Vacuum suction casting method and equipment for continuous alumina fiber reinforced aluminum-based composite material
Through vacuum casting methods and equipment, the problem of complex and high cost of alumina fiber reinforced aluminum matrix composite materials is solved, the simplified process and performance improvement of the material is achieved, and the denser and higher performance alumina fiber reinforced aluminum matrix is obtained. Composite material.
Patent Information
- Application Number
- CN202410928352.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-01
AI Technical Summary
The preparation process of alumina fiber reinforced aluminum-based composite materials is complex and costly. The existing aluminum alloy casting technology has problems such as high molding complexity, limited mechanical properties, and high manufacturing costs.
Using vacuum casting methods and equipment for reinforced aluminum-based composite materials, a mold containing alumina fibers is prepared by melting an aluminum alloy ingot in a resistor furnace, and filling the mold with molten metal in a vacuum state. The mold is corroded after removal to obtain an alumina fiber reinforced aluminum matrix composite.
The process flow is simplified, the emergence of impurities is avoided, the preparation cost is significantly reduced, and the density and mechanical properties of the material are improved.
Smart Images

Figure CN118875252A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy casting, and in particular to a vacuum suction casting method and equipment for continuous alumina fiber reinforced aluminum-based composite materials. Background Art
[0002] Traditional aluminum alloy casting technology usually uses methods such as sand casting or die casting. Although these methods meet the needs of aluminum alloy castings to a certain extent, they also have some limitations. For example, there are problems such as high molding complexity, limited mechanical properties, and high manufacturing costs. In order to improve the performance of castings, people have begun to study fiber-reinforced aluminum-based materials. By adding fibers to aluminum-based materials, the strength, stiffness, and wear resistance of castings can be significantly improved. Alumina fiber-reinforced aluminum-based composites have the advantages of high specific strength, high specific stiffness, low thermal expansion, good fatigue resistance and heat resistance, and have great application potential as composite core materials for power transmission conductors. However, the current preparation process of alumina fiber-reinforced aluminum-based composites is complex and the cost is high. Summary of the invention
[0003] In view of this, the present invention provides a vacuum suction casting method and equipment for continuous alumina fiber reinforced aluminum-based composite materials, which are used to solve the technical problems of complex preparation process and high cost of existing alumina fiber reinforced aluminum-based composite materials.
[0004] In order to solve the above technical problems, the present invention adopts the following technical solution:
[0005] A vacuum suction casting method for continuous alumina fiber reinforced aluminum-based composite material comprises the following steps:
[0006] The aluminum alloy ingot is placed in a crucible in a resistance furnace for smelting;
[0007] preparing a mold containing alumina fibers;
[0008] Putting the mold into a preheating furnace for preheating;
[0009] placing the preheated mold into the resistance furnace;
[0010] Filling the mold with molten metal by vacuum casting;
[0011] The mold is taken out and cooled, and then the mold is corroded to obtain a structural member of an alumina fiber reinforced aluminum-based composite material.
[0012] In some embodiments of the vacuum suction casting method, placing the aluminum alloy ingot into a crucible in a resistance furnace for smelting comprises the following steps:
[0013] placing an aluminum alloy ingot into a crucible in a resistance furnace;
[0014] The crucible is evacuated and argon gas is introduced;
[0015] The crucible is heated to perform smelting.
[0016] In some embodiments of the vacuum suction casting method, heating the crucible for melting comprises the following steps:
[0017] heating the crucible;
[0018] The aluminum alloy ingot in the crucible is stirred after heating.
[0019] In some embodiments of the vacuum suction casting method, the preparation of the mold containing the alumina fiber comprises the following steps:
[0020] Supplied with alumina fiber and two sheets of aluminum foil
[0021] Placing alumina fiber between two sheets of aluminum foil and rolling it up and placing it in the mold;
[0022] The inlet of the mold was sealed with an aluminum block.
[0023] In some embodiments of the vacuum suction casting method, when the preheated mold is placed in the resistance furnace, the aluminum block sealing the mold entrance is immersed in the crucible.
[0024] In some embodiments of the vacuum suction casting method, in the step of placing the mold into a preheating furnace for preheating, the preheating temperature is 500° C.-600° C., the preheating time is 20 min-40 min, and argon gas is introduced.
[0025] In some embodiments of the vacuum suction casting method, the mold is made of stainless steel, and the corrosive liquid for corroding the mold is concentrated nitric acid.
[0026] In order to solve the above technical problems, the second technical solution adopted by the present invention is:
[0027] A vacuum suction casting device, comprising:
[0028] A container having a receiving space capable of receiving the mold, wherein the container is provided with a first hole and a second hole capable of connecting the receiving space with the outside, wherein the first hole is used for introducing a protective gas;
[0029] A crucible, contained in the containing space;
[0030] A heating component, contained in the containing space and capable of heating the crucible;
[0031] and a negative pressure component connected to the second hole.
[0032] In an embodiment of the vacuum suction casting equipment, the vacuum suction casting equipment further comprises a support member, wherein the support member is connected to an inner wall of the container, and the support member is used to support the mold so that the mold can be suspended in the receiving space.
[0033] In an embodiment of a vacuum suction casting device, the support member divides the receiving space into a first space and a second space, the first hole is connected to the first space, the second hole is connected to the second space, the heating component and the crucible are both received in the second space, and the heating component is arranged around the crucible.
[0034] Implementing the embodiments of the present invention will have at least the following beneficial effects:
[0035] The above-mentioned vacuum suction casting method of continuous alumina fiber reinforced aluminum-based composite material has the effect of simplifying the process. Specifically, the vacuum suction casting method of the present invention can fill the mold with the molten metal in the crucible by vacuum suction casting to obtain the alumina fiber reinforced aluminum-based composite material. Due to the vacuum state, there will be no other impurities, which simplifies the process flow and solves the technical problems of complex and high cost of the existing preparation process of alumina fiber reinforced aluminum-based composite materials.
[0036] The above-mentioned vacuum suction casting equipment achieves vacuum suction casting by arranging a crucible and a heating component in a container and then evacuating the container through a negative pressure component. Due to the vacuum state, there will be no other impurities, which simplifies the process flow and solves the technical problems of the existing complex and high cost preparation process of alumina fiber reinforced aluminum-based composite materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0038] Figure 1 A schematic diagram of a vacuum suction casting method according to an embodiment;
[0039] Figure 2 A schematic diagram of a vacuum suction casting method according to an embodiment;
[0040] Figure 3 A schematic diagram of the structure of a vacuum suction casting device in one embodiment;
[0041] Figure 4 for Figure 3 A cross-sectional view of the vacuum suction casting equipment shown.
[0042] Among them: 1. second hole; 2. container; 3. support member; 4. mold; 5. heating component; 6. alumina fiber; 7. aluminum block; 8. molten metal; 9. crucible; 10. first hole. DETAILED DESCRIPTION
[0043] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. Preferred embodiments of the present invention are provided in the drawings. However, the present invention can be implemented in many other different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0044] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only.
[0045] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0046] Combine the following Figure 1-4 The vacuum suction casting method and equipment involved in the present invention are explained.
[0047] In an embodiment of a vacuum suction casting method for continuous alumina fiber 6 reinforced aluminum-based composite material, the following steps are included:
[0048] S101, placing the aluminum alloy ingot into the crucible 9 in the resistance furnace for smelting.
[0049] S102, preparing a mold 4 containing alumina fibers 6.
[0050] S103, placing the mold 4 into a preheating furnace for preheating.
[0051] S104, placing the preheated mold 4 into the resistance furnace.
[0052] S105, filling the mold 4 with the molten metal 8 by vacuum suction casting.
[0053] S106, taking out the mold 4, cooling it, and then corroding the mold 4 to obtain a structural member of an aluminum-based composite material reinforced with alumina fibers 6.
[0054] In this embodiment, the molten metal 8 in the crucible 9 can be filled into the mold 4 by vacuum casting to obtain an alumina fiber 6 reinforced aluminum-based composite material. Due to the vacuum state, there will be no other impurities, which simplifies the process flow and solves the technical problems of complex and high cost preparation processes of existing alumina fiber 6 reinforced aluminum-based composite materials.
[0055] In an embodiment of the vacuum suction casting method, the step of placing the aluminum alloy ingot into the crucible 9 in the resistance furnace for smelting comprises the following steps:
[0056] S1011, placing the aluminum alloy ingot into the crucible 9 in the resistance furnace.
[0057] S1012, evacuate the crucible 9 and introduce argon gas.
[0058] S1013, heating the crucible 9 for smelting.
[0059] In this embodiment, impurities can be reduced by introducing argon gas during the process of melting the aluminum alloy in the crucible 9 .
[0060] In an embodiment of the vacuum suction casting method, heating the crucible 9 for smelting comprises the following steps:
[0061] S10131, heating the crucible 9.
[0062] S10132, stirring the aluminum alloy ingot in the crucible 9 after heating.
[0063] In this embodiment, stirring is performed to ensure that the composition of the molten metal 8 is more uniform, and the number of stirring times may be 4-6 times.
[0064] In an embodiment of the vacuum suction casting method, the preparation of the mold 4 containing the alumina fiber 6 comprises the following steps:
[0065] S1021, provide alumina fiber 6 and two aluminum foils
[0066] S1022, place the alumina fiber 6 between two aluminum foils and roll it up and put it into the mold 4.
[0067] S1022, sealing the entrance of the mold 4 with an aluminum block 7.
[0068] In this embodiment, specifically, the mold 4 takes a tubular shape as an example, and a columnar structure can be obtained. Because vacuum casting is adopted, the mold 4 needs to have an inlet and an outlet. In this embodiment, an aluminum block 7 is used to seal the fiber when it is placed in the mold 4. The material of the aluminum block 7 will not introduce impurities, which is convenient for the subsequent melting of the aluminum block 7 and mixing together. The same is true for aluminum foil. In this way, during the suction casting process, the molten metal 8 will gradually fill the mold 4 and mix with the alumina fiber 6.
[0069] In an embodiment of the vacuum suction casting method, when the preheated mold 4 is placed in the resistance furnace, the aluminum block 7 sealing the entrance of the mold 4 is immersed in the crucible 9.
[0070] In this embodiment, by immersing the aluminum block 7 into the crucible 9, the aluminum block 7 can be melted quickly and conveniently, and the melting of the aluminum block 7 can facilitate the molten metal 8 in the crucible 9 to enter the mold 4 or the alumina fiber 6 in the mold 4 to enter the crucible 9 for mixing.
[0071] In addition, the mold 4 is placed in a preheating furnace for preheating at a temperature of 500-600°C for a preheating time of 20-40 minutes and argon is introduced. The mold 4 is made of stainless steel, and the etching liquid for etching the mold 4 is concentrated nitric acid.
[0072] In combination with the above embodiments, the vacuum suction casting method of the present invention comprises the following steps:
[0073] S1. Vacuum resistance furnace smelting aluminum alloy: put the aluminum alloy ingot into the crucible 9 in the resistance furnace, evacuate the furnace and pass argon gas into the furnace, heat the crucible 9 and stir and smelt repeatedly for 4-6 times.
[0074] S2. Place the fiber into the stainless steel mold 4: provide alumina fiber 6 and two aluminum foils, place the alumina fiber 6 between the two aluminum foils and roll it up and place it into the stainless steel mold 4, seal the entrance of the mold 4 with an aluminum block 7 to prepare a mold 4 containing the alumina fiber 6.
[0075] S3, preheating the mold 4: put the mold 4 into a preheating furnace for preheating, the preheating temperature is 500°C-600°C, the preheating time is 20min-40min and argon gas is introduced, and immediately put it into a vacuum resistance furnace after preheating.
[0076] S4. Vacuum suction casting: adjust the position of the mold 4 so that the sealed end of the aluminum block 7 on the mold 4 is immersed in the crucible 9, and the molten metal 8 is filled with the mold 4 through vacuum suction casting.
[0077] S5, etching the mold 4: after vacuum suction casting is completed, the mold 4 is taken out and cooled naturally, and then the mold 4 is etched away using concentrated nitric acid to obtain a structural member of an aluminum-based composite material reinforced with alumina fibers 6.
[0078] Example 1
[0079] S11. Vacuum resistance furnace smelting aluminum alloy: the aluminum alloy ingot is placed in the crucible 9 in the resistance furnace, vacuuming the furnace and passing argon gas into the furnace, heating the crucible 9 and stirring to repeat the smelting for 5 times.
[0080] S21. Place the fiber into the stainless steel mold 4: provide alumina fiber 6 and two aluminum foils, place the alumina fiber 6 between the two aluminum foils and roll it up and place it into the stainless steel mold 4, seal the entrance of the mold 4 with an aluminum block 7 to prepare a mold 4 containing the alumina fiber 6.
[0081] S31, preheating the mold 4: put the mold 4 into a preheating furnace for preheating, the preheating temperature is 560°C, the preheating time is 30 minutes and argon gas is introduced, and immediately put it into a vacuum resistance furnace after preheating.
[0082] S41, vacuum suction casting: adjust the position of the mold 4 so that the end of the mold 4 sealed by the aluminum block 7 is immersed in the crucible 9, and the mold 4 is filled with the molten metal 8 by vacuum suction casting.
[0083] S51, etching the mold 4: after vacuum casting is completed, the mold 4 is taken out and cooled naturally, and then the mold 4 is etched away using concentrated nitric acid to obtain a structural member of an aluminum-based composite material reinforced with an alumina fiber 6.
[0084] Example 2
[0085] S12. Vacuum resistance furnace smelting aluminum alloy: the aluminum alloy ingot is placed in the crucible 9 in the resistance furnace, vacuuming the furnace and passing argon gas into the furnace, and the crucible 9 is heated and stirred and smelted repeatedly for 6 times.
[0086] S22. Place the fiber into the stainless steel mold 4: provide alumina fiber 6 and two aluminum foils, place the alumina fiber 6 between the two aluminum foils and roll it up and place it into the stainless steel mold 4, seal the entrance of the mold 4 with an aluminum block 7 to prepare a mold 4 containing the alumina fiber 6.
[0087] S32, preheating the mold 4: placing the mold 4 in a preheating furnace for preheating at a temperature of 600° C. for 40 minutes and introducing argon gas. Immediately after preheating, placing the mold 4 in a vacuum resistance furnace.
[0088] S42, vacuum suction casting: adjust the position of the mold 4 so that the end of the mold 4 sealed by the aluminum block 7 is immersed in the crucible 9, and the mold 4 is filled with the molten metal 8 by vacuum suction casting.
[0089] S52, etching the mold 4: after vacuum casting is completed, the mold 4 is taken out and cooled naturally, and then the mold 4 is etched away using concentrated nitric acid to obtain a structural member of an aluminum-based composite material reinforced with an alumina fiber 6.
[0090] Example 3
[0091] S13, melting aluminum alloy in a vacuum resistance furnace: placing the aluminum alloy ingot into the crucible 9 in the resistance furnace, evacuating the furnace and passing argon gas into the furnace, heating the crucible 9 and stirring and melting repeatedly for 4 times.
[0092] S23, placing the fiber into the stainless steel mold 4: provide alumina fiber 6 and two aluminum foils, place the alumina fiber 6 between the two aluminum foils and roll it up and place it into the stainless steel mold 4, seal the entrance of the mold 4 with an aluminum block 7 to prepare a mold 4 containing the alumina fiber 6.
[0093] S33, preheating the mold 4: put the mold 4 into a preheating furnace for preheating, the preheating temperature is 500° C., the preheating time is 20 min and argon gas is introduced, and immediately put it into a vacuum resistance furnace after preheating is completed.
[0094] S43, vacuum suction casting: adjust the position of the mold 4 so that the end of the mold 4 sealed with the aluminum block 7 is immersed in the crucible 9, and the mold 4 is filled with the molten metal 8 by vacuum suction casting.
[0095] S53, etching the mold 4: after vacuum casting is completed, the mold 4 is taken out and cooled naturally, and then the mold 4 is etched away using concentrated nitric acid to obtain a structural member of an aluminum-based composite material reinforced with an alumina fiber 6.
[0096] Compared with the structural parts obtained by the existing methods, the structural parts obtained by the above three embodiments can have denser materials, fewer defects and higher mechanical properties.
[0097] The present invention also relates to a vacuum suction casting device, comprising a container 2, a crucible 9, a heating component 5 and a negative pressure component. A receiving space capable of receiving a mold 4 is provided in the container 2, and a first hole 10 and a second hole 1 are provided on the container 2, which enable the receiving space to communicate with the outside, and the first hole 10 is used to introduce protective gas. The crucible 9 is received in the receiving space. The heating component 5 is received in the receiving space and can heat the crucible 9. The negative pressure component is connected to the second hole 1.
[0098] In this embodiment, a crucible 9 and a heating component 5 are arranged in a container 2, and vacuum suction casting is achieved by evacuating a negative pressure component. Since it is in a vacuum state, there will be no other impurities, which simplifies the process flow and solves the technical problem of complex and high cost of the existing preparation process of alumina fiber 6 reinforced aluminum-based composite materials.
[0099] In addition, it should be noted that the heating component 5 can be a resistance wire, and the combination with the container 2 is the resistance furnace mentioned in the above embodiment.
[0100] In an embodiment of the vacuum suction casting device, the vacuum suction casting device further includes a support member 3, wherein the support member 3 is connected to the inner wall of the container 2, and the support member 3 is used to support the mold 4 so that the mold 4 can be suspended in the receiving space.
[0101] In this embodiment, the support member 3 is provided to facilitate the suspension of the mold 4. Specifically, the support member 3 can be a plate-like member, and the outer peripheral side wall of the support member 3 and the inner wall of the container 2 are fixed by means such as welding. A hole penetrating the support member 3 is opened on the support member 3, and the end of the mold 4 close to the outlet can be set into a T shape so that it can be suspended on the support member 3.
[0102] In an embodiment of a vacuum suction casting device, the support member 3 divides the receiving space into a first space and a second space, the first hole 10 is connected to the first space, the second hole 1 is connected to the second space, the heating component 5 and the crucible 9 are both received in the second space, and the heating component 5 is arranged around the crucible 9.
[0103] Under the action of the support member 3, the receiving space is divided, and the first space maintains a vacuum state under the action of the negative pressure component, so as to facilitate suction casting, while argon gas is introduced into the second space through the second hole 1 to eliminate interference, and the heating component 5 is arranged in a ring to improve uniform heat.
[0104] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0105] The above embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent application. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A vacuum suction casting method for continuous alumina fiber reinforced aluminum-based composite materials, characterized in that: The following steps are involved: The aluminum alloy ingot is placed in a crucible in a resistance furnace for smelting; preparing a mold containing alumina fibers; Putting the mold into a preheating furnace for preheating; placing the preheated mold into the resistance furnace; Filling the mold with molten metal by vacuum casting; The mold is taken out and cooled, and then the mold is corroded to obtain a structural member of an alumina fiber reinforced aluminum-based composite material.
2. The vacuum suction casting method according to claim 1, characterized in that: The step of placing the aluminum alloy ingot into a crucible in a resistance furnace for smelting comprises the following steps: placing an aluminum alloy ingot into a crucible in a resistance furnace; The crucible is evacuated and argon gas is introduced; The crucible is heated to perform smelting.
3. The vacuum suction casting method according to claim 2, characterized in that: The heating of the crucible for smelting comprises the following steps: heating the crucible; The aluminum alloy ingot in the crucible is stirred after heating.
4. The vacuum suction casting method according to claim 1, characterized in that: The method for preparing a mold containing aluminum oxide fibers comprises the following steps: Supplied with alumina fiber and two sheets of aluminum foil Placing alumina fiber between two sheets of aluminum foil and rolling it up and placing it in the mold; The inlet of the mold was sealed with an aluminum block.
5. The vacuum suction casting method according to claim 4, characterized in that: When the preheated mold is placed in the resistance furnace, the aluminum block sealing the mold entrance is immersed in the crucible.
6. The vacuum suction casting method according to claim 1, characterized in that: The mold is placed in a preheating furnace for preheating, the preheating temperature is 500° C.-600° C., the preheating time is 20 min-40 min, and argon gas is introduced.
7. The vacuum suction casting method according to claim 1, characterized in that: The material of the mold is stainless steel, and the corrosive liquid for corroding the mold is concentrated nitric acid.
8. A vacuum suction casting device, characterized in that: include: A container, wherein a receiving space capable of receiving the mold is provided therein, wherein a first hole and a second hole are provided on the container, which enable the receiving space to communicate with the outside, and the first hole is used for introducing a protective gas; A crucible, contained in the containing space; A heating component, contained in the containing space and capable of heating the crucible; and a negative pressure component connected to the second hole.
9. The vacuum suction casting equipment according to claim 8, characterized in that: The vacuum suction casting equipment further comprises a support member, wherein the support member is connected to the inner wall of the container, and the support member is used to support the mold so that the mold can be suspended in the receiving space.
10. The vacuum suction casting equipment according to claim 9, characterized in that: The support member divides the receiving space into a first space and a second space, the first hole is connected to the first space, the second hole is connected to the second space, the heating component and the crucible are both received in the second space, and the heating component is arranged around the crucible.