Processing method of alloy composite part based on nano injection molding

Through the surface pretreatment, anodization and electrochemical deposition steps in nanoinjection molding technology, combined with toughened polyphenylene sulfide resin and silicon carbide whiskers, the problem of bonding strength difference caused by the difference in expansion coefficient between polyester materials and metals is solved. , significantly improve the interface bonding strength and durability of alloy composite parts.

CN118876327AActive Publication Date: 2024-11-01DONGGUAN YUKUN NANO INJECTION TECH CO LTD

Patent Information

Application Number
CN202410913793.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-01
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

In nano injection molding technology, the difference in expansion coefficients between polyester materials and metals leads to poor bonding power, warping, peeling and insufficient weather resistance after molding.

Method used

Using nano-injection molding-based alloy composite processing methods, including surface pretreatment, anodization treatment, electrochemical deposition and nano-injection molding steps, using toughened polyphenylene sulfide resin and silicon carbide whiskers and other materials, through double potential electrodeposition The nanoporous structure is formed by reaming the oxide film to improve the interface bonding strength between metal and plastic.

Benefits of technology

The interface bonding and durability of alloy composite parts are significantly improved, the problems of poor bonding and insufficient weathering in traditional methods are solved, and the mechanical properties and thermal expansion coefficient matching of the material are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of nano injection molding, and discloses a processing method of an alloy composite part based on nano injection molding, which comprises the following steps: surface pretreatment: sequentially carrying out oil removal, oxide film removal and chemical polishing treatment on the surface of an aluminum alloy; anodic oxidation treatment is conducted, specifically, the aluminum alloy subjected to surface pretreatment is sequentially subjected to first-time anodic oxidation, oxidation film removal, second-time anodic oxidation and oxidation film chambering; electrochemical deposition is conducted, specifically, the aluminum alloy subjected to anodic oxidation treatment is subjected to double-potential electrodeposition; and nanometer injection molding is conducted, specifically, the toughened polyphenylene sulfide resin serves as matrix resin to conduct nanometer injection molding on the surface of the aluminum alloy subjected to electrochemical deposition, and the alloy composite part is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nano injection molding, in particular to a processing method of an alloy composite part based on nano injection molding. Background Art

[0002] Nano Molding Technology (NMT) is a new technology that integrates metal and plastic. Through this technology, the metal surface is treated at the nano level, such as T treatment or E treatment, to form nano holes, and then the molten plastic is injected into the metal surface using an injection molding machine. These plastics enter the nano holes under pressure and cool and solidify, thus generating a strong bonding force called the "anchor effect". This technology not only improves the strength of the metal and plastic combined parts, but also simplifies the manufacturing process and reduces environmental impact.

[0003] NMT technology is widely used in the fields of communications, smart terminals, e-book readers, and tablet computers. In addition, NMT also shows great market potential in the fields of smart furniture and home appliances and lightweight automobiles. It is one of the important technologies in the era of 5G, logistics, and Internet of Vehicles. Although traditional methods such as adhesive bonding and insert injection molding have their own advantages, NMT achieves higher bonding strength and processing efficiency through nano-processing and injection molding.

[0004] Although NMT has significant advantages, there are also some problems in its application. The expansion coefficients of polyester materials and metals are quite different, which may lead to problems such as poor bonding between resin and metal after molding, warping, peeling and insufficient weather resistance. Therefore, it is of great significance to develop a processing method for alloy composite parts that can be applied to nano injection molding technology and have strong bonding with metal. Summary of the invention

[0005] The object of the present invention is to provide a processing method of an alloy composite part based on nano injection molding to solve the problems raised in the above background technology.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A processing method for alloy composite parts based on nano injection molding comprises the following steps:

[0008] S1: Surface pretreatment: Degreasing, removing oxide film and chemical polishing the aluminum alloy surface in sequence;

[0009] S2: Anodizing treatment: The aluminum alloy after surface pretreatment is subjected to first anodizing, oxide film removal, second anodizing, and oxide film pore expansion in sequence;

[0010] S3: Electrochemical deposition: The aluminum alloy after anodizing is subjected to double potential electrodeposition;

[0011] S4: Nano-injection molding: The toughened polyphenylene sulfide resin is used as a matrix resin to perform nano-injection molding on the surface of the aluminum alloy after electrochemical deposition to obtain an alloy composite part.

[0012] Furthermore, the degreasing step includes grinding the surface of the aluminum alloy flat, immersing it in acetone and anhydrous ethanol for ultrasonic cleaning for 5-10 minutes, taking it out, washing it with deionized water, and drying it.

[0013] Furthermore, the oxide film removal step includes immersing the degreased aluminum alloy in a mixed solution consisting of 30-35 g / L sodium hydroxide and 30-35 g / L sodium carbonate, heating to 55-60° C. for reaction for 40-45 seconds, taking out, washing with deionized water, and drying.

[0014] Objective To remove the loose, porous and uneven oxide film on the surface of aluminum alloy and avoid the decrease of orderliness of the oxide film obtained during the subsequent anodizing process.

[0015] Furthermore, the chemical polishing treatment step includes placing the aluminum alloy after the oxide film is formed into a mixed solution composed of 400-420g / L sodium hydroxide, 300-320g / L sodium nitrate, 60-65g / L sodium fluoride, and 100-120g / L sodium silicate, heating to 95-100°C for reaction for 1-5min, taking out, washing with deionized water, and drying.

[0016] Purpose To maintain the flatness of the aluminum alloy surface and facilitate the acquisition of a highly ordered oxide film during the subsequent anodizing process.

[0017] Furthermore, in the first anodization, the electrolyte is 0.3-0.6 mol / L oxalic acid solution, the oxidation voltage is 35-45 V, the oxidation temperature is 15-25° C., and the oxidation time is 4-4.5 h.

[0018] Furthermore, the oxide film removal step includes immersing the first anodized aluminum alloy in a mixed solution composed of 6-7wt% phosphoric acid and 1.8-2wt% chromic acid at 60-65° C. and reacting for 1-2 minutes.

[0019] Objective To remove the disordered oxide film formed by the first anodization and reduce the disorder of the nanopore size.

[0020] Furthermore, the oxidation time in the second anodization is 6-6.5 hours, and the other anodization process parameters are the same as those of the first anodization.

[0021] Objective To improve the orderliness and uniformity of the nanopore distribution and the aspect ratio of the nanopore size in the oxide film on the surface of aluminum alloy.

[0022] Furthermore, the oxide film pore expansion step includes immersing the aluminum alloy after the second anodization in a 6-7wt% phosphoric acid solution at 30-35°C for reaction for 15-30 minutes.

[0023] The purpose is to adjust the size of the nanopores to make them more uniform and improve orderliness; by expanding the pores, the cylindrical nanopores formed during the anodization process are expanded along the pore growth direction, and the bottom structure of the nanopores is expanded to form a "trapezoidal" truncated cone structure nanopore, thereby improving the anchoring performance. On the other hand, impurities on the surface of the oxide film are removed to facilitate the subsequent coating of the triazine dithiol polymer on the surface of the porous oxide film.

[0024] Furthermore, the oxalic acid solution solvent is anhydrous ethanol and deionized water in a volume ratio of 1:4.

[0025] Furthermore, in the anodization, the anode and cathode are aluminum alloy and graphite plate respectively.

[0026] Furthermore, the distance between the aluminum alloy and the graphite plate is 5 cm.

[0027] Furthermore, in the dual-potential electrodeposition, the aluminum alloy after anodization treatment is used as the working electrode, the saturated calomel electrode is used as the reference electrode, and the stainless steel sheet is used as the auxiliary electrode.

[0028] Furthermore, the electrolyte consists of 5-6 mmol / L triazine dithiol and 0.15-0.18 mol / L sodium nitrate solution.

[0029] Furthermore, in the dual potential deposition method, the step potential of step 1 is 1.6V, the step time is 30s, the step potential of step 2 is 6V, and the step time is 10s; the deposition temperature is 5-10°C.

[0030] The purpose is to form triazine dithiol metal salt on the surface of aluminum alloy, which can adsorb negatively charged compounds or react to form chemical bonds, thereby improving the interface bonding strength between plastic and metal of alloy composite parts; in the nano injection molding process, an anchoring effect is formed through the reaction between aluminum alloy-triazine dithiol metal salt-toughened polyphenylene sulfide resin, thereby further improving the interface bonding strength and the durability of the interface bonding strength.

[0031] Furthermore, the nano injection molding step includes injection pressurization, pressure holding, cooling, and ejection.

[0032] Furthermore, the injection speed is 250-350 mm / s, the injection pressure is 60-80 MPa, the holding pressure is 40-60 MPa, and the holding time is 8-10 s.

[0033] Objective To control the injection speed, injection pressure and holding pressure so that after the toughened polyphenylene sulfide resin molecular chains enter the truncated cone-shaped holes, the resin molecular chains will fill the truncated cone-shaped holes under the dragging and pressure of the molecular chains in the holes. Compared with the straight-up-down cylindrical holes, the truncated cone-shaped holes can form a mechanical interlocking structure between plastic and metal, further improving the interface bonding strength.

[0034] Furthermore, the diameter of the nano injection molding cylinder is 20 mm.

[0035] Furthermore, the temperatures of the zones of the nano injection molding cylinder are 270°C, 275°C, 265°C, 245°C, 10°C, and 75°C, and the mold temperature is 140°C.

[0036] Furthermore, the components of the toughened polyphenylene sulfide resin include polyphenylene sulfide, polybutylene terephthalate, silicon carbide whiskers, ethylene acrylic acid ethylene resin, glycidyl ester-containing random copolymer, antioxidant, and release agent.

[0037] Furthermore, the components in the toughened polyphenylene sulfide resin are calculated by weight as follows: 50-65 parts of polyphenylene sulfide, 15-30 parts of polybutylene terephthalate, 10-30 parts of silicon carbide whiskers, 1-10 parts of ethylene acrylic acid ethylene resin, 1-10 parts of glycidyl ester random copolymer, 0.1-1 parts of antioxidant, and 0.1-2 parts of release agent.

[0038] Furthermore, the glycidyl ester-containing random copolymer is a random copolymer of ethylene acrylate and glycidyl methacrylate.

[0039] Furthermore, the antioxidant is antioxidant 1098.

[0040] Furthermore, the release agent is release agent SEED.

[0041] Furthermore, the method for preparing the silicon carbide whisker comprises the following steps:

[0042] Add carbon silicon mixed powder, catalyst, aluminum powder and anhydrous ethanol into a ball mill, stir evenly, add phenolic resin, stir for 12-14 hours, press into billets, heat to 200-205°C and cure for 24 hours, heat the cured billet to 1200-1400°C at a heating rate of 5°C / min under coke conditions and keep warm for 2-2.5 hours, cool and grind to obtain silicon carbide whiskers.

[0043] Furthermore, the molar ratio of carbon to silicon in the carbon-silicon mixed powder is 1:1, and the catalyst includes any one of cobalt trioxide, chromium trioxide, and aluminum fluoride trihydrate.

[0044] Furthermore, the catalyst addition amount is 2-4wt% of the mass of the carbon silicon mixed powder, the aluminum powder addition amount is 1-1.5wt% of the total mass of the silicon carbide mixed powder and the catalyst, and the phenolic resin addition amount is 5-6wt% of the total mass of the carbon silicon mixed powder, the catalyst and the aluminum powder.

[0045] Furthermore, the carbon-silicon mixed body consists of silicon powder and nano carbon black.

[0046] Furthermore, the aluminum alloy includes any one of 6000 series aluminum alloy and 7000 series aluminum alloy.

[0047] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: the present invention uses polyphenylene sulfide as the main matrix resin, and uses polybutylene terephthalate, ethylene acrylic acid ethylene resin, and random copolymer containing glycidyl ester as composite toughening agents to toughen polyphenylene sulfide and improve its own mechanical properties; and selects silicon carbide whiskers with similar polarity, thermal expansion coefficient, and heat resistance as glass fiber to replace glass fiber as to enhance resin strength, adjust thermal expansion coefficient, reduce internal stress after metal material and plastic are combined, and enhance nano anchor effect; the self-made silicon carbide whiskers of the present invention have nanometer-scale diameter (50-90nm) and micrometer-scale length (5-7μm), and the size is much smaller than that of glass fiber, which solves the problem that the glass fiber is too large to enter the nanopores and is only in the resin outside the nanopores, resulting in a difference in thermal expansion coefficients inside and outside the nanopores, leading to the failure of the nano anchor effect. On this basis, the present invention further combines surface pretreatment, anodizing, and electrochemical deposition steps, so that the prepared alloy composite has excellent interface bonding force. DETAILED DESCRIPTION

[0048] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] In the following examples, nano carbon black was purchased from Tianjin Tianyi Chemical Co., Ltd.; silicon powder was purchased from Qinghe County Chaoneng Alloy Material Co., Ltd.; aluminum powder was purchased from Ruitai Magang New Material Technology Co., Ltd.; phenolic resin CAS: 9003-35-4 was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; polyphenylene sulfide model is CXP-500C, purchased from Zhuhai Changxian; polybutylene terephthalate model is 1200-211D; ethylene acrylic acid ethylene resin model is Amplify EA 102, purchased from Dow, USA; ethylene acrylate and methacrylate glycidyl ester random copolymer model is AX8900, purchased from Arkema, France; glass fiber model is ECS13-4.5-534A, purchased from China Jushi Co., Ltd.; the remaining raw materials are commercially available.

[0050] Embodiment 1: A processing method of alloy composite parts based on nano injection molding: S1: Preparation of silicon carbide whiskers: Add carbon-silicon mixed powder, catalyst, aluminum powder, and anhydrous ethanol into a ball mill, stir evenly, add phenolic resin, stir for 12-14 hours, press into a blank, heat to 200-205°C and cure for 24 hours, heat the solidified blank to 1200-1400°C at a heating rate of 5°C / min under coke conditions and keep warm for 2-2.5 hours, cool, and grind to obtain silicon carbide whiskers;

[0051] S2: Surface pretreatment: Grind the aluminum alloy surface flat, immerse it in acetone and anhydrous ethanol for ultrasonic cleaning for 5 minutes, take it out, wash it with deionized water, and dry it; immerse the deoiled aluminum alloy in a mixed solution composed of 30g / L sodium hydroxide and 30g / L sodium carbonate, heat it to 55℃ for reaction for 40s, take it out, wash it with deionized water, and dry it; put the aluminum alloy with oxide film into a mixed solution composed of 400g / L sodium hydroxide, 300g / L sodium nitrate, 60g / L sodium fluoride, and 100g / L sodium silicate, heat it to 95℃ for reaction for 2 minutes, take it out, wash it with deionized water, and dry it;

[0052] S3: Anodizing treatment: The aluminum alloy after surface pretreatment is used as the anode and the graphite plate is used as the cathode for the first anodizing in oxalic acid electrolyte. During the first anodizing process, the electrolyte is 0.3 mol / L oxalic acid solution, the oxidation voltage is 40 V, the oxidation temperature is 20°C, and the oxidation time is 4 hours; the aluminum alloy anodized for the first time is immersed in a mixed solution composed of 6wt% phosphoric acid and 1.8wt% chromic acid at 60°C, reacted for 1 minute, and the oxide film is removed; the aluminum alloy after the oxide film is removed is anodized for the second time, and the oxidation time is 6 hours; the aluminum alloy after the second anodizing is immersed in a 30°C, 6wt% phosphoric acid solution for reaction for 15 minutes, and the oxide film is expanded;

[0053] S4: Electrochemical deposition: The aluminum alloy after anodizing treatment is subjected to double potential electrodeposition; wherein, the aluminum alloy after anodizing treatment is used as the working electrode, the saturated calomel electrode is used as the reference electrode, and the stainless steel sheet is used as the auxiliary electrode; a mixed solution consisting of 5mmol / L triazine dithiol and 0.15mol / L sodium nitrate solution is used as the electrolyte; in the double potential deposition method, the step potential of step 1 is 1.6V, the step time is 30s, and the step potential of step 2 is 6V, the step time is 10s; the deposition temperature is 5℃;

[0054] S5: Nano-injection molding: The toughened polyphenylene sulfide resin is used as the matrix resin to perform nano-injection molding on the surface of the aluminum alloy after electrochemical deposition to obtain an alloy composite; wherein the toughened polyphenylene sulfide resin is composed of 65 parts of polyphenylene sulfide, 30 parts of polybutylene terephthalate, 10 parts of silicon carbide whiskers, 5 parts of ethylene acrylic acid ethylene resin, 5 parts of ethylene acrylate and glycidyl methacrylate random copolymer, 0.2 parts of antioxidant 1098, and 0.8 parts of mold release agent SEED; the injection speed in the nano-injection molding process is 300 mm / s, the injection pressure is 60 MPa, the holding pressure is 40 MPa, and the holding time is 8 s.

[0055] Example 2: A processing method for alloy composite parts based on nano-injection molding: S5: Nano-injection molding: Use toughened polyphenylene sulfide resin as a matrix resin to perform nano-injection molding on the surface of the aluminum alloy after electrochemical deposition to obtain an alloy composite part; wherein the toughened polyphenylene sulfide resin is composed of 65 parts of polyphenylene sulfide, 30 parts of polybutylene terephthalate, 20 parts of silicon carbide whiskers, 5 parts of ethylene acrylic acid ethylene resin, 5 parts of ethylene acrylate and glycidyl methacrylate random copolymer, 0.2 parts of antioxidant 1098, and 0.8 parts of mold release agent SEED; the injection speed in the nano-injection molding process is 300 mm / s, the injection pressure is 60 MPa, the holding pressure is 40 MPa, and the holding time is 8s.

[0056] The remaining steps are the same as those in Example 1.

[0057] Example 3: A processing method for alloy composite parts based on nano-injection molding: S5: Nano-injection molding: Use toughened polyphenylene sulfide resin as a matrix resin to perform nano-injection molding on the surface of the aluminum alloy after electrochemical deposition to obtain an alloy composite part; wherein the toughened polyphenylene sulfide resin is composed of 65 parts of polyphenylene sulfide, 30 parts of polybutylene terephthalate, 30 parts of silicon carbide whiskers, 5 parts of ethylene acrylic acid ethylene resin, 5 parts of ethylene acrylate and glycidyl methacrylate random copolymer, 0.2 parts of antioxidant 1098, and 0.8 parts of release agent SEED; the injection speed in the nano-injection molding process is 300 mm / s, the injection pressure is 60 MPa, the holding pressure is 40 MPa, and the holding time is 8 s.

[0058] The remaining steps are the same as those in Example 1.

[0059] Comparative Example 1: A processing method for alloy composite parts based on nano injection molding: S3: Anodizing treatment: The aluminum alloy after surface pretreatment is used as the anode and the graphite plate is used as the cathode for the first anodizing in oxalic acid electrolyte. During the first anodizing process, the electrolyte is 0.8 mol / L oxalic acid solution, the oxidation voltage is 40 V, the oxidation temperature is 20°C, and the oxidation time is 4 hours; the anodized aluminum alloy is immersed in a mixed solution of 6wt% phosphoric acid and 1.8wt% chromic acid at 60°C, reacted for 1 minute, and the oxide film is removed; the aluminum alloy after the oxide film is removed is anodized for a second time, and the oxidation time is 6 hours; the aluminum alloy after the second anodizing is immersed in a 30°C, 6wt% phosphoric acid solution for reaction for 15 minutes, and the oxide film is expanded.

[0060] The remaining steps are the same as those in Example 1.

[0061] Comparative Example 2: A processing method for alloy composite parts based on nano injection molding: S3: Anodizing treatment: The aluminum alloy after surface pretreatment is used as the anode and the graphite plate as the cathode for the first anodizing in oxalic acid electrolyte. During the first anodizing process, the electrolyte is 0.3 mol / L oxalic acid solution, the oxidation voltage is 60 V, the oxidation temperature is 20°C, and the oxidation time is 4 hours; the first anodized aluminum alloy is immersed in a mixed solution of 6wt% phosphoric acid and 1.8wt% chromic acid at 60°C, reacted for 1 minute, and the oxide film is removed; the aluminum alloy after the oxide film is removed is anodized for a second time, and the oxidation time is 6 hours; the aluminum alloy after the second anodizing is immersed in a 30°C, 6wt% phosphoric acid solution for reaction for 15 minutes, and the oxide film is expanded.

[0062] The remaining steps are the same as those in Example 1.

[0063] Comparative Example 3: A processing method for alloy composite parts based on nano injection molding: S3: Anodizing treatment: The aluminum alloy after surface pretreatment is used as the anode and the graphite plate as the cathode for the first anodizing in oxalic acid electrolyte. During the first anodizing process, the electrolyte is 0.3 mol / L oxalic acid solution, the oxidation voltage is 40 V, the oxidation temperature is 30°C, and the oxidation time is 4 hours; the anodized aluminum alloy is immersed in a mixed solution of 6wt% phosphoric acid and 1.8wt% chromic acid at 60°C, reacted for 1 minute, and the oxide film is removed; the aluminum alloy after the oxide film is removed is anodized for a second time, and the oxidation time is 6 hours; the aluminum alloy after the second anodizing is immersed in a 30°C, 6wt% phosphoric acid solution for reaction for 15 minutes, and the oxide film is expanded.

[0064] The remaining steps are the same as those in Example 1.

[0065] Comparative Example 4: A processing method for alloy composite parts based on nano injection molding: S3: Anodizing treatment: The aluminum alloy after surface pretreatment is used as the anode and the graphite plate as the cathode for the first anodizing in oxalic acid electrolyte. During the first anodizing process, the electrolyte is 0.3 mol / L oxalic acid solution, the oxidation voltage is 40 V, the oxidation temperature is 20°C, and the oxidation time is 4 hours; the anodized aluminum alloy is immersed in a mixed solution of 6wt% phosphoric acid and 1.8wt% chromic acid at 60°C, reacted for 1 minute, and the oxide film is removed; the aluminum alloy after the oxide film is removed is anodized for a second time, and the oxidation time is 6 hours; the aluminum alloy after the second anodizing is immersed in a 30°C, 6wt% phosphoric acid solution for reaction for 45 minutes, and the oxide film is expanded.

[0066] The remaining steps are the same as those in Example 1.

[0067] Comparative Example 5: A processing method for alloy composite parts based on nano injection molding: S1: Preparation of silicon carbide whiskers: Add carbon-silicon mixed powder, catalyst, aluminum powder, and anhydrous ethanol into a ball mill, stir evenly, add phenolic resin, stir for 12-14 hours, press into a blank, heat to 200-205°C and cure for 24 hours, heat the solidified blank to 1200-1400°C at a heating rate of 5°C / min under coke conditions and keep warm for 2-2.5 hours, cool, and grind to obtain silicon carbide whiskers;

[0068] S2: Surface pretreatment: Grind the aluminum alloy surface flat, immerse it in acetone and anhydrous ethanol for ultrasonic cleaning for 5 minutes, take it out, wash it with deionized water, and dry it; immerse the deoiled aluminum alloy in a mixed solution composed of 30g / L sodium hydroxide and 30g / L sodium carbonate, heat it to 55℃ for reaction for 40s, take it out, wash it with deionized water, and dry it; put the aluminum alloy with oxide film into a mixed solution composed of 400g / L sodium hydroxide, 300g / L sodium nitrate, 60g / L sodium fluoride, and 100g / L sodium silicate, heat it to 95℃ for reaction for 2 minutes, take it out, wash it with deionized water, and dry it;

[0069] S3: Anodizing treatment: The aluminum alloy after surface pretreatment is used as the anode and the graphite plate is used as the cathode for the first anodizing in oxalic acid electrolyte. During the first anodizing process, the electrolyte is 0.3 mol / L oxalic acid solution, the oxidation voltage is 40 V, the oxidation temperature is 20°C, and the oxidation time is 4 hours; the aluminum alloy anodized for the first time is immersed in a mixed solution composed of 6wt% phosphoric acid and 1.8wt% chromic acid at 60°C, reacted for 1 minute, and the oxide film is removed; the aluminum alloy after the oxide film is removed is anodized for the second time, and the oxidation time is 6 hours; the aluminum alloy after the second anodizing is immersed in a 30°C, 6wt% phosphoric acid solution for reaction for 15 minutes, and the oxide film is expanded;

[0070] S4: Nano-injection molding: The toughened polyphenylene sulfide resin is used as the matrix resin to perform nano-injection molding on the surface of the aluminum alloy to obtain an alloy composite; wherein the toughened polyphenylene sulfide resin is composed of 65 parts of polyphenylene sulfide, 30 parts of polybutylene terephthalate, 10 parts of silicon carbide whiskers, 5 parts of ethylene acrylic acid ethylene resin, 5 parts of ethylene acrylate and glycidyl methacrylate random copolymer, 0.2 parts of antioxidant 1098, and 0.8 parts of mold release agent SEED; the injection speed during the nano-injection molding process is 150 mm / s, the injection pressure is 60 MPa, the holding pressure is 40 MPa, and the holding time is 8 s.

[0071] Comparative Example 6: A processing method for an alloy composite part based on nano-injection molding: S5: Nano-injection molding: Use toughened polyphenylene sulfide resin as a matrix resin to perform nano-injection molding on the surface of an aluminum alloy after electrochemical deposition to obtain an alloy composite part; wherein the toughened polyphenylene sulfide resin is composed of 65 parts of polyphenylene sulfide, 30 parts of polybutylene terephthalate, 10 parts of silicon carbide whiskers, 5 parts of ethylene acrylic acid ethylene resin, 5 parts of a random copolymer of ethylene acrylate and glycidyl methacrylate, 0.2 parts of an antioxidant 1098, and 0.8 parts of a release agent SEED; during the nano-injection molding process, the injection speed is 300 mm / s, the injection pressure is 60 MPa, the holding pressure is 40 MPa, and the holding time is 8 s.

[0072] The remaining steps are the same as those in Example 1.

[0073] Comparative Example 7: A processing method for an alloy composite part based on nano-injection molding: S5: Nano-injection molding: Use toughened polyphenylene sulfide resin as a matrix resin to perform nano-injection molding on the surface of an aluminum alloy after electrochemical deposition to obtain an alloy composite part; wherein the toughened polyphenylene sulfide resin is composed of 65 parts of polyphenylene sulfide, 30 parts of polybutylene terephthalate, 10 parts of silicon carbide whiskers, 5 parts of ethylene acrylic acid ethylene resin, 5 parts of a random copolymer of ethylene acrylate and glycidyl methacrylate, 0.2 parts of an antioxidant 1098, and 0.8 parts of a release agent SEED; during the nano-injection molding process, the injection speed is 500 mm / s, the injection pressure is 60 MPa, the holding pressure is 40 MPa, and the holding time is 8 s.

[0074] The remaining steps are the same as those in Example 1.

[0075] Comparative Example 8: A processing method for an alloy composite part based on nano-injection molding: S5: Nano-injection molding: Use toughened polyphenylene sulfide resin as a matrix resin to perform nano-injection molding on the surface of an aluminum alloy after electrochemical deposition to obtain an alloy composite part; wherein the toughened polyphenylene sulfide resin is composed of 65 parts of polyphenylene sulfide, 30 parts of polybutylene terephthalate, 10 parts of glass fiber, 5 parts of ethylene acrylic acid ethylene resin, 5 parts of a random copolymer of ethylene acrylate and glycidyl methacrylate, 0.2 parts of an antioxidant 1098, and 0.8 parts of a release agent SEED; during the nano-injection molding process, the injection speed is 300 mm / s, the injection pressure is 60 MPa, the holding pressure is 40 MPa, and the holding time is 8 s.

[0076] The remaining steps are the same as those in Example 1.

[0077] Experiment: Plastic-metal bonding performance test:

[0078] The plastic-metal test piece was prepared according to the patented method of Japan Dacheng Nano Injection Molding. The size of the aluminum alloy sheet is 20mm×45mm×1.5mm, the size of the plastic piece is 10mm×45mm×3mm, and the area of ​​plastic-metal bonding is 0.5cm 2 .

[0079] According to the standards in Japanese Taisei Chemical Patent 8057890, the plastic-metal test piece is tested for its plastic-metal bonding performance.

[0080] Table 1 Plastic-metal bonding performance test data table

[0081]

[0082] Conclusion: The alloy composite prepared by the present invention has excellent interface bonding strength.

[0083] In Comparative Example 1, the oxalic acid concentration during the anodization process was too high, resulting in excessively large nanopore diameters and pore collapse, which reduced the interfacial bonding strength.

[0084] In Comparative Example 2, the oxidation voltage during the anodization process was too high, resulting in an unstable growth process of the nanopore structure, irregular nanopore shapes, and different nanopore sizes, which led to a decrease in the interface bonding force.

[0085] In Comparative Example 3, the oxidation temperature during the anodization process was too high, resulting in severe corrosion of the electrolyte, the nanopore structure was connected together, the porous structure was destroyed, and the interface bonding force was reduced.

[0086] In Comparative Example 4, the hole expansion time during the oxide film expansion process was too long, resulting in severe corrosion of the oxide film, and the holes were connected and collapsed, resulting in reduced interface bonding strength.

[0087] In Comparative Example 5, electrochemical deposition was not performed after anodization, and the anchoring effect formed by the reaction between the aluminum alloy-triazine dithiol metal salt-toughened polyphenylene sulfide resin was lacking, resulting in reduced interface bonding strength.

[0088] In Comparative Example 6, the injection speed during the nano-injection molding process is too slow, and the filling process is restricted by the metal pore wall, which is prone to distortion, resulting in a reduction in the pore size, and the molecular chains accumulate and clog at the entrance of the nanopores, resulting in reduced interfacial bonding strength.

[0089] In Comparative Example 7, the injection speed during the nano-injection molding process was too fast, and the bonding strength of the resin in the nano-pores was reduced, resulting in reduced interface bonding strength.

[0090] In Comparative Example 8, the silicon carbide whiskers in the toughened polyphenylene sulfide resin were replaced with glass fibers. The glass fibers were too large to enter the nanopores and were only in the resin outside the nanopores, resulting in a difference in thermal expansion coefficients inside and outside the nanopores, and the failure of the nano-anchor effect, leading to reduced interfacial bonding strength.

[0091] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for processing alloy composite parts based on nano injection molding, characterized in that: The following steps are involved: S1: Surface pretreatment: Degreasing, removing oxide film and chemical polishing the aluminum alloy surface in sequence; S2: Anodizing treatment: The aluminum alloy after surface pretreatment is subjected to first anodizing, oxide film removal, second anodizing, and oxide film pore expansion in sequence; S3: Electrochemical deposition: The aluminum alloy after anodizing is subjected to double potential electrodeposition; S4: Nano-injection molding: The toughened polyphenylene sulfide resin is used as a matrix resin to perform nano-injection molding on the surface of the aluminum alloy after electrochemical deposition to obtain an alloy composite part.

2. The method for processing alloy composite parts based on nano injection molding according to claim 1, characterized in that: In step S1, the degreasing step includes grinding the surface of the aluminum alloy flat, immersing it in acetone and anhydrous ethanol for ultrasonic cleaning for 5-10 minutes, taking it out, washing it with deionized water, and drying it; the oxide film removal step includes immersing the degreased aluminum alloy in a mixed solution composed of 30-35g / L sodium hydroxide and 30-35g / L sodium carbonate, heating it to 55-60°C for reaction for 40-45s, taking it out, washing it with deionized water, and drying it; the chemical polishing step includes placing the aluminum alloy after the oxide film is removed into a mixed solution composed of 400-420g / L sodium hydroxide, 300-320g / L sodium nitrate, 60-65g / L sodium fluoride, and 100-120g / L sodium silicate, heating it to 95-100°C for reaction for 1-5 minutes, taking it out, washing it with deionized water, and drying it.

3. The method for processing alloy composite parts based on nano injection molding according to claim 1, characterized in that: In step S2, the electrolyte in the first anodization is a 0.3-0.6 mol / L oxalic acid solution, the oxidation voltage is 35-45 V, the oxidation temperature is 15-25° C., and the oxidation time is 4-4.5 h; the oxide film removal step comprises immersing the first anodized aluminum alloy in a mixed solution of 6-7 wt% phosphoric acid and 1.8-2 wt% chromic acid at 60-65° C., and reacting for 1-2 min; the oxidation time in the second anodization is 6-6.5 h, and the other anodization process parameters are the same as those of the first anodization; the oxide film pore expansion step comprises immersing the aluminum alloy after the second anodization in a 6-7 wt% phosphoric acid solution at 30-35° C. and reacting for 15-30 min.

4. The method for processing alloy composite parts based on nano injection molding according to claim 1, characterized in that: In the dual potential electrodeposition, the aluminum alloy after anodization is used as the working electrode, the saturated calomel electrode is used as the reference electrode, and the stainless steel sheet is used as the auxiliary electrode; The electrolyte consists of 5-6 mmol / L triazine dithiol and 0.15-0.18 mol / L sodium nitrate solution.

5. The method for processing alloy composite parts based on nano injection molding according to claim 1, characterized in that: In step S4, the nano injection molding step includes injection pressurization, pressure holding, cooling, and ejection; the injection speed is 250-350 mm / s, the injection pressurization pressure is 60-80 MPa, the pressure holding pressure is 40-60 MPa, and the pressure holding time is 8-10 s.

6. The method for processing alloy composite parts based on nano injection molding according to claim 1, characterized in that: The components of the toughened polyphenylene sulfide resin include polyphenylene sulfide, polybutylene terephthalate, silicon carbide whisker, ethylene acrylic acid ethylene resin, glycidyl ester-containing random copolymer, antioxidant and release agent.

7. The method for processing alloy composite parts based on nano injection molding according to claim 1, characterized in that: The components in the toughened polyphenylene sulfide resin are calculated by weight: 50-65 parts of polyphenylene sulfide, 15-30 parts of polybutylene terephthalate, 10-30 parts of silicon carbide whiskers, 1-10 parts of ethylene acrylic acid resin, 1-10 parts of glycidyl ester random copolymer, 0.1-1 parts of antioxidant, and 0.1-2 parts of release agent.

8. The method for processing alloy composite parts based on nano injection molding according to claim 6, characterized in that: The method for preparing the silicon carbide whisker comprises the following steps: Add carbon silicon mixed powder, catalyst, aluminum powder and anhydrous ethanol into a ball mill, stir evenly, add phenolic resin, stir for 12-14 hours, press into billets, heat to 200-205°C and cure for 24 hours, heat the cured billet to 1200-1400°C at a heating rate of 5°C / min under coke conditions and keep warm for 2-2.5 hours, cool and grind to obtain silicon carbide whiskers.

9. The method for processing alloy composite parts based on nano injection molding according to claim 8, characterized in that: The carbon-silicon molar ratio in the carbon-silicon mixed powder is 1:1, and the catalyst includes any one of cobalt trioxide, chromium trioxide, and aluminum fluoride trihydrate; the catalyst addition amount is 2-4wt% of the mass of the carbon-silicon mixed powder, the aluminum powder addition amount is 1-1.5wt% of the total mass of the silicon carbide mixed powder and the catalyst, and the phenolic resin addition amount is 5-6wt% of the total mass of the carbon-silicon mixed powder, the catalyst, and the aluminum powder.

10. An alloy composite part prepared according to the processing method of an alloy composite part based on nano injection molding according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Resin-metal bonded body and method for producing the same

    CN101896645A

  • Polyphenylene sulfide resin composition, and moulding and manufacturing process for moulding thereof

    CN105377991A

  • Apparatus and method of forming a compound structure

    CN106102364A

  • Metal-plastic composite, preparation method and preparation device

    CN112318814A

  • Preparation method of metal-plastic mixed structural part based on secondary anodic oxidation method

    CN112721352A

Cited By

  • High-binding-force injection molding alloy part and preparation method thereof

    CN121227032A