Method for manufacturing high-performance powder high-temperature alloy with low cost and short process

By using prealloy powder with different melting points in the powder high-temperature alloy process for thermal isostatic sintering, the manufacturing of high-performance powder high-temperature alloy without boundaries is achieved, the boundary defect problem is solved, the cost and process complexity is reduced, and the production is improved efficiency.

CN118875286APending Publication Date: 2024-11-01UNIV OF SCI & TECH BEIJING
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410880425.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing powder high-temperature alloy process inevitably produces boundary defects of the original powder particles, which affects the mechanical properties and reliability of the material. The existing elimination methods are costly, complex in process and poor in effect.

Method used

Two prealloy powders with different melting points are used for thermal isostatic sintering, and the low-melting alloy powder is melted to form a liquid phase, wetting the surface of the high-melting powder, realizing isothermal solidification, and avoiding the formation of powder particles boundaries.

Benefits of technology

It realizes high-performance powder high-temperature alloy manufacturing without the boundary of original powder particles, reduces process costs and process complexity, improves production efficiency, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118875286A_ABST
    Figure CN118875286A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of powder metallurgy high-temperature alloy, and relates to a low-cost short-process method for manufacturing high-performance powder high-temperature alloy. Two kinds of pre-alloyed powder with melting point difference are adopted as sintering raw materials, and the comprehensive components of the two kinds of pre-alloyed powder are completely equal to target alloy components. In the hot isostatic pressing process, the low-melting powder is melted to form a liquid phase, the liquid phase wets the surface of the high-melting powder, and impurities and oxide layers on the surfaces of powder particles are removed; and the liquid phase and the solid phase are rapidly and mutually diffused, isothermal solidification and component homogenization are achieved, and finally an equiaxed crystal powder high-temperature alloy structure which is uniform in structure and fine in grain is formed. The technology can be used for preparing the nickel-based powder high-temperature alloy and can also be used for preparing other high-temperature alloys. According to the method, the original powder particle boundary defect generated by the conventional hot isostatic pressing powder superalloy can be effectively avoided, the defect can be eliminated without adopting additional processing steps or adding additional chemical components, and the hot isostatic pressing formed powder superalloy component can be prepared with low cost and short process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of powder metallurgy high-temperature alloys, and provides a method for manufacturing high-performance powder high-temperature alloys with low cost and short process, thereby realizing the short process preparation of powder high-temperature alloys without original powder particle boundary defects. Background Art

[0002] Powder superalloy is a high-temperature structural material with no macrosegregation, uniform structure, fine grains, and excellent comprehensive mechanical properties. It has become the preferred material for manufacturing key hot end components such as turbine disks, compressor disks, and baffles of advanced aircraft engines. At present, powder superalloys are usually manufactured by solid powder hot isostatic pressing, but the powder superalloys prepared by this process will inevitably produce defects at the boundary of the original powder particles. This defect is a layer of fine and continuous second phase particles precipitated along the surface of the original solid powder, which will hinder the metallurgical bonding between the powder particles and is a potential crack source. This defect damages the mechanical properties of the powder superalloy, especially the impact toughness and low-cycle fatigue performance, and seriously endangers the reliability of the powder superalloy material [Huang Xina, Guo Sirui, Yue Wen, et al. Research status of the original particle boundary of powder superalloy prepared by hot isostatic pressing [J]. Powder Metallurgy Technology, 2023, 41(05): 402-409+419.].

[0003] In order to effectively eliminate or avoid the defects of the original powder particle boundaries of powder high-temperature alloys, researchers at home and abroad have conducted extensive research. Current research results show that the second phase particles on the boundaries of the original powder particles are generally related to the alloy composition, usually composed of MC-type carbides and oxides, and cannot be eliminated by conventional heat treatment and other processes. At present, the general measures to prevent or eliminate the boundaries of the original powder particles are mainly the following: (1) Using the "hot isostatic pressing + hot plastic processing" process, hot extrusion, isothermal forging and other hot plastic processing are performed on the hot isostatic pressed powder high-temperature alloy to mechanically crush the second phase particles on the surface of the solid phase powder [A nickel-based powder high-temperature alloy and its forming method, publication number: CN111647764A; Elimination of the critical deformation amount and extrusion process parameter determination method of powder high-temperature alloy PPB, publication number: CN113343516A]. This process method can effectively eliminate the defects of the original powder particle boundaries of the powder, but it requires expensive large-scale hot plastic processing equipment, greatly increases the process cost, prolongs the process flow, and has poor process stability. (2) Control the composition of high-temperature alloys, add strong carbide-forming elements such as Hf to powder metallurgy high-temperature alloys, strictly reduce the carbon content, and reduce the tendency of carbides to precipitate at the boundaries of original powder particles, but this method can only eliminate the boundaries of original powder particles to a certain extent. (3) Use the "powder low-temperature heat treatment + hot isostatic pressing" process, first preheat the solid phase powder within a certain temperature range to form stable carbides inside the powder, and then perform hot isostatic pressing [A device and method for preparing fine-grained powder high-temperature alloy hot isostatic pressing parts, publication number: CN114210977A; A method and device for automatic vacuum degassing of metal powders, publication number: CN114192773A] This method can reduce the severity of defects at the boundaries of original powder particles, but it cannot completely eliminate defects. It also requires additional process steps and equipment, increasing manufacturing costs. (4) Two-step hot isostatic pressing process, in which the temperature is first raised to a higher level during the heating process, and then the temperature is lowered for hot isostatic pressing sintering [a hot isostatic pressing molding method for nickel-based high-temperature alloy powder, publication number: CN110666175A]. This process can only suppress the original powder particle boundary defects of the powder high-temperature alloy to a certain extent, but cannot completely eliminate them, and this process is only applicable to high-temperature alloys with special components. (5) The "powder high-temperature atmosphere reduction + hot isostatic pressing" process is adopted. This process places the powder in a high-temperature CO atmosphere for reduction treatment to remove oxygen attached to the powder surface and avoid carbides and oxides from nucleating and growing on the surface of the powder particles, thereby eliminating the original powder particle boundaries [a device and method for preparing fine-grained powder high-temperature alloy hot isostatic pressing parts, publication number: CN114210977A]. This method can eliminate the original powder particle boundaries, but requires additional process steps and special equipment, which increases the process cost.(6) The "oscillation pressure sintering" process uses a special process equipment with axial oscillation pressure to prepare powder high-temperature alloys [a method for preparing fine-grained powder high-temperature alloys that inhibits the formation of original powder particle boundaries, publication number: CN111304476A]. It can effectively eliminate the original powder particle boundaries, but is only suitable for preparing small experimental samples. The preparation of large samples will produce serious density non-uniformity and cannot be used on a large scale.

[0004] Obviously, thermoplastic processing can effectively eliminate the original powder particle boundary defects of powder high temperature alloys, but it increases the process cost and prolongs the process flow. Other methods to avoid or eliminate the original powder particle boundary are in the experimental stage, and the process effect is not good. Therefore, it is urgent to develop a low-cost, short-process process for preparing powder metallurgy high temperature alloys without original powder particle boundaries suitable for industrial production. Summary of the invention

[0005] The invention discloses a process method for directly manufacturing a powder high-temperature alloy without original powder particle boundaries by hot isostatic pressing, which realizes low-cost short-process manufacturing without hot plastic processing or adding alloy elements and avoids the original powder particle boundary defects in the hot isostatic pressed powder high-temperature alloy.

[0006] A method for manufacturing high-performance powder high-temperature alloys with low cost and short process, characterized in that two pre-alloyed powders with different melting points are used as sintering raw materials, and the comprehensive composition of the two pre-alloyed powders is completely equivalent to the target alloy composition; during the sintering process, the low-melting alloy powder melts to form a liquid phase to fully wet the particle surface, clean up impurities attached to the particle surface, and undergo solid-liquid interdiffusion with the high-melting powder to achieve isothermal solidification, and finally form a high-performance powder high-temperature alloy without original powder particle boundaries.

[0007] The method for manufacturing high-performance powder high-temperature alloy with low cost and short process as described above has the following specific process steps:

[0008] 1) According to the chemical composition of the powder high-temperature alloy to be prepared, design and prepare low-melting alloy powder and high-melting alloy powder. The particle size of the alloy powder should be less than or equal to 100 microns, and the shape of the alloy powder should be nearly spherical powder;

[0009] 2) Weigh low-melting alloy powder and high-melting alloy powder according to the required mass ratio, and mix them evenly by ball milling. The ball mill speed is 120-200r / min, and the ball milling time is 120-150min;

[0010] 3) Fill the mixed powder into a low-carbon steel jacket, degas at a high temperature of 180°C to 300°C, and then perform vacuum sealing;

[0011] 4) placing the prepared package in a hot isostatic pressing device, and performing hot isostatic pressing sintering by simultaneously increasing the temperature and pressure or first increasing the temperature and then increasing the pressure; the sintering temperature is 1150-1300°C, the holding time is 2-4h, and the sintering pressure is 120-150MPa;

[0012] 5) After the hot isostatic pressing process is completed, take out the sample when the furnace temperature cools to room temperature.

[0013] Furthermore, in the two mixed powders with different melting points, the low-melting alloy powder is a binary, ternary or multi-element alloy powder of common elements in high-temperature alloys (Ni, Cr, Co, Ti, Al, Ta), with a melting point lower than 1250°C and a volume fraction of 10%-50% in the mixed powder; the high-melting alloy powder composition is determined by the target alloy composition, and the high-melting alloy composition is designed according to the requirement that the mixed composition of the high-melting alloy powder composition and the low-melting alloy powder composition is the target powder high-temperature alloy composition.

[0014] Furthermore, the low-melting alloy powder composition is Ni-Al-Ta-Ti, and the mass percentage is: Ta 14.5-16.5wt.%, Al 6.0-7.0wt.%, Ti 14.8-15.8wt.%, and the balance is Ni. The mass percentage composition of the selected high-melting alloy powder includes but is not limited to: Cr 15.5-16.5wt.%, Co 14.0-15.0wt.%, Mo 5.0-5.5wt.%, W5.0-5.5wt.%, Nb 2.6-3.0wt.%, C 0.025-0.045wt.%, and the balance is Ni.

[0015] Furthermore, the low-melting alloy powder composition is Ni-Cr-Ta-Ti, and the mass percentage is: Cr 11.7-12.5wt.%, Ta 3.2-4.5wt.%, Ti 9.2-10.9wt.%, and the balance is Ni. The mass percentage composition of the selected high-melting alloy powder includes but is not limited to: Cr 11.5-13.5wt.%, Co 9.0-11.0wt.%, Mo 1.0-3.5wt.%, W9.0-10.5wt.%, Nb 0.6-1.0wt.%, C 0.025-0.045wt.%, and the balance is Ni.

[0016] Further, the low-melting alloy powder composition is Ni-Co-Ti-Al-Ta, and the mass percentage is: Co 13.7-14.5wt.%, Ti 5.6-7.5wt.%, Al 3.3-3.9wt.%, Ta 14.8-19.8wt.%, and the balance is Ni. The mass percentage composition of the selected high-melting alloy powder includes but is not limited to: Cr 4.5-8.5wt.%, Co 5.0-7.0wt.%, Mo3.0-7.5wt.%, W 1.0-3.5wt.%, Nb 1.6-2.0wt.%, C 0.015-0.025wt.%, and the balance is Ni.

[0017] Further, the low-melting alloy powder composition is Ni-Cr-Co-Al-Ta, and the mass percentage is: Co 13.7-14.5wt.%, Cr 5.6-7.5wt.%, Al 3.2-5.9wt.%, Ta 18.8-19.8wt.%, and the balance is Ni. The mass percentage composition of the selected high-melting alloy powder includes but is not limited to: Cr 14.5-18.5wt.%, Co 15.0-16.0wt.%, Mo 0.5-3.5wt.%, W 2.0-1.5wt.%, Nb 4.6-5.0wt.%, C 0.015-0.025wt.%, and the balance is Ni.

[0018] Further, the low-melting alloy powder composition is Ni-Cr-Co-Al-Ti, and the mass percentage is: Cr 15.7-16.5wt.%, Co 8.2-9.5wt.%, Al 6.2-7.9wt.%, Ti 14.8-19.8wt.%, and the balance is Ni. The mass percentage composition of the selected high-melting alloy powder includes but is not limited to: Cr 14.9-17.1wt.%, Co 12.1-13.5wt.%, Mo 3.2-4.1wt.%, W 4.1-5.0wt.%, Al 1.9-2.1wt.%, Nb 1.9-2.7wt.%, C 0.045-0.065wt.%, and the balance is Ni.

[0019] Further, the low-melting alloy powder composition is Ni-Cr-Al-Ta-Ti, and the mass percentage is: Cr 11.7-12.5wt.%, Al 6.2-7.9 wt.%, Ta 8.2-9.5 wt.%, Ti 14.8-19.8wt.%, and the balance is Ni. The mass percentage composition of the selected high-melting alloy powder includes but is not limited to: Cr 11.9-13.1wt.%, Co 12.8-11.5wt.%, Mo 3.2-5.1wt.%, W 2.1-3.1wt.%, Al 2.9-3.1 wt.%, Nb 0.9-1.7wt.%, C 0.041-0.051wt.%, and the balance is Ni.

[0020] Furthermore, the low-melting alloy powder composition is Ni-Ti, and the mass percentage is: Ti 68.0-72.0wt.%, and the balance is Ni. The mass percentage composition of the selected high-melting alloy powder includes but is not limited to: Cr 16.5-17.5wt.%, Co13.5-14.5wt.%, Mo 4.2-4.8wt.%, W 4.2-4.8wt.%, Al 2.3-2.5wt.%, Nb 2.6-3.0wt.%, C 0.055-0.085wt.%, and the balance is Ni.

[0021] Furthermore, the low-melting alloy powder is Ni-Al, with a mass percentage of Al 90.0-92.0wt.%, and the balance is Ni. The mass percentage components of the selected high-melting alloy powder include but are not limited to: Cr 9.5-11.5wt.%, Co 11.0-13.0wt.%, Mo 2.0-3.0wt.%, Nb 0.5-1.0wt.%, C 0.021-0.035wt.%, and the balance is Ni.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The present invention proposes a new process method to avoid the appearance of powder original powder particle boundaries in hot isostatic pressed powder high-temperature alloys, without the need for additional processing steps and additional chemical component additions, which can reduce process costs, improve production efficiency, and achieve low-cost and short-process preparation of high-performance powder high-temperature alloys. This technology can be used to prepare nickel-based powder high-temperature alloys and can also be used to prepare other high-temperature alloys.

[0024] 2. The physical process of preparing powder high-temperature alloys in the present invention is an isothermal solidification process. During the sintering process, the low-melting powder melts to form a liquid phase, the liquid phase wets the surface of the high-melting powder particles, the components between the liquid phase and the solid phase diffuse, the surface of the solid phase powder is slightly dissolved, and the liquid phase begins to solidify isothermally, realizing the rapid manufacture of equiaxed crystal powder high-temperature alloys with uniform structure and fine grains. In this process, there are no physical conditions for forming the boundaries of the original powder particles, and this defect is completely avoided. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a schematic diagram of the process principle for preparing a powder high-temperature alloy without original powder particle boundaries according to the present invention.

[0026] Figure 2 This is a scanning electron microscope photograph of the powder high-temperature alloy structure in Example 1. DETAILED DESCRIPTION

[0027] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments, but the protection scope of the present invention is not limited thereto.

[0028] The present invention is a process method for avoiding the boundary defects of the original powder particles of the hot isostatic pressing powder high-temperature alloy and manufacturing high-performance powder high-temperature alloy in a short process. The specific process of this embodiment includes the following steps:

[0029] 1) According to the chemical composition of the powder high-temperature alloy to be prepared, design and prepare low-melting alloy powder and high-melting alloy powder. The particle size of the alloy powder should be less than or equal to 100 microns, and the shape of the alloy powder should be nearly spherical powder.

[0030] 2) Weigh low-melting alloy powder and high-melting alloy powder according to the required mass ratio, and mix them evenly with ball mill at a speed of 120-200 r / min and a ball milling time of 120-150 min.

[0031] 3) Fill the mixed powder into a low-carbon steel sheath, degas at a high temperature of 180°C to 300°C, and then perform vacuum sealing.

[0032] 4) Place the prepared package in a hot isostatic pressing device, and heat and press simultaneously or heat and press first and then press to perform hot isostatic pressing sintering. The sintering temperature is 1150-1300°C, the holding time is 2-4h, and the sintering pressure is 120-150MPa.

[0033] 5) After the hot isostatic pressing process is completed, take out the sample when the furnace temperature cools to room temperature.

[0034] Example 1

[0035] In this embodiment, the existing powder high-temperature alloy FGH4096 is prepared by the process of the present invention, and the mass fractions of the alloy components are: Cr 15.5-16.5wt.%, Co 12.5-13.5wt.%, W 3.8-4.2wt.%, Mo 3.8-4.2wt.%, Al2.0-2.4wt.%, Ti 3.5-3.9wt.%, Nb 0.6-0.8wt.%, C 0.045-0.060wt.%, and the balance is Ni.

[0036] The specific process is as follows:

[0037] 1) The designed mass fraction of low-melting alloy powder is: Ti 68.0~72.0wt.%, and the balance is Ni; the mass percentage of high-melting alloy powder is: Cr 16.5~17.5wt.%, Co 13.5~14.5 wt.%, Mo 4.2~4.8wt.%, W 4.2~4.8wt.%, Al 2.3~2.5 wt.%, Nb 2.6~3.0wt.%, C 0.045~0.065wt.%; the particle size of the powder is less than or equal to 100 microns, and the shape of the powder is nearly spherical powder.

[0038] 2) Weigh the two powders and mix them evenly by ball milling. The ball milling speed is 150 r / min and the ball milling time is 120 min. The volume fraction of the low-melting alloy powder is 8%.

[0039] 3) Fill the mixed powder into a low-carbon steel bag, degas at 250°C, and then perform vacuum sealing.

[0040] 4) Place the prepared package in a hot isostatic pressing device, and heat and press simultaneously or heat and press first and then press to perform hot isostatic pressing sintering. The sintering temperature is 1180°C, the holding time is 4 hours, and the sintering pressure is 120 MPa.

[0041] 5) After the hot isostatic pressing process is completed, take out the sample when the furnace temperature cools to room temperature.

[0042] The prepared powder high-temperature alloy sample was cut open, the cross section was polished and then the structure was observed. No defects were found at the boundary of the original powder particles, such as Figure 1 shown.

[0043] Example 2

[0044] This embodiment adopts the process of the present invention to prepare a high-temperature alloy, and the mass fractions of the alloy components are: Cr 15.5-16.5wt.%, Co 12.5-13.5wt.%, W 3.8-4.2wt.%, Mo 3.8-4.2wt.%, Al 2.0-2.4wt.%, Ta3.5-4.0wt.%, Ti 3.5-3.9wt.%, Nb 0.6-0.8wt.%, C 0.045-0.060wt.%, and the balance is Ni and unavoidable impurities.

[0045] The specific process is as follows:

[0046] 1) The designed mass fraction of low-melting alloy powder is: Ta 15.5~16.5wt.%, Al 6.0~7.0 wt.%, Ti14.8~15.8wt.%, and the balance is Ni; the mass percentage of high-melting alloy powder is: Cr 15.5~16.5wt.%, Co 14.0~15.0wt.%, Mo 5.0~5.5wt.%, W 5.0~5.5wt.%, Nb 2.6~3.0wt.%, C 0.045~0.065wt.%, and the balance is Ni and unavoidable impurities; the particle size of the powder is less than or equal to 100 microns, and the shape of the powder is nearly spherical powder.

[0047] 2) Weigh the two powders and mix them evenly by ball milling. The ball milling speed is 100r / min and the ball milling time is 150min. The volume fraction of the low-melting alloy powder is 30%.

[0048] 3) Fill the mixed powder into a low-carbon steel sheath, degas at 300°C, and then perform vacuum sealing.

[0049] 4) Place the prepared package in a hot isostatic pressing device, and heat and press simultaneously or heat and press first and then press to perform hot isostatic pressing sintering. The sintering temperature is 1180°C, the holding time is 4h, and the sintering pressure is 150MPa.

[0050] 5) After the hot isostatic pressing process is completed, take out the sample when the furnace temperature cools to room temperature.

[0051] Example 3

[0052] This embodiment adopts the process of the present invention to prepare an existing powder high-temperature alloy, and the mass fractions of the alloy components are: Cr 9.5-11.5wt.%, Co 12.5-13.5wt.%, Mo2.5-3.5wt.%, Al 6.0-7.0wt.%, Nb 0.6-0.8wt.%, C 0.045-0.060wt.%, and the balance is Ni.

[0053] The specific process is as follows:

[0054] 1) The designed mass fraction of low-melting alloy powder is: Al 90.0~92.0wt.%, the balance is Ni; the mass percentage of high-melting alloy powder is: Cr 9.5~11.5wt.%, Co 11.0~13.0wt.%, Mo 2.0~3.0wt.%, Nb 0.5~1.0wt.%, C 0.045~0.065wt.%, the balance is Ni and unavoidable impurities; the particle size of the powder is less than or equal to 100 microns, and the shape of the powder is nearly spherical powder.

[0055] 2) Weigh the two powders and mix them evenly by ball milling. The ball milling speed is 80r / min and the ball milling time is 150min. The volume fraction of the low-melting alloy powder is 15%.

[0056] 3) Fill the mixed powder into a low-carbon steel sheath, degas at 300°C, and then perform vacuum sealing.

[0057] 4) Place the prepared package in a hot isostatic pressing device, and heat and press simultaneously or heat and press first and then press to perform hot isostatic pressing sintering. The sintering temperature is 1200°C, the holding time is 2h, and the sintering pressure is 130MPa.

[0058] After the hot isostatic pressing process is completed, take out the sample when the furnace temperature cools to room temperature.

Claims

1. A method for manufacturing high-performance powder high-temperature alloys with low cost and short process, characterized in that: The sintering raw materials are two pre-alloyed powders with different melting points. The comprehensive composition of the two pre-alloyed powders is completely equivalent to the target alloy composition. During the sintering process, the low-melting alloy powder melts to form a liquid phase to fully wet the particle surface, clean up impurities attached to the particle surface, and undergo solid-liquid interdiffusion with the high-melting powder to achieve isothermal solidification, and finally form a high-performance powder high-temperature alloy without the original powder particle boundaries.

2. The method for manufacturing high-performance powder high-temperature alloy with low cost and short process according to claim 1 is characterized in that The specific process steps are as follows: 1) According to the chemical composition of the powder high-temperature alloy to be prepared, design and prepare low-melting alloy powder and high-melting alloy powder. The particle size of the alloy powder should be less than or equal to 100 microns, and the shape of the alloy powder should be nearly spherical powder; 2) Weigh low-melting alloy powder and high-melting alloy powder according to the required mass ratio, and mix them evenly by ball milling. The ball mill speed is 120-200r / min, and the ball milling time is 120-150min; 3) Fill the mixed powder into a low-carbon steel jacket, degas at a high temperature of 180°C to 300°C, and then perform vacuum sealing; 4) placing the prepared package in a hot isostatic pressing device, and performing hot isostatic pressing sintering by simultaneously increasing the temperature and pressure or first increasing the temperature and then increasing the pressure; the sintering temperature is 1150-1300°C, the holding time is 2-4h, and the sintering pressure is 120-150MPa; 5) After the hot isostatic pressing process is completed, take out the sample when the furnace temperature cools to room temperature.

3. The method for manufacturing high-performance powder high-temperature alloy with low cost and short process according to claim 1 or 2, characterized in that: The two mixed powders with different melting points are characterized in that the low-melting alloy powder is a binary, ternary or multi-element alloy powder of common elements in high-temperature alloys (Ni, Cr, Co, Ti, Al, Ta), has a melting point lower than 1250°C, and its volume fraction in the mixed powder is 10%-50%; the composition of the high-melting alloy powder is determined by the target alloy composition, and the high-melting alloy composition is designed according to the requirement that the comprehensive composition of the high-melting alloy powder composition and the low-melting alloy powder composition is the target powder high-temperature alloy composition.

4. The method for manufacturing high-performance powder high-temperature alloy with low cost and short process according to claim 3 is characterized in that: The low-melting alloy powder has a composition of Ni-Al-Ta-Ti, with the mass percentages being: Ta 14.5-16.5wt.%, Al 6.0-7.0wt.%, Ti 14.8-15.8wt.%, and the balance being Ni; the high-melting alloy composition matched with the low-melting alloy composition is Cr 15.5-16.5wt.%, Co 14.0-15.0wt.%, Mo 5.0-5.5wt.%, W 5.0-5.5wt.%, Nb 2.6-3.0wt.%, C0.025-0.045wt.%, and the balance being Ni.

5. The method for manufacturing high-performance powder high-temperature alloy with low cost and short process according to claim 3 is characterized in that: The low-melting alloy powder composition is Ni-Cr-Ta-Ti, and the mass percentage is: Cr 11.7-12.5wt.%, Ta 3.2-4.5wt.%, Ti 9.2-10.9 wt.%, and the balance is Ni; the high-melting alloy composition matched with the low-melting alloy composition is Cr 11.5-13.5wt.%, Co 9.0-11.0wt.%, Mo 1.0-3.5wt.%, W 9.0-10.5wt.%, Nb 0.6-1.0wt.%, C0.025-0.045wt.%, and the balance is Ni.

6. The method for manufacturing high-performance powder high-temperature alloy with low cost and short process according to claim 3 is characterized in that: The low-melting alloy powder composition is Ni-Cr-Co-Al-Ti, and the mass percentage is: Cr 15.7-16.5wt.%, Co 8.2-9.5 wt.%, Al 6.2-7.9 wt.%, Ti 14.8-19.8wt.%, and the balance is Ni; the high-melting alloy composition matched with the low-melting alloy composition is Cr 14.9-17.1wt.%, Co 12.1-13.5 wt.%, Mo 3.2-4.1wt.%, W 4.1-5.0wt.%, Al 1.9-2.1 wt.%, Nb 1.9-2.7wt.%, C 0.045-0.065wt.%, and the balance is Ni.

7. The method for manufacturing high-performance powder high-temperature alloy with low cost and short process according to claim 3 is characterized in that: The low-melting alloy powder composition is Ni-Cr-Co-Al-Ta, and the mass percentage is: Co 13.7~14.5wt.%, Cr 5.6~7.5 wt.%, Al 3.2~5.9 wt.%, Ta 18.8~19.8wt.%, and the balance is Ni; the high-melting alloy composition matched with the low-melting alloy composition is Cr 14.5~18.5wt.%, Co 15.0~16.0wt.%, Mo 0.5~3.5wt.%, W 2.0~1.5wt.%, Nb 4.6~5.0wt.%, C 0.015~0.025wt.%, and the balance is Ni.

8. The method for manufacturing high-performance powder high-temperature alloy with low cost and short process according to claim 3 is characterized in that: The low-melting alloy powder composition is Ni-Ta-Ti, and the mass percentage is: Ta 15.7~16.5wt.%, Ti 14.8~19.8wt.%, and the balance is Ni; the high-melting alloy composition matched with the low-melting alloy composition is Cr 14.9~17.1wt.%, Co 12.1~13.5 wt.%, Mo 3.2~4.1wt.%, W 4.1~5.0wt.%, Nb 1.9~2.7wt.%, C 0.045~0.065wt.%, and the balance is Ni.

9. The method for manufacturing high-performance powder high-temperature alloy with low cost and short process according to claim 3, characterized in that: The low-melting alloy powder composition is Ni-Cr-Al-Ta-Ti, and the mass percentage is: Cr 11.7~12.5wt.%, Al 6.2~7.9 wt.%, Ta 8.2~9.5 wt.%, Ti 14.8~19.8wt.%, and the balance is Ni; the high-melting alloy composition matched with the low-melting alloy composition is Cr 11.9~13.1wt.%, Co 12.8~11.5 wt.%, Mo 3.2~4.1wt.%, W 2.1~5.1wt.%, Al 2.9~3.1 wt.%, Nb 0.9~1.7wt.%, C 0.041~0.051wt.%, and the balance is Ni.

10. The method for manufacturing high-performance powder high-temperature alloy with low cost and short process according to claim 3, characterized in that: The low-melting alloy powder has a composition of Ni-Ti, with a mass percentage of: Ti 68.0-72.0wt.%, and the balance is Ni; the high-melting alloy composition matched with the low-melting alloy composition is Cr 16.5-17.5wt.%, Co 13.5-14.5 wt.%, Mo 4.2-4.8wt.%, W 4.2-4.8wt.%, Al 2.3-2.5 wt.%, Nb 2.6-3.0wt.%, C 0.055-0.085wt.%, and the balance is Ni.

Citation Information

Cited By

  • Preparation method of powder metallurgy prefabricated part for nickel-based superalloy damage defect shape remodeling and prefabricated part

    CN120325972A

  • Method for manufacturing powder superalloy

    WO2026008002A1