimentation, filter press, regeneration purification and wastewater neutralization, and low-concentration carbide slag milk is added to each dosing point by a metering pump according to production needs;

[0096] S3. The coarse concentrate and high-concentration carbide slag milk are put into the raw material mill for wet grinding and pulping. The amount of high-concentration carbide slag milk is expressed as the amount of carbide slag added on a dry basis of 0.8kg / t· dry ore to form a pH of 10.8 qualified pulp for flotation process;

[0097] S4. The slurry obtained in S3 is put into the pre-flotation buffer stirring tank together with low-concentration carbide slag milk (50 g / t· ore dry weight) and flotation reagents (dimethyl sulfoxide and amyl xanthate, in amounts of 30 g / t· ore dry weight and 100 g / t· ore dry weight, respectively) to complete the de-drug pretreatment;

[0098] S5. After the ore pulp is subjected to multiple flotation processes, a concentrate slurry and a tailings slurry are obtained; wherein the concentrate slurry is a high-grade copper concentrate slurry (copper grade 25.55%, copper recovery rate 80.05%), a nickel concentrate slurry (nickel grade 18.16%, nickel recovery rate 88.47%) and a cobalt concentrate slurry (cobalt grade 0.72%, cobalt recovery rate 63.23%); the copper concentrate slurry is concentrated to obtain copper concentrate concentrated water and copper concentrate concentrated slurry; the nickel concentrate slurry is concentrated to obtain nickel concentrate concentrated water and nickel concentrate concentrated slurry; the cobalt concentrate slurry is concentrated to obtain cobalt concentrate concentrated water and cobalt concentrate concentrated slurry; the tailings slurry is concentrated to obtain tailings concentrated water and tailings concentrated slurry; wherein the copper concentrate concentrated water, the nickel concentrate concentrated water, the cobalt concentrate concentrated water and the tailings concentrated water are combined into concentrated water;

[0099] S6. Concentrated water at 1.2kg / M 3 Add low-concentration carbide slag milk and stir to perform coagulation and sedimentation for 30 minutes to precipitate harmful heavy metal ions in the slurry;

[0100] S7. The copper concentrate slurry is concentrated and filtered to obtain copper concentrate and copper concentrate concentrated filter water; the nickel concentrate slurry is concentrated and filtered to obtain nickel concentrate and nickel concentrate concentrated filter water; the cobalt concentrate slurry is concentrated and filtered to obtain cobalt concentrate and cobalt concentrate concentrated filter water; the tailings concentrated slurry is concentrated and filtered to obtain 50kg / M 3 The tailings and tailings concentrated filter press water were obtained by adding low-concentration carbide slag milk and stirring for 15 minutes to promote the tailings mud to coagulate into larger aggregates, and then concentrated filter press water was obtained. It should be noted that compared with the case where the tailings were not added with carbide slag milk, the time required for concentrated filter press water with the addition of low-concentration carbide slag milk was shortened by 1 / 3; wherein, the concentrated filter press water of copper concentrate, the concentrated filter press water of nickel concentrate, the concentrated filter press water of cobalt concentrate and the concentrated filter press water of tailings were combined into concentrated filter press water;

[0101] S8. Concentrated filter water at 11kg / M 3Add low-concentration carbide slag emulsion and polyferric sulfate for precipitation, drug removal, regeneration and purification, remove heavy metals and mineral processing agents and other harmful substances in concentrated filter press water to make them enter the sludge, and reuse the purified water as production water;

[0102] S9. The pH of the acidic cleaning wastewater generated during equipment maintenance is 0.5, and the pH value is 328 kg / M 3 Low-concentration carbide slag emulsion is added for neutralization, and the neutralized wastewater is discharged in compliance with the standards.

[0103] Comparative Example 1

[0104] Comparative Example 1 and Example 1 process the same coarse concentrate, except that lime milk is used to replace carbide slag milk in grinding and flotation in Comparative Example 1. Specifically, in Comparative Example 1, lime milk and warm water are prepared to obtain 42% high-concentration lime milk and 7% low-concentration lime milk; in step S3, the amount of high-concentration lime milk is 0.8 kg / t·dry weight of ore on a dry basis, and a qualified ore pulp with a pH of 10.8 is prepared and sent to the flotation process; in step S4, the amount of low-concentration lime milk is 50 g / t·dry weight of ore, and dimethyl sulfoxide and amyl xanthate are used as flotation reagents, and the amounts are 50 g / t·dry weight of ore and 150 g / t·dry weight of ore, respectively.

[0105] Comparative Example 2

[0106] Comparative Example 2 and Example 2 process the same ore, except that lime milk is used instead of carbide slag milk for grinding and flotation in Comparative Example 2. Specifically, in Comparative Example 2, lime milk and warm water are prepared to obtain 28.7% high-concentration lime milk and 4.7% low-concentration lime milk; in step S3, the crushed raw ore and the high-concentration lime milk are fed into the raw mill for wet grinding and pulping (primary grinding), the amount of lime milk is 41.44 kg / t·dry ore on a dry basis, and the slurry with a pH of 12.1 is prepared and sent to the flotation process; the mixed concentrate obtained by flotation and the high-concentration lime milk are fed into the raw mill for wet grinding and pulping (re-grinding), the amount of high-concentration lime milk is 9.21 kg / t·dry ore on a dry basis, and the slurry with a pH of 11.2 is prepared and sent to the flotation process; in step S4, the amount of low-concentration lime milk is 180 g / t·dry ore, and the flotation reagents are dimethyl sulfoxide and amyl xanthate, and the amounts are 100 g / t·dry ore and 200 g / t·dry ore, respectively.

[0107] Comparative Example 3

[0108] Comparative Example 3 and Example 3 process the same concentrate, except that lime milk is used instead of carbide slag milk in grinding and flotation in Comparative Example 3. Specifically, in Comparative Example 3, lime milk and warm water are prepared to obtain 48% high-concentration lime milk and 8% low-concentration lime milk; in step S3, the amount of high-concentration lime milk is 0.8 kg / t·dry weight of ore on a dry basis, and a qualified ore pulp with a pH of 10.8 is prepared and sent to the flotation process; in step S4, the amount of low-concentration lime milk is 50 g / t·dry weight of ore, and the flotation reagents are dimethyl sulfoxide and amyl xanthate, and the amounts are 30 g / t·dry weight of ore and 100 g / t·dry weight of ore, respectively.

[0109] Comparative Example 4

[0110] Comparative Example 4 and Example 1 process the same coarse concentrate, except that lime milk is used instead of carbide slag milk in coagulation sedimentation, filter pressing, regeneration purification and wastewater neutralization in Comparative Example 4. Specifically, the 7% low-concentration carbide slag milk in steps S6 to S9 is replaced by 7% low-concentration lime milk.

[0111] Comparative Example 5

[0112] Comparative Example 5 and Example 2 process the same coarse concentrate, except that lime milk is used instead of carbide slag milk in coagulation sedimentation, filter pressing, regeneration purification and wastewater neutralization in Comparative Example 5. Specifically, the 4.7% low-concentration carbide slag milk in steps S6 to S9 is replaced by 4.7% low-concentration lime milk.

[0113] Comparative Example 6

[0114] Comparative Example 6 and Example 3 process the same coarse concentrate, except that lime milk is used instead of carbide slag milk in coagulation sedimentation, filter pressing, regeneration purification and wastewater neutralization in Comparative Example 6. Specifically, 8% of low-concentration carbide slag milk in steps S6 to S9 is replaced by 8% of low-concentration lime milk.

[0115] Experimental Example 1

[0116] In order to verify the effect of the method of using carbide slag emulsion for the separation of non-ferrous metal sulfide ores disclosed in the present invention, the grade and recovery rate of the concentrate slurries obtained in Examples 1 to 3 and Comparative Examples 1 to 3 were tested and statistically analyzed, and the results are shown in the following table:

[0117]

[0118] The results show that using carbide slag milk instead of lime milk for the separation of non-ferrous metal sulfide ores can improve the separation accuracy, thereby significantly improving the grade and recovery rate of the concentrate.

[0119] Experimental Example 2

[0120] In order to verify the effect of the method of using carbide slag emulsion for the separation of non-ferrous metal sulfide ores disclosed in the present invention, the effects of coagulation sedimentation, filter pressing, regeneration purification and wastewater neutralization in Examples 1 to 3 and Comparative Examples 4 to 6 were compared, and the results are shown in the following table:

[0121]

[0122]

[0123] The results show that the use of carbide slag milk instead of lime milk in coagulation sedimentation, filtration, regeneration purification and wastewater neutralization in the separation of non-ferrous metal sulfide ores can not only improve the removal rate of heavy metal ions in the mineral processing wastewater, but also shorten the time for concentrated filtration of tailings concentrated slurry.

[0124] Experimental Example 3

[0125] A method for separating non-ferrous metal sulfide ores using carbide slag emulsion disclosed in the present invention (such as Figure 1 ) and a prior art method for separating nonferrous metal sulfide ores using quicklime (lime) (as shown in Figure 2 The energy consumption of the two types of energy consumption (as shown) is compared, and the results are shown in the following table:

[0126]

[0127] The results show that using carbide slag milk instead of quicklime for the separation of non-ferrous metal sulfide ores can not only produce better results, but also reduce energy consumption and costs.

[0128] The above is only a preferred embodiment of the present disclosure. It should be understood that the present disclosure is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art do not deviate from the spirit and scope of the present disclosure, and should be within the scope of protection of the claims attached to the present disclosure.

Claims

1. A method for separating non-ferrous metal sulfide ores using high calcium waste slag emulsion, characterized in that: The separation includes grinding, flotation, coagulation sedimentation, filter pressing, regeneration purification and wastewater neutralization; the method includes: The high-calcium waste residue emulsion is used to replace at least one of quicklime, limestone, slaked lime, lime milk and calcium hydroxide for at least one of the grinding, flotation, coagulation and sedimentation, filter pressing, regeneration and purification and wastewater neutralization; wherein the high-calcium waste residue emulsion includes carbide slag emulsion.

2. The method according to claim 1, characterized in that The method for preparing the carbide slag milk comprises: Carbide slag is pretreated to obtain the carbide slag milk; wherein the particle size of the carbide slag milk is -0.074mm; in the carbide slag milk, the mass percentage of iron is less than or equal to 0.1%, and the mass percentage of calcium hydroxide is 20% to 36%.

3. The method according to claim 2, characterized in that The water content of the carbide slag is 23% to 55%, and the mass percentage of calcium hydroxide is greater than or equal to 40%.

4. The method according to claim 2, characterized in that: The pre-processing comprises: At least one of large particles of carbide slag and ferrosilicon particles is removed.

5. The method according to claim 1, characterized in that The grinding includes primary grinding.

6. The method according to claim 5, characterized in that In the case where the carbide slag milk is used for the ore grinding, the carbide slag milk and the mineral are subjected to the ore grinding; And / or, when the carbide slag milk is used for the flotation, the flotation agent, the carbide slag milk and the ore pulp obtained by the primary grinding are subjected to the flotation; wherein the flotation agent includes dimethyl sulfoxide and amyl xanthate.

7. The method according to claim 1, wherein at least part of the flotation pulp obtained by the flotation is concentrated to obtain concentrated water and concentrated pulp respectively; wherein: The flotation slurry includes concentrate slurry and tailings slurry; When the carbide slag milk is used for the coagulation and sedimentation, the carbide slag milk and the concentrated water are subjected to the coagulation and sedimentation to precipitate heavy metal ions; and / or, when the carbide slag milk is used for the filter press, the carbide slag milk and at least part of the concentrated slurry are subjected to the filter press.

8. The method according to claim 1 or 7, in the case where the carbide slag milk is used for the regeneration and purification, an inorganic polymer flocculant, the carbide slag milk and the filter press water obtained by the filter press are subjected to the regeneration and purification; And / or, when the carbide slag milk is used for neutralizing the wastewater, the carbide slag milk is used for neutralizing the wastewater with acidic wastewater.

9. The method according to claim 1, characterized in that: The non-ferrous metal sulfide ore includes copper-containing sulfide ore.

10. The method according to claim 9, characterized in that The copper-containing sulfide ore includes nickel-cobalt-containing copper sulfide ore.

Citation Information

Patent Citations

  • Lime milk adding method

    CN110813548A

  • Flocculating and settling process for flotation of tungsten ore tailings

    CN114308402A

  • Flotation separation reagent for waste rock containing copper and cobalt and application of flotation separation reagent

    CN117599960A