Method for using cationic surfactant for iron ore reverse flotation at normal temperature
By using cationic surfactant dodecylmorpholine and other chemicals in iron ore counterflotation, the problems of high energy consumption and large amount of agents in the prior art are solved, and low-cost and efficient iron ore recovery is achieved and green mine construction.
Patent Information
- Application Number
- CN202411157386.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-01
AI Technical Summary
The existing iron ore anti-flotation process consumes high energy and high chemical dosage, resulting in serious production costs and environmental pollution, and it is difficult to achieve the goal of low-carbon and green mines.
The cationic surfactant dodecylmorpholine is used as the collector, combined with the solution of prilandosaccharide and sodium hydroxide, and iron ore reverse flotation is performed at room temperature to reduce the amount of agent and reduce energy consumption.
It has achieved efficient iron ore anti-flotation under low agent dosage and room temperature conditions, reduced production costs and environmental pollution risks, and promoted energy conservation and emission reduction in the iron ore ore process and green mine construction.
Smart Images

Figure CN118874693A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of mineral processing and flotation, and in particular relates to a method for reverse flotation of iron ore using a cationic surfactant at room temperature. Background Art
[0002] . my country has rich reserves of iron ore resources, but due to its low average iron grade, poor endowment and difficulty in utilization, it has long relied heavily on imported iron ore. Therefore, the efficient development and utilization of low-grade and difficult-to-select iron ore has gradually become a research focus. The current main method for recovering iron resources is the combined process of stage grinding-magnetic-flotation. In the flotation stage, most concentrators use anion reverse flotation technology to improve quality and reduce impurities, so as to achieve efficient development and utilization of difficult-to-select iron ore.
[0003] At present, the anionic collectors used in the reverse flotation of iron ore in industry are mainly fatty acid collectors. Although the use of this type of collector has the advantages of stable production and good indicators, the temperature required for its configuration and flotation is relatively high (the configuration temperature is usually 50-70°C, and the pulp temperature is generally 35-40°C), which results in the need for heating the pulp during flotation, resulting in huge energy consumption. For example, patent CN106492998A proposes a collector prepared by stirring at above 80°C for 5-7h. The collector requires a lot of energy during the configuration process, thereby increasing production energy consumption and cost. In addition, this type of collector also has the problem of high flotation alkalinity and large dosage during its reuse. Among them, the suitable pH for flotation is mostly in the range of 11-12. The pulp pH of the flotation product is too high, which in turn makes it difficult to recycle the flotation wastewater; and the excessive dosage of the reagent leads to high production costs and carbon emissions in the mineral processing production process. For example, patent CN103934115A discloses a high-efficiency collector for reverse flotation of hematite, which needs to be separated at 39-41°C and pulp pH greater than 11. Although it can achieve good flotation indicators, the huge energy consumption generated by heating tons of pulp in the production process and the high pulp pH causing serious environmental pollution limit its application. With the continuous improvement of low-carbon, green and environmental protection requirements, the efficient flotation separation of difficult-to-select iron ore will face greater challenges. Therefore, finding a room-temperature high-efficiency iron ore collector is of great significance to the utilization of my country's iron ore resources, and it is the future development trend of iron ore dressing agents. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention solves the problems of high energy consumption and large dosage of reagents in the process of iron ore resource recovery, and provides a method for reverse flotation of iron ore using a cationic surfactant as a collector under normal temperature conditions. The collector used in the method can be applied to the flotation process after being configured at room temperature, and efficient reverse flotation of iron ore can be achieved at a lower dosage of reagents, and energy conservation and emission reduction in the iron ore selection process and the construction of green mines can be further promoted.
[0005] In order to solve the above technical problems, the specific technical solutions of the present invention are as follows:
[0006] A method for reverse flotation of iron ore using a cationic surfactant at room temperature, specifically comprising the following steps:
[0007] (1) The raw ore is subjected to staged closed-circuit grinding to obtain a slurry with a grinding fineness of -0.074 mm and a content of 60-95%;
[0008] (2) Pumping the slurry in step (1) into a weak magnetic separator for magnetic separation to obtain weak magnetic concentrate and weak magnetic tailings, and feeding the weak magnetic tailings into a strong magnetic separator again to recover weak magnetic minerals, and mixing the obtained weak magnetic concentrate with the strong magnetic concentrate to form a mixed concentrate with a TFe grade of 40-60%, and feeding it into a mixing tank for slurry adjustment to obtain flotation feed;
[0009] (3) adding a pullulan solution as an inhibitor to the flotation feed to inhibit the iron minerals in the ore, then adding a sodium hydroxide solution to adjust the pH of the slurry, and finally adding a collector dodecylmorpholine solution to fully adjust the slurry, and feeding the slurry into a flotation machine for roughing operation to obtain a roughing concentrate product and a roughing tailings product respectively;
[0010] (4) While maintaining the pH value of the roughing concentrate product unchanged, a collector dodecylmorpholine solution is added to carry out a first-stage concentration operation to obtain iron concentrate and concentrated tailings; the roughing tailings are scavenged without adding a collector to obtain flotation tailings.
[0011] in:
[0012] In the step (2), the mass concentration of the ore pulp fed for flotation is 30-50%.
[0013] In the step (3), the pullulan solution is prepared by dissolving pullulan in water at room temperature and stirring the solution sufficiently to obtain a solution with a mass concentration of 0.1-1%.
[0014] In the step (3), the sodium hydroxide solution is prepared by dissolving sodium hydroxide in water at room temperature and stirring the solution sufficiently, and the mass concentration of the solution is 0.1-1%.
[0015] In the steps (3) and (4), the preparation method of the dodecylmorpholine solution is: dissolving dodecylmorpholine in water at room temperature and stirring sufficiently to obtain the solution, wherein the mass concentration of the solution is 0.1-1%.
[0016] In the step (3), the pH value of the slurry is adjusted to 10-11; after adding the collector to adjust the slurry, the pH value of the slurry is kept unchanged.
[0017] In the step (3), the amount of the inhibitor is 200 to 1000 g·t -1 , the collector dosage is 50~500g·t -1 .
[0018] In the step (4), the amount of collector added in the cleaning operation is 20 to 100 g·t -1 .
[0019] In the step (4), the scavenging operation is divided into three stages. The selected tailings obtained from the first stage of the scavenging operation are combined with the first scavenging concentrate and returned to the roughing process in step (3) for reselection; the second scavenging concentrate and the third scavenging concentrate are returned to the previous scavenging process in turn for reselection.
[0020] In the step (4), the TFe grade of the iron ore concentrate is ≥65%.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention adopts dodecylmorpholine as a collector and pullulan as an inhibitor to carry out reverse flotation of iron ore. Both agents have good water solubility and the preparation process is simple.
[0023] 2. The collector of the present invention has a lower dosage than the traditional fatty acid collector during use, thus saving the cost of the reagent during the flotation process.
[0024] 3. At present, the treatment technology for mineral processing wastewater containing dodecylmorpholine is relatively mature, so the risk of environmental pollution caused by the collector used in the present invention for reverse flotation operation is relatively small. After the collector is applied to the iron ore reverse flotation recovery process, while ensuring the flotation index, it can reduce the production cost and thus improve the development and utilization of low-grade iron ore and the resource self-sufficiency rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 A process flow chart of a cationic surfactant used for reverse flotation of iron ore at room temperature. DETAILED DESCRIPTION
[0026] In order to further illustrate the technical means and effects of the present invention to achieve the expected effects, the present invention will be described in detail below in conjunction with the accompanying drawings and embodiments of the specification. Obviously, the embodiments described are only some implementation cases of the present invention. Therefore, it should be noted that the scope of protection of the present invention is not limited to the following specific embodiments, and the embodiments obtained in the art without significant creative improvements on the basis of the present invention belong to the protection scope of the present invention.
[0027] In the embodiment of the present invention, the pullulan solution, sodium hydroxide solution and dodecylmorpholine are prepared by dissolving pullulan, sodium hydroxide and dodecylmorpholine in water at room temperature respectively and stirring them sufficiently.
[0028] Example 1
[0029] A method for reverse flotation of iron ore using a cationic surfactant at room temperature, the process flow is as follows: Figure 1 As shown, the specific steps include:
[0030] (1) After a certain iron ore is crushed, it is subjected to staged closed-circuit grinding to obtain a slurry with a grinding fineness of -0.074 mm and a content of 80%;
[0031] (2) The slurry in step (1) is pumped into a weak magnetic separator through a slurry pump for magnetic separation to obtain weak magnetic concentrate and weak magnetic tailings, and the weak magnetic tailings are fed into a strong magnetic separator again to recover weak magnetic minerals. The obtained weak magnetic concentrate and strong magnetic concentrate are mixed to form a mixed concentrate with a TFe grade of 43.88% and a SiO2 content of 19.41%. The main metal mineral components in the mixed concentrate are hematite and magnetite, and the non-metallic gangue minerals are mainly quartz; the mixed concentrate is fed into a stirring barrel for slurry adjustment to obtain a flotation feed with a slurry mass concentration of 30%;
[0032] (3) Add 400 g·t of pullulan solution, an inhibitor, with a mass concentration of 0.3% to the flotation feed. -1 , used to inhibit iron minerals in the ore; then add a 1% sodium hydroxide solution to adjust the slurry pH to 10.5, and finally add a 0.3% collector dodecyl morpholine solution to fully adjust the slurry. The addition amount is 350g·t -1 After slurry adjustment, the pH value of the slurry is kept unchanged, and the slurry is fed into the flotation machine for roughing operation to obtain roughing concentrate products and roughing tailings products respectively;
[0033] (4) While maintaining the pH value of the rough concentrate product unchanged, add 0.3% dodecyl morpholine solution as a collector in an amount of 60 g·t -1 , a first-stage concentration operation is performed to obtain iron concentrate and concentrated tailings; the roughing tailings are scavenged without adding a collector, and the scavenging operation is divided into three stages. The concentrated tailings obtained from the first stage of the concentration operation are combined with the first scavenging concentrate, and returned to the roughing process in step (3) for reselection; the second scavenging concentrate and the third scavenging concentrate are returned to the previous scavenging process for reselection in turn to obtain flotation tailings. The indicators of the obtained iron concentrate and flotation tailings are shown in Table 1.
[0034] Table 1 Index of products obtained in Example 1
[0035] Product Name TFe grade / % Recovery rate / % Iron Concentrate 65.64 57.98 Flotation tailings 13.86 42.02 total 43.88 100
[0036] Example 2
[0037] A method for reverse flotation of iron ore using a cationic surfactant at room temperature, specifically comprising the following steps:
[0038] (1) After a certain iron ore is crushed, it is subjected to staged closed-circuit grinding to obtain a slurry with a grinding fineness of -0.074 mm and a content of 85%;
[0039] (2) The slurry in step (1) is pumped into a weak magnetic separator through a slurry pump for magnetic separation to obtain weak magnetic concentrate and weak magnetic tailings, and the weak magnetic tailings are fed into a strong magnetic separator again to recover weak magnetic minerals. The obtained weak magnetic concentrate and strong magnetic concentrate are mixed to form a mixed concentrate with a TFe grade of 47.58% and a SiO2 content of 21.33%, wherein the main metal mineral components in the mixed concentrate are hematite and magnetite, and the non-metallic gangue minerals are mainly quartz; the mixed concentrate is fed into a mixing barrel for slurry adjustment to obtain a flotation feed with a slurry mass concentration of 35%;
[0040] (3) Add 700 g·t of pullulan solution, a 0.5% inhibitor, to the flotation feed. -1 , used to suppress the iron minerals in the ore; then add a 1% sodium hydroxide solution to adjust the slurry pH to 10, and finally add a 0.8% collector dodecyl morpholine solution to fully adjust the slurry. The addition amount is 400g·t -1 After slurry adjustment, the pH value of the slurry is kept unchanged, and the slurry is fed into the flotation machine for roughing operation to obtain roughing concentrate products and roughing tailings products respectively;
[0041] (4) While maintaining the pH value of the rough concentrate product unchanged, add 0.8% dodecyl morpholine solution as a collector in an amount of 40 g·t -1 , a first-stage concentration operation is performed to obtain iron concentrate and concentrated tailings; the roughing tailings are scavenged without adding a collector, and the scavenging operation is divided into three stages. The concentrated tailings obtained from the first stage of the concentration operation are combined with the first scavenging concentrate, and returned to the roughing process in step (3) for reselection; the second scavenging concentrate and the third scavenging concentrate are returned to the previous scavenging process for reselection in turn to obtain flotation tailings. The indicators of the obtained iron concentrate and flotation tailings are shown in Table 2.
[0042] Table 2 Index of products obtained in Example 2
[0043] Product Name TFe grade / % Recovery rate / % Iron Concentrate 65.84 66.65 Flotation tailings 11.09 33.35 total 47.58 100
[0044] Example 3
[0045] A method for reverse flotation of iron ore using a cationic surfactant at room temperature, specifically comprising the following steps:
[0046] (1) After a certain iron ore is crushed, it is subjected to staged closed-circuit grinding to obtain a slurry with a grinding fineness of -0.074 mm and a content of 90%;
[0047] (2) The slurry in step (1) is pumped into a weak magnetic separator through a slurry pump for magnetic separation to obtain weak magnetic concentrate and weak magnetic tailings. The weak magnetic tailings are fed into a strong magnetic separator again to recover weak magnetic minerals. The obtained weak magnetic concentrate and strong magnetic concentrate are mixed to form a mixed concentrate with a TFe grade of 43.14% and a SiO2 content of 20.54%. The main metal mineral components in the mixed concentrate are hematite and magnetite, and the non-metallic gangue minerals are mainly quartz. The mixed concentrate is fed into a mixing barrel for slurry adjustment to obtain a flotation feed with a slurry mass concentration of 40%;
[0048] (3) Add 0.2% pullulan solution as an inhibitor to the flotation feed, with an addition amount of 300 g·t -1 , used to inhibit iron minerals in the ore; then add a 1% sodium hydroxide solution to adjust the slurry pH to 11, and finally add a 0.1% collector dodecyl morpholine solution to fully adjust the slurry. The addition amount is 300g·t -1 After slurry adjustment, the pH value of the slurry is kept unchanged, and the slurry is fed into the flotation machine for roughing operation to obtain roughing concentrate products and roughing tailings products respectively;
[0049] (4) While maintaining the pH value of the rough concentrate product unchanged, add 0.1% dodecyl morpholine solution as a collector in an amount of 30 g·t -1 , a first-stage concentration operation is performed to obtain iron concentrate and concentrated tailings; the roughing tailings are scavenged without adding a collector, and the scavenging operation is divided into three stages. The concentrated tailings obtained from the first stage of the concentration operation are combined with the first scavenging concentrate, and returned to the roughing process in step (3) for reselection; the second scavenging concentrate and the third scavenging concentrate are returned to the previous scavenging process for reselection in turn to obtain flotation tailings. The indicators of the obtained iron concentrate and flotation tailings are shown in Table 3.
[0050] Table 3 Index of products obtained in Example 3
[0051] Product Name TFe grade / % Recovery rate / % Iron Concentrate 65.86 54.83 Flotation tailings 15.56 45.17 total 43.14 100
[0052] Example 4
[0053] A method for reverse flotation of iron ore using a cationic surfactant at room temperature, specifically comprising the following steps:
[0054] (1) After a certain iron ore is crushed, it is subjected to staged closed-circuit grinding to obtain a slurry with a grinding fineness of -0.074 mm and a content of 95%;
[0055] (2) The slurry in step (1) is pumped into a weak magnetic separator through a slurry pump for magnetic separation to obtain weak magnetic concentrate and weak magnetic tailings. The weak magnetic tailings are fed into a strong magnetic separator again to recover weak magnetic minerals. The obtained weak magnetic concentrate and strong magnetic concentrate are mixed to form a mixed concentrate with a TFe grade of 53.93% and a SiO2 content of 15.71%. The main metal mineral components in the mixed concentrate are hematite and magnetite, and the non-metallic gangue minerals are mainly quartz. The mixed concentrate is fed into a mixing barrel for slurry adjustment to obtain a flotation feed with a slurry mass concentration of 50%;
[0056] (3) Add 800 g·t of pullulan solution, a 0.6% inhibitor, to the flotation feed. -1 , used to inhibit iron minerals in the ore; then add a 1% sodium hydroxide solution to adjust the slurry pH to 10, and finally add a 1% collector dodecyl morpholine solution to fully adjust the slurry. The addition amount is 150g·t -1 After slurry adjustment, the pH value of the slurry is kept unchanged, and the slurry is fed into the flotation machine for roughing operation to obtain roughing concentrate products and roughing tailings products respectively;
[0057] (4) While maintaining the pH value of the rough concentrate product, add 1% collector dodecylmorpholine solution in an amount of 20 g·t -1 , a first-stage concentration operation is performed to obtain iron concentrate and concentrated tailings; the roughing tailings are scavenged without adding a collector, and the scavenging operation is divided into three stages. The concentrated tailings obtained from the first stage of the concentration operation are combined with the first scavenging concentrate, and returned to the roughing process in step (3) for reselection; the second scavenging concentrate and the third scavenging concentrate are returned to the previous scavenging process for reselection in turn to obtain flotation tailings. The indicators of the obtained iron concentrate and flotation tailings are shown in Table 4.
[0058] Table 4 Product indicators of Example 4
[0059] Product Name TFe grade / % Recovery rate / % Iron Concentrate 66.73 75.88 Flotation tailings 13.66 24.12 total 53.93 100
[0060] Example 5
[0061] A method for reverse flotation of iron ore using a cationic surfactant at room temperature, specifically comprising the following steps:
[0062] (1) After a certain iron ore is crushed, it is subjected to staged closed-circuit grinding to obtain a slurry with a grinding fineness of -0.074 mm and a content of 90%;
[0063] (2) The slurry in step (1) is pumped into a weak magnetic separator through a slurry pump for magnetic separation to obtain weak magnetic concentrate and weak magnetic tailings. The weak magnetic tailings are fed into a strong magnetic separator again to recover weak magnetic minerals. The obtained weak magnetic concentrate and strong magnetic concentrate are mixed to form a mixed concentrate with a TFe grade of 46.75% and a SiO2 content of 22.96%. The main metal mineral components in the mixed concentrate are hematite and magnetite, and the non-metallic gangue minerals are mainly quartz. The mixed concentrate is fed into a mixing barrel for slurry adjustment to obtain a flotation feed with a slurry mass concentration of 30%;
[0064] (3) Add 0.1% pullulan solution as an inhibitor to the flotation feed, with an addition amount of 600 g·t -1 , used to inhibit iron minerals in the ore; then add a 1% sodium hydroxide solution to adjust the slurry pH to 10, and finally add a 0.7% collector dodecyl morpholine solution to fully adjust the slurry. The addition amount is 200g·t -1 After slurry adjustment, the pH value of the slurry is kept unchanged, and the slurry is fed into the flotation machine for roughing operation to obtain roughing concentrate products and roughing tailings products respectively;
[0065] (4) While maintaining the pH value of the rough concentrate product unchanged, add 0.7% dodecyl morpholine solution as a collector in an amount of 50 g·t -1 , a first stage of concentration operation is carried out to obtain iron concentrate and concentrated tailings; the roughing tailings are scavenged without adding a collector, and the scavenging operation is divided into three stages. The concentrated tailings obtained from the first stage of concentration operation are combined with the first scavenging concentrate, and returned to the roughing process in step (3) for reselection; the second scavenging concentrate and the third scavenging concentrate are returned to the previous scavenging process for reselection in turn to obtain flotation tailings. The indicators of the obtained iron concentrate and flotation tailings are shown in Table 5.
[0066] Table 5 Index of products obtained in Example 5
[0067] Product Name TFe grade / % Recovery rate / % Iron Concentrate 65.24 62.54 Flotation tailings 15.88 37.46 total 46.75 100
[0068] Example 6
[0069] A method for reverse flotation of iron ore using a cationic surfactant at room temperature, specifically comprising the following steps:
[0070] (1) After a certain iron ore is crushed, it is subjected to staged closed-circuit grinding to obtain a slurry with a grinding fineness of -0.074 mm and a content of 85%;
[0071] (2) The slurry in step (1) is pumped into a weak magnetic separator through a slurry pump for magnetic separation to obtain weak magnetic concentrate and weak magnetic tailings. The weak magnetic tailings are fed into a strong magnetic separator again to recover weak magnetic minerals. The obtained weak magnetic concentrate and strong magnetic concentrate are mixed to form a mixed concentrate with a TFe grade of 41.61% and a SiO2 content of 22.09%. The main metal mineral components in the mixed concentrate are hematite and magnetite, and the non-metallic gangue minerals are mainly quartz. The mixed concentrate is fed into a mixing barrel for slurry adjustment to obtain a flotation feed with a slurry mass concentration of 45%;
[0072] (3) Add 1% pullulan solution as an inhibitor to the flotation feed, with an addition amount of 300 g·t -1 , used to inhibit iron minerals in the ore; then add a 1% sodium hydroxide solution to adjust the slurry pH to 10.5, and finally add a 0.5% collector dodecyl morpholine solution to fully adjust the slurry. The addition amount is 300g·t -1 After slurry adjustment, the pH value of the slurry is kept unchanged, and the slurry is fed into the flotation machine for roughing operation to obtain roughing concentrate products and roughing tailings products respectively;
[0073] (4) While maintaining the pH value of the rough concentrate product unchanged, add 0.5% collector dodecyl morpholine solution in an amount of 70 g·t -1 , a first-stage concentration operation is performed to obtain iron concentrate and concentrated tailings; the roughing tailings are scavenged without adding a collector, and the scavenging operation is divided into three stages. The concentrated tailings obtained from the first stage of the concentration operation are combined with the first scavenging concentrate, and returned to the roughing process in step (3) for reselection; the second scavenging concentrate and the third scavenging concentrate are returned to the previous scavenging process for reselection in turn to obtain flotation tailings. The indicators of the obtained iron concentrate and flotation tailings are shown in Table 6.
[0074] Table 6 Index of the product obtained in Example 6
[0075]
[0076]
[0077] Comparative Example 1
[0078] A method for reverse flotation of iron ore using a cationic surfactant at room temperature, specifically comprising the following steps:
[0079] (1) After a certain iron ore is crushed, it is subjected to staged closed-circuit grinding to obtain a slurry with a grinding fineness of -0.074 mm and a content of 90%;
[0080] (2) The slurry in step (1) is pumped into a weak magnetic separator through a slurry pump for magnetic separation to obtain weak magnetic concentrate and weak magnetic tailings. The weak magnetic tailings are fed into a strong magnetic separator again to recover weak magnetic minerals. The obtained weak magnetic concentrate and strong magnetic concentrate are mixed to form a mixed concentrate with a TFe grade of 43.14% and a SiO2 content of 20.54%. The main metal mineral components in the mixed concentrate are hematite and magnetite, and the non-metallic gangue minerals are mainly quartz. The mixed concentrate is fed into a mixing barrel for slurry adjustment to obtain a flotation feed with a slurry mass concentration of 40%;
[0081] (3) Add 0.2% pullulan solution as an inhibitor to the flotation feed, with an addition amount of 300 g·t -1 , used to inhibit the iron minerals in the ore; then add a 1% mass concentration of activator calcium oxide solution to activate the siliceous gangue, the addition amount is 70g·t -1 , and adjust the pulp pH to 11, and finally add 0.1% sodium oleate solution for full pulping, the addition amount is 700g·t -1 After slurry adjustment, the pH value of the slurry is kept unchanged, and the slurry is fed into the flotation machine for roughing operation to obtain roughing concentrate products and roughing tailings products respectively;
[0082] (4) Add 0.1% sodium oleate solution and 1% calcium oxide solution to the rough concentrate product. The amount of sodium oleate solution added is 350 g·t -1 , the amount of calcium oxide solution added is 30g·t -1 , a first-stage concentration operation is performed to obtain iron concentrate and concentrated tailings; the roughing tailings are scavenged without adding a collector, and the scavenging operation is divided into three stages. The concentrated tailings obtained from the first stage of the concentration operation are combined with the first scavenging concentrate, and returned to the roughing process in step (3) for reselection; the second scavenging concentrate and the third scavenging concentrate are returned to the previous scavenging process for reselection in turn to obtain flotation tailings. The indicators of the obtained iron concentrate and flotation tailings are shown in Table 7.
[0083] Table 7 Comparative Example 1 Product Index
[0084] Product Name TFe grade / % Recovery rate / % Iron Concentrate 64.24 50.35 Flotation tailings 21.74 49.65 total 43.14 100
[0085] Comparative Example 2
[0086] A method for reverse flotation of iron ore using a cationic surfactant at room temperature, specifically comprising the following steps:
[0087] (1) After a certain iron ore is crushed, it is subjected to staged closed-circuit grinding to obtain a slurry with a grinding fineness of -0.074 mm and a content of 85%;
[0088] (2) The slurry in step (1) is pumped into a weak magnetic separator through a slurry pump for magnetic separation to obtain weak magnetic concentrate and weak magnetic tailings. The weak magnetic tailings are fed into a strong magnetic separator again to recover weak magnetic minerals. The obtained weak magnetic concentrate and strong magnetic concentrate are mixed to form a mixed concentrate with a TFe grade of 41.61% and a SiO2 content of 22.09%. The main metal mineral components in the mixed concentrate are hematite and magnetite, and the non-metallic gangue minerals are mainly quartz. The mixed concentrate is fed into a mixing barrel for slurry adjustment to obtain a flotation feed with a slurry mass concentration of 45%;
[0089] (3) Add 1% pullulan solution as an inhibitor to the flotation feed, with an addition amount of 300 g·t -1 , used to inhibit the iron minerals in the ore; then add a 1% mass concentration of activator calcium oxide solution to activate the siliceous gangue, the addition amount is 140g·t -1 , and adjust the pulp pH to 10.5, and finally add 0.5% sodium oleate solution for full pulping, the addition amount is 800g·t -1 After slurry adjustment, the pH value of the slurry is kept unchanged, and the slurry is fed into the flotation machine for roughing operation to obtain roughing concentrate products and roughing tailings products respectively;
[0090] (4) Add 0.5% sodium oleate solution and 1% calcium oxide solution to the rough concentrate product. The amount of sodium oleate solution added is 400 g·t -1 , the amount of calcium oxide solution added is 50g·t -1 , a first-stage concentration operation is performed to obtain iron concentrate and concentrated tailings; the roughing tailings are scavenged without adding a collector, and the scavenging operation is divided into three stages. The concentrated tailings obtained from the first stage of the concentration operation are combined with the first scavenging concentrate, and returned to the roughing process in step (3) for reselection; the second scavenging concentrate and the third scavenging concentrate are returned to the previous scavenging process for reselection in turn to obtain flotation tailings. The indicators of the obtained iron concentrate and flotation tailings are shown in Table 8.
[0091] Table 8 Product indexes of comparative example 2
[0092] Product Name TFe grade / % Recovery rate / % Iron Concentrate 64.41 50.21 Flotation tailings 18.62 49.79 total 41.61 100
[0093] The above are only preferred examples of the present invention and cannot limit the scope of implementation of the present invention. That is, all embodiments obtained in the art without significant creative improvements based on the present invention belong to the protection scope of the present invention.
Claims
1. A method for reverse flotation of iron ore using a cationic surfactant at room temperature, characterized in that: The specific steps include: (1) The raw ore is subjected to staged closed-circuit grinding to obtain a slurry with a grinding fineness of -0.074 mm and a content of 60-95%; (2) Pumping the slurry in step (1) into a weak magnetic separator for magnetic separation to obtain weak magnetic concentrate and weak magnetic tailings, and feeding the weak magnetic tailings into a strong magnetic separator again to recover weak magnetic minerals, and mixing the obtained weak magnetic concentrate with the strong magnetic concentrate to form a mixed concentrate with a TFe grade of 40-60%, and feeding it into a mixing tank for slurry adjustment to obtain flotation feed; (3) adding a pullulan solution as an inhibitor to the flotation feed to inhibit the iron minerals in the ore, then adding a sodium hydroxide solution to adjust the pH of the slurry, and finally adding a collector dodecylmorpholine solution to fully adjust the slurry, and feeding the slurry into a flotation machine for roughing operation to obtain a roughing concentrate product and a roughing tailings product respectively; (4) While maintaining the pH value of the roughing concentrate product unchanged, a collector dodecylmorpholine solution is added to carry out a first-stage concentration operation to obtain iron concentrate and concentrated tailings; the roughing tailings are scavenged without adding a collector to obtain flotation tailings.
2. The method for reverse flotation of iron ore using a cationic surfactant at room temperature according to claim 1, characterized in that: In the step (2), the mass concentration of the ore pulp fed for flotation is 30-50%.
3. The method for reverse flotation of iron ore using a cationic surfactant at room temperature according to claim 1, characterized in that: In the step (3), the pullulan solution is prepared by dissolving pullulan in water at room temperature and stirring the solution sufficiently to obtain a solution with a mass concentration of 0.1-1%.
4. The method for reverse flotation of iron ore using a cationic surfactant at room temperature according to claim 1, characterized in that: In the step (3), the sodium hydroxide solution is prepared by dissolving sodium hydroxide in water at room temperature and stirring the solution sufficiently, and the mass concentration of the solution is 0.1-1%.
5. The method for reverse flotation of iron ore using a cationic surfactant at room temperature according to claim 1, characterized in that: In the steps (3) and (4), the preparation method of the dodecylmorpholine solution is: dissolving dodecylmorpholine in water at room temperature and stirring sufficiently to obtain the solution, wherein the mass concentration of the solution is 0.1-1%.
6. The method for reverse flotation of iron ore using a cationic surfactant at room temperature according to claim 1, characterized in that: In the step (3), the pH value of the slurry is adjusted to 10-11; after adding the collector to adjust the slurry, the pH value of the slurry is kept unchanged.
7. The method for reverse flotation of iron ore using a cationic surfactant at room temperature according to claim 1, characterized in that: In the step (3), the amount of the inhibitor is 200 to 1000 g·t -1 , the collector dosage is 50~500g·t -1 .
8. The method for reverse flotation of iron ore using a cationic surfactant at room temperature according to claim 1, characterized in that: In the step (4), the amount of collector added in the cleaning operation is 20 to 100 g·t -1 .
9. The method for reverse flotation of iron ore using a cationic surfactant at room temperature according to claim 1, characterized in that: In the step (4), the scavenging operation is divided into three stages. The selected tailings obtained from the first stage of the scavenging operation are combined with the first scavenging concentrate and returned to the roughing process in step (3) for reselection; the second scavenging concentrate and the third scavenging concentrate are returned to the previous scavenging process in turn for reselection.
10. The method for reverse flotation of iron ore using a cationic surfactant at room temperature according to claim 1, characterized in that: In the step (4), the TFe grade of the iron ore concentrate is ≥65%.
Citation Information
Patent Citations
Flotation collector for obtaining high-grade magnesite concentrate from low-grade magnesite and method thereof
CN103272702A
Separation method for strengthening recycling of fine-grain low-intensity-magnetic iron ore through magnetic levitation stage agent addition
CN106824507A
Morpholine quaternary ammonium salt Gemini surface active agent for mineral flotation
CN107442288A
Method for reducing emission by reverse flotation reagent for carnallite mine
CN108355842A
Flotation separation method for iron-containing silicate gangue minerals
CN114054215A