Welding process method for folding butt joint circular seam of 1000 MPa strength grade water diversion steel pipe

Through the asymmetric welding bevel design and high-frequency pulse DC welding mode, combined with ultrasonic non-destructive detection, the high restraint stress and welding cold cracking tendency of the closed butt joint of the 1000MPa steel pipe is solved, and high-quality welding is achieved to avoid Weld cracks and residual stress problems are solved to ensure the success of welding.

CN118875437APending Publication Date: 2024-11-01CHINA THREE GORGES PROJECTS DEV CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411017394.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the water turbine generator set, the closing butt joint joint joint welding of the 1000MPa strength grade water diversion steel pipe has high restraint stress and a high tendency to weld cold cracks, which makes it difficult to solve the welding crack problem.

Method used

Adopt asymmetric welding bevel design, melted electrode gas protective welding, equal strength high plastic toughness welding wire, one-way pulse DC reverse mode and segmented interval welding sequence, combined with ultrasonic non-destructive detection, improve the plastic toughness and welding quality of weld metal , reduce pores and residual stresses inside the weld.

Benefits of technology

Effectively suppress the occurrence of cold cracks in welding, ensure the quality of welds and the success of welding, reduce cracking problems caused by residual stress in welds, and improve the welding performance of 1000MPa strength grade water-transmitting steel pipes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118875437A_ABST
    Figure CN118875437A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of water-turbine generator sets, and discloses a welding process method for folding and butt-joint circular seams of water diversion steel pipes with the strength grade of 1000 MPa. By combining the high restraint stress state and the high welding cold crack tendency characteristic of the folding and butt-joint circular seams of the water diversion steel pipes with the strength grade of 1000 MPa, welding grooves of the folding and butt-joint circular seams are designed to be of an asymmetric structure; the depth h1 of the front side area of a welding groove is 70% of the thickness t of a butt joint circular seam, ternary weak oxidizing mixed welding protective gas is used, the welding electrical characteristic is a unitary pulse direct current reverse connection mode, the welding preheating temperature T0 is larger than or equal to 130 DEG C, the interlayer temperature T1 is 130-170 DEG C, welding is conducted in a segmented and spaced mode, and heat preservation is conducted for 4-6 hours within the temperature range of 250-280 DEG C after welding. According to the welding process provided by the invention, the plasticity and toughness of welding seam metal of the water diversion steel pipe closure butt-joint girth with the strength grade of 1000 MPa can be improved, the defect of air holes in the welding seam is reduced, the welding seam quality is improved, the residual stress after welding is improved, and the generation of welding cracks of the water diversion steel pipe closure butt-joint girth with the strength grade of 1000 MPa is inhibited.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of hydro-turbine generator sets, and in particular to a welding process for closing and butting annular seams of a water diversion steel pipe with a strength grade of 1000MPa. Background Art

[0002] With the needs of my country's economic development, the demand for energy continues to increase. More and more hydropower generators that use water potential energy to convert into electrical energy are being developed and built, and are developing in the direction of high-head, large-capacity, and high-power generators. As an important water diversion component of a hydropower generator, the demand for steel plates for water diversion steel pipes has gradually developed in the direction of high reinforcement and thickening. Since the mid-1970s, the scale of steel used for water diversion steel pipes has grown exponentially, and 600MPa and 800MPa strength grade steel plates have been widely used. With the construction of ultra-high head pumped storage hydropower stations, 1000MPa strength grade steel plates have begun to be used to manufacture water diversion steel pipes, achieving a series of benefits such as reducing the weight of steel plates, reducing welding, shortening the manufacturing and installation period, and reducing the cost of power station construction. The closed butt joint annular seam of the water diversion steel pipe is welded under a strong restrained stress state after the butt welds of other pipe sections are welded. The welding process of the closed butt joint annular seam mainly solves the problem of welding cracks under a high restrained state, especially for the water diversion steel pipe made of 1000MPa strength grade high-strength steel plate with a high tendency of welding cold cracking. The present invention combines the high restrained stress state and high welding cold cracking tendency characteristics of the closed butt joint annular seam of the 1000MPa strength grade water diversion steel pipe to provide a welding process for the closed butt joint annular seam of the 1000MPa strength grade water diversion steel pipe. Summary of the invention

[0003] The present invention provides a welding process for closing and butting the annular seam of a water diversion steel pipe with a strength level of 1000MPa. The present invention is achieved through the following technical solutions:

[0004] S1. The welding groove of the water diversion steel pipe is designed to be an asymmetric groove structure, and the depth h1 of the positive side area of ​​the welding groove is 70% of the thickness t of the butt joint;

[0005] S2. The butt joint is welded by using metal arc welding equipment. The welding shielding gas is a ternary weak oxidizing mixed shielding gas with a shielding gas component ratio of 60% Ar + 30% He + 10% CO2.

[0006] S3. Use equal strength high plastic toughness welding wire for closing butt joint. The yield strength of the deposited metal is R p0.2 800~890MPa, tensile strength R m 950~1050MPa, elongation A≥16%, impact toughness KV2≥47J at -60℃;

[0007] S4. The welding electrical characteristics used for the closed butt girth welding are the single-element pulse DC reverse connection mode;

[0008] S5. The welding preheating temperature T0 during the welding of the closed butt joint is ≥130℃, and the interlayer temperature T1 is 130~170℃;

[0009] S6, the closed butt joint ring seam is evenly distributed along the circumference into 8 weld sections, namely weld section 1, weld section 2, weld section 3, weld section 4, weld section 5, weld section 6, weld section 7, and weld section 8, firstly, the positive side areas of the welding grooves of weld section 1, weld section 3, weld section 5, and weld section 7 are completed synchronously without stopping welding; then, the positive side areas of the welding grooves of weld section 2, weld section 4, weld section 6, and weld section 8 are completed synchronously without stopping welding;

[0010] S7. Grind and remove the root weld on the positive side of the welding groove in the back area of ​​the closed butt joint annular seam;

[0011] S8, synchronously welding the back side areas of the welding grooves of weld section 1, weld section 2, weld section 3, weld section 4, weld section 5, weld section 6, weld section 7, and weld section 8;

[0012] S9, after completing step S8, on the basis of preheating temperature T0 ≥ 130°C, the temperature of the closed butt joint annular seam and the surrounding area within the range of 3 times the weld thickness t after welding is rapidly raised to 250°C, and kept in the temperature range of 250-280°C for 4-6 hours;

[0013] S10, according to step S9, the closed butt joint annular seam is kept at a temperature range of 250-280° C. for 4-6 hours and cooled to room temperature for 72 hours, and then non-destructive flaw detection of the closed butt joint annular seam is performed using two non-destructive flaw detection technologies, ultrasonic pulse echo and ultrasonic diffraction time difference.

[0014] Furthermore, in step S1, the welding groove of the closed butt joint of the water diversion steel pipe is designed to be an asymmetric K-type or X-type groove structure.

[0015] Furthermore, in step S2, the welding shielding gas composition ratio is 50% Ar+45% He+5% CO2.

[0016] Furthermore, in step S4, the welding process parameters for closing the butt joint are as follows: the pulse frequency f is 190-210 Hz, the average welding current I is 240-260 A, the welding voltage U is 25-27 V, and the welding line energy q is 20-25 kJ / cm.

[0017] Furthermore, in step S5, the preheating range of the closed butt joint annular seam welding is the closed butt joint annular seam and the surrounding area within a range of 3 times the weld thickness t.

[0018] Technical Effects

[0019] 1. The present invention combines the high welding cold crack tendency characteristics of the 1000MPa strength grade water diversion steel pipe, and uses high plasticity and toughness welding materials, ternary weakly oxidizing mixed welding shielding gas, and a one-element pulse DC reverse electrical characteristic mode to improve the plasticity and toughness of the weld metal, reduce the internal pores of the weld, and inhibit the generation of welding cold cracks under high constraint conditions to ensure the quality of the weld.

[0020] 2. The present invention combines the high restraint stress state characteristics of the closed butt joint annular seam of the water diversion steel pipe, designs an asymmetric closed butt joint annular seam welding groove structure, and adopts a segmented interval welding sequence to improve the residual stress state of the closed weld of the water diversion steel pipe, avoid cracking caused by the residual stress of the weld being higher than the fracture strength of the weld metal, and ensure the successful welding of the closed weld of the water diversion steel pipe with a strength grade of 1000MPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The following is a brief introduction to the drawings required for use in the embodiments of the present invention.

[0022] Figure 1 This is a schematic diagram of the closed butt-jointed circumferential seam welding structure of the 1000MPa strength grade water diversion steel pipe.

[0023] Figure 2 This is the asymmetric X-shaped welding groove diagram of the closed butt circumferential seam of the 1000MPa strength grade water diversion steel pipe.

[0024] Figure 3 for Figure 1 A--A cross-sectional view.

[0025] Figure 4 This is the asymmetric K-type welding groove diagram of the closed butt annular seam of the 1000MPa strength grade water diversion steel pipe.

[0026] Description of reference numerals:

[0027] 1- water diversion steel pipe; 2- closed butt joint; 3- front side area of ​​welding groove; 4- back side area of ​​welding groove; 5- weld section 1; 6- weld section 2; 7- weld section 3; 8- weld section 4; 9- weld section 5; 10- weld section 6; 11- weld section 7; 12- weld section 8. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical scheme and technical effect of the present invention clearer, further explanation will be given below in conjunction with the drawings and specific embodiments, but each embodiment does not constitute a limitation of the present invention. The specific implementation methods described in the drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0029] The present invention combines the high restraint stress state and high welding cold crack tendency characteristics of the 1000MPa strength grade water diversion steel pipe closed butt joint annular seam, provides a high plastic toughness welding process, solves the 1000MPa strength grade water diversion steel pipe closed butt joint annular seam welding crack problem, the specific implementation of the present invention is:

[0030] Embodiment 1:

[0031] S1, such as Figure 1 and Figure 2 As shown, the welding groove of the water diversion steel pipe 1 closing the butt joint circumferential seam 2 is designed as an asymmetric X-shaped structure, and the depth h1 of the positive side area 3 of the welding groove is 70% of the thickness t of the butt joint circumferential seam 2;

[0032] S2, butt joint 2 is welded by metal arc welding equipment, the welding shielding gas is a ternary weak oxidizing mixed shielding gas, the component ratio is 60% Ar + 30% He + 10% CO2, and the shielding gas flow rate is 18-22L / min;

[0033] S3. The closed butt joint is welded with equal strength high plastic toughness welding wire. The yield strength of the deposited metal is R p0.2 800~890MPa, tensile strength R m 950~1050MPa, elongation A≥16%, impact toughness KV2≥47J at -60℃;

[0034] S4, the welding electrical characteristics used for the welding of the closed butt joint 2 are a single-element pulse DC reverse connection mode, the welding process parameters are a pulse frequency f of 190-210 Hz, an average welding current I of 240-260 A, a welding voltage U of 25-27 V, and a welding line energy q of 20-25 kJ / cm;

[0035] S5. The welding preheating temperature T0 during the welding of the closed butt joint 2 is ≥ 130°C. The preheating range is the closed butt joint 2 and the surrounding area within 3 times the weld thickness t. The interlayer temperature T1 is 130-170°C.

[0036] S6, such as Figure 3 As shown, the closed butt joint circumferential seam 2 is evenly divided into 8 weld sections along the circumference, namely, weld section 1 5, weld section 2 6, weld section 3 7, weld section 4 8, weld section 5 9, weld section 6 10, weld section 7 11, and weld section 8 12. First, four welders synchronously and non-stop weld to complete the positive side area 3 of the weld groove of weld section 1 5, weld section 3 7, weld section 5 9, and weld section 7 11; then, four welders synchronously and non-stop weld to complete the positive side area 3 of the weld groove of weld section 2 6, weld section 4 8, weld section 6 10, and weld section 8 12;

[0037] S7. Grind and remove the root weld of the positive side area 3 of the welding groove in the back area 4 of the closed butt joint 2. When grinding and removing, keep the preheating temperature of the closed butt joint 2 and the surrounding area within the range of 3 times the weld thickness t not less than 130°C;

[0038] S8, synchronously weld the back side area 4 of the weld groove of weld 1 section 5, weld 2 section 6, weld 3 section 7, weld 4 section 8, weld 5 section 9, weld 6 section 10, weld 7 section 11, and weld 8 section 12;

[0039] S9, after completing step S8, on the basis of the preheating temperature T0 ≥ 130°C, the temperature of the closed butt joint circumferential seam 2 and the surrounding area within the range of 3 times the weld thickness t after the welding is completed is rapidly raised to 250°C, and kept in the temperature range of 250-280°C for 4-6 hours;

[0040] S10. After the closed butt joint annular seam 2 is kept at a temperature range of 250 to 280° C. for 4 to 6 hours and cooled to room temperature for 72 hours according to step S9, the closed butt joint annular seam 2 is subjected to nondestructive testing by using ultrasonic pulse echo and ultrasonic diffraction time difference nondestructive testing techniques. After the test is qualified, the weld surface is subjected to nondestructive testing by using magnetic particle testing technology.

[0041] The welding groove of the closed butt joint of the water diversion steel pipe is designed as an asymmetric X-shaped groove structure. The depth h1 of the positive side area of ​​the welding groove is 70% of the thickness t of the butt joint. The root weld on the back of the closed butt joint can be removed on the basis of 70% of the thickness of the closed butt joint to avoid cracking due to insufficient weld strength when the root weld is removed from the back of the closed butt joint. The closed butt joint welding uses a ternary weakly oxidizing mixed welding shielding gas of 60% Ar+30% He+10% CO2. Compared with the traditional 80% Ar+20% CO2 binary mixed welding shielding gas, reducing the proportion of CO2 in the welding shielding gas can reduce the O content in the weld deposited metal and improve the plasticity and toughness of the weld metal. Adding 30% He can improve the wettability of the molten metal in the welding pool, which is beneficial to the escape of gas and welding slag inside the molten metal and reduces weld porosity. , slag inclusion defects are generated; the closed butt ring seam welding uses a single-element pulse DC mode, and the high-frequency pulse can effectively improve the fluidity of the molten pool metal. The larger arc force forms a mechanical impact and stirring on the molten pool, further increasing the escape rate of the gas and slag inside the molten metal in the welding molten pool, which can effectively reduce or even eliminate the weld porosity and slag inclusion defects, and improve the weld quality; the closed butt ring seam is evenly distributed along the circumference and is divided into 8 welds. First, when the front area of ​​the weld groove of 4 of them is welded synchronously at intervals, the welding stress can be released through the remaining 4 unwelded welds, and the peak residual stress inside the weld can be reduced; when the front area of ​​the weld groove of the remaining 4 welds is welded, the local compressive stress is generated on the 4 welds that were welded first due to the shrinkage of the welding joint, which can offset the tensile stress of part of the welding joint, improve the residual stress state of the closed weld of the water diversion steel pipe, and ensure the successful welding of the closed weld of the water diversion steel pipe.

[0042] Embodiment 2:

[0043] This embodiment is further improved on the basis of embodiment 1, such as Figure 4 As shown, the welding groove of the water diversion steel pipe 1 closing the butt annular seam 2 is designed as an asymmetric K-shaped groove structure, and the depth h1 of the positive side area 3 of the welding groove is 70% of the thickness t of the butt annular seam 2.

[0044] The welding groove of the closed butt joint of the water diversion steel pipe is designed as an asymmetric K-type groove structure. The welding groove only needs to be prepared on one side of the water diversion steel pipe. The water diversion steel pipe on the other side does not need to be prepared after increasing the installation adjustment margin and cutting off the remaining amount according to the actual installation size requirements, thereby reducing the workload of the water diversion steel pipe installation process and shortening the production cycle.

[0045] Embodiment 3:

[0046] This embodiment is further improved on the basis of the embodiment 1. The component ratio of the ternary weak oxidizing mixed shielding gas for welding is 50% Ar+45% He+5% CO2, and the shielding gas flow rate is 18-22 L / min.

[0047] The closed butt girth welding uses a ternary weakly oxidizing mixed welding shielding gas of 50% Ar + 45% He + 5% CO2, which further reduces the CO2 content in the welding shielding gas, reduces the O content in the weld deposited metal, and improves the plasticity and toughness of the weld metal; increases the He content in the welding shielding gas, further improves the wettability of the molten metal in the welding pool, increases the escape rate of gas and slag inside the molten metal, reduces weld porosity and slag inclusion defects, and improves weld quality.

[0048] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, it should be clear to those skilled in the art that the technical solutions described in the aforementioned embodiments may be modified, or some or all of the technical features therein may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A welding process for closing the butt joint of a 1000MPa strength grade water diversion steel pipe, characterized by comprising the following steps: S1. The welding groove of the water diversion steel pipe (1) closing the butt joint (2) is designed to be an asymmetric groove structure, and the depth h1 of the positive side area (3) of the welding groove is 70% of the thickness t of the butt joint (2); S2. Closing the butt joint (2) using a metal arc welding device, the welding shielding gas is a ternary weak oxidizing mixed shielding gas, the shielding gas component ratio is 60% Ar + 30% He + 10% CO2; S3. For butt welding, use equal strength high plastic toughness welding wire, and the yield strength of the deposited metal of the welding wire is R p0.2 800~890MPa, tensile strength R m 950~1050MPa, elongation A≥16%, impact toughness KV2≥47J at -60℃; S4. The welding electrical characteristics used in the welding of the closing butt joint (2) are a single-element pulse DC reverse connection mode; S5. During the welding process of closing the butt joint (2), the welding preheating temperature T0 is ≥ 130°C, and the interlayer temperature T1 is 130-170°C; S6, the closed butt joint ring seam (2) is evenly distributed along the circumference to form 8 weld sections, namely weld section 1 (5), weld section 2 (6), weld section 3 (7), weld section 4 (8), weld section 5 (9), weld section 6 (10), weld section 7 (11), and weld section 8 (12), firstly, the positive side area (3) of the welding groove of weld section 1 (5), weld section 3 (7), weld section 5 (9), and weld section 7 (11) is completed by synchronous and non-stop welding; then, the positive side area (3) of the welding groove of weld section 2 (6), weld section 4 (8), weld section 6 (10), and weld section 8 (12) is completed by synchronous and non-stop welding; S7, grinding and removing the root weld of the positive side area (3) of the welding groove in the back area (4) of the closed butt joint annular seam (2); S8, synchronously welding the back side area (4) of the welding groove of weld section 1 (5), weld section 2 (6), weld section 3 (7), weld section 4 (8), weld section 5 (9), weld section 6 (10), weld section 7 (11), and weld section 8 (12); S9, after completing step S8, on the basis of the preheating temperature T0 ≥ 130°C, the temperature of the closed butt joint annular seam (2) after welding and the surrounding area within the range of 3 times the weld thickness t is rapidly raised to 250°C, and kept in the temperature range of 250-280°C for 4-6 hours; S10, according to step S9, the closed butt joint annular seam (2) is kept at a temperature range of 250-280° C. for 4-6 hours and cooled to room temperature for 72 hours, and then non-destructive flaw detection is performed on the closed butt joint annular seam (2) using two non-destructive flaw detection techniques, ultrasonic pulse echo and ultrasonic diffraction time difference.

2. The welding process for closing the butt joint of a 1000MPa strength grade water diversion steel pipe according to claim 1 is characterized in that: In the step S1, the welding groove of the water diversion steel pipe (1) closing the annular seam (2) is designed to be an asymmetric K-shaped or X-shaped groove structure.

3. The welding process for closing the butt joint of a 1000MPa strength grade water diversion steel pipe according to claim 1 is characterized in that: In step S2, the welding shielding gas composition ratio is 50% Ar+45% He+5% CO2.

4. The welding process for closing the butt joint of a 1000MPa strength grade water diversion steel pipe according to claim 1 is characterized in that: In the step S4, the welding process parameters for closing the butt joint (2) are as follows: the pulse frequency f is 190-210 Hz, the average welding current I is 240-260 A, the welding voltage U is 25-27 V, and the welding line energy q is 20-25 kJ / cm.

5. The welding process for closing the butt joint of a 1000MPa strength grade water diversion steel pipe according to claim 1 is characterized in that: In the step S5, the welding preheating range of the closed butt joint annular seam (2) is the closed butt joint annular seam (2) and the surrounding area within the range of three times the weld thickness t.