Preparation method of uniform bicrystal phase tricalcium phosphate powder
By grinding and calcining calcium carbonate and calcium hydrogen phosphate with grinding microspheres in double-crystalline calcium phosphate bone cement, the problem of uneven crystal distribution is solved, the uniformity and compressive strength of bone cement is improved, and new Bone growth.
Patent Information
- Application Number
- CN202311064033.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-23
- Publication Date
- 2024-11-01
AI Technical Summary
In the prior art, the crystal distribution of α-tricalcium phosphate and β-tricalcium phosphate in the dual-crystalline calcium phosphate bone cement is uneven, which affects the curing performance and bone regeneration process.
By mixing calcium carbonate and calcium biphosphate in a specific molar ratio and ball milling and calcining with grinding microspheres, a uniform bi-crystalline tricalcium phosphate powder is formed, and the crystal phase scale and distribution are controlled using the sintering process and delayed cooling characteristics.
The uniformity and in-situ composite properties of the double-crystal phase tricalcium phosphate powder are achieved, the compressive strength of bone cement is improved, the porosity and pore size of the bone growth is promoted, and the preparation process is simplified.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of bone repair materials, and in particular to a method for preparing uniform twin-phase tricalcium phosphate powder. Background Art
[0002] In the past few decades, autologous bone has been considered the gold standard for bone transplantation. However, the limited supply of autologous bone has restricted its clinical application. Calcium phosphate-based materials are widely used in bone transplantation due to their good biocompatibility and osteoconductivity.
[0003] Calcium phosphate materials come in different forms, such as prefabricated particles or blocks, which are difficult to handle from a clinical perspective. Self-curing calcium phosphate bone cement can be used as a scaffold material for bone tissue engineering because it has osteoconductivity and completely matches the surrounding tissue when injected in situ. Self-curing calcium phosphate artificial bone is composed of two parts: calcium phosphate powder and curing liquid. When used, the two are mixed in a certain proportion to form a paste, which is filled in the bone defect and can be trimmed at will according to the anatomical requirements of the bone defect to achieve accurate repair of the bone defect.
[0004] There are many kinds of compositions for preparing self-setting calcium phosphate cement (CPC), which can be divided into α-tricalcium phosphate (α-TCP) single-solid-phase CPC, TTCP (tetracalcium phosphate) multi-solid-phase CPC, and α-TCP multi-solid-phase CPC according to the solid phase components. The final solidified product is calcium-deficient hydroxyapatite (CDHA) or hydroxyapatite (HA).
[0005] However, the main disadvantage of hydroxyapatite and its derivatives is that they degrade slowly, which does not match the rate of new bone formation in the human body, which hinders bone regeneration. A new method is to introduce β-tricalcium phosphate, which has a higher degradation rate, into α-tricalcium phosphate to form a twin-phase calcium phosphate system. Currently, α-tricalcium phosphate powder and β-tricalcium phosphate powder are directly mixed to obtain a twin-phase calcium phosphate system, but this physical blending method is difficult to make the raw materials compounded uniformly, which affects the curing properties of the twin-phase calcium phosphate. Summary of the invention
[0006] In order to overcome the deficiencies of the prior art, the object of the present invention is to provide a method for preparing a uniform dual-phase tricalcium phosphate powder to solve the problem of uneven distribution of α-tricalcium phosphate and β-tricalcium phosphate crystals in dual-phase tricalcium phosphate bone cement.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows: A method for preparing uniform twin-phase tricalcium phosphate powder comprises the following steps: 1) Calcium carbonate and calcium hydrogen phosphate are mixed uniformly at a molar ratio of 1:(1.95-2.05), and ball-milled to obtain a mixture A; 2) Mixing mixture A and ground microspheres at a mass ratio of 1:(0.3-0.8) to obtain mixture B; 3) The mixture B is placed in a muffle furnace for calcination, grinding, and sieving to obtain twin-phase tricalcium phosphate powder.
[0008] Furthermore, before the ball milling in step 1), an anhydrous volatile solvent is added for mixing.
[0009] Furthermore, in the step 1), the mass ratio of the calcium carbonate and calcium hydrogen phosphate to the anhydrous volatile solvent is 1:1-3.
[0010] Preferably, in step 1), the mass ratio of the mixture to the anhydrous volatile solvent is 1:2.
[0011] Preferably, in step 1), the anhydrous volatile solvent is ethanol.
[0012] Furthermore, in the step 1), the ball milling is carried out in a ball mill at a ball milling speed of 200 rpm-500 rpm and a ball milling time of 4-6 h.
[0013] Preferably, in the step 1), the ball milling is carried out in a ball mill at a ball milling speed of 400 rpm and a ball milling time of 5 h.
[0014] Furthermore, in the step 2), the grinding microspheres are selected from one or more of aluminum oxide microspheres, zirconium oxide microspheres, silicon carbide microspheres, and silicon nitride microspheres.
[0015] Preferably, in step 2), the grinding microspheres are zirconium oxide microspheres.
[0016] Furthermore, in the step 2), the particle size of the grinding microspheres is 10-20 μm.
[0017] Preferably, in the step 2), the particle size of the grinding microspheres is 15 μm.
[0018] Furthermore, in the step 2), the mixture A is mixed with the grinding microspheres and then ground for 2-4 hours.
[0019] Preferably, in the step 2), the mixture A is mixed with the grinding microspheres and then ground for 3 hours.
[0020] Furthermore, in the step 2), the mixture A and the grinding microspheres are mixed at a mass ratio of 1:0.6.
[0021] Furthermore, the grinding in step 3) is to place the powder in a planetary ball mill at a grinding speed of 200 rpm-500 rpm and a grinding time of 4-6 hours.
[0022] Preferably, the grinding in step 3) is to place the powder in a planetary ball mill and mill it at a speed of 400 rpm for 5 hours.
[0023] Furthermore, the aperture of the sieve used for screening in step 3) is smaller than the particle size of the ground microspheres.
[0024] Preferably, the mesh size of the sieve in step 3) is 2000 mesh.
[0025] Furthermore, in the step 3), the calcination temperature in the muffle furnace is 1300-1400° C. and the calcination time is 0.5-1 h.
[0026] Preferably, in step 3), the mixture B is placed in a muffle furnace at 1350° C. and calcined for 45 minutes.
[0027] Beneficial effects of the present invention: The present invention provides a method for preparing a uniform twin-phase tricalcium phosphate powder, which uses a sintering process to prepare a uniformly synthesized twin-phase calcium phosphate at a crystal phase scale. The method for preparing a uniform twin-phase tricalcium phosphate powder of the present invention fully utilizes the delayed cooling characteristics of the grinding microspheres and the adjustable heat transfer medium distribution, reduces the conversion of β-tricalcium phosphate to α-tricalcium phosphate, maintains the uniformity and in-situ composite characteristics of α-TCP and β-TCP twin-phase tricalcium phosphate powders, and has a simple preparation process; in addition, the grinding microspheres can be reused. Implementation
[0028] To better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be understood by those skilled in the art that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0029] In the examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified. Example
[0030] (1) Calcium carbonate (CaCO 3 ) and calcium hydrogen phosphate (CaHPO 4 •2H 2 O) are mixed in a molar ratio of 1:2, anhydrous ethanol is added in a ratio of the total mass of calcium carbonate and calcium hydrogen phosphate to anhydrous ethanol of 1:2, and ball milled in a ball mill at a speed of 400 rpm for 5 h to obtain a mixture A; (2) Mixture A and zirconium oxide microspheres were mixed in a mass ratio of 1:0.6, the average particle size of the zirconium oxide microspheres was 15 μm, and ground for 3 h to obtain mixture B; (3) The mixture B is calcined in a muffle furnace at 1350° C. for 45 min, cooled in the furnace, and then ball-milled in a planetary ball mill at 400 rpm for 5 h. The powder is sieved through a 2000 mesh sieve, and the sieved powder is collected to obtain the uniform twin-phase tricalcium phosphate powder. Example
[0031] (1) Calcium carbonate (CaCO 3 ) and calcium hydrogen phosphate (CaHPO 4 •2H 2 O) were mixed uniformly in a molar ratio of 1:2.05, anhydrous ethanol was added in a ratio of the total mass of calcium carbonate and calcium hydrogen phosphate to anhydrous ethanol of 1:3, and ball milled in a ball mill at a speed of 500 rpm for 6 h to obtain a mixture A; (2) Mixture A and zirconium oxide microspheres were mixed in a mass ratio of 1:0.8, the average particle size of the zirconium oxide microspheres was 20 μm, and the mixture was ground for 4 h to obtain mixture B; (3) The mixture B is calcined in a muffle furnace at 1350° C. for 1 hour, cooled in the furnace, and then ball-milled in a planetary ball mill at a speed of 500 rpm for 6 hours. The powder is sieved through a 2000 mesh sieve, and the sieved powder is collected to obtain the uniform twin-phase tricalcium phosphate powder. Example
[0032] (1) Calcium carbonate (CaCO 3 ) and calcium hydrogen phosphate (CaHPO 4 •2H 2 O) were mixed uniformly in a molar ratio of 1:1.95, anhydrous ethanol was added in a ratio of the total mass of calcium carbonate and calcium hydrogen phosphate to anhydrous ethanol of 1:1, and ball milled in a ball mill at a speed of 200 rpm for 4 h to obtain a mixture A; (2) Mixture A and zirconium oxide microspheres were mixed in a mass ratio of 1:0.3, the average particle size of the zirconium oxide microspheres was 10 μm, and ground for 3 h to obtain mixture B; (3) The mixture B is calcined in a muffle furnace at 1350° C. for 30 min, cooled in the furnace, and then ball-milled in a planetary ball mill at a speed of 200 rpm for 4 h. The powder is sieved through a 2000 mesh sieve, and the sieved powder is collected to obtain the uniform twin-phase tricalcium phosphate powder. Example
[0033] (1) Calcium carbonate (CaCO 3 ) and calcium hydrogen phosphate (CaHPO 4 •2H 2 O) mixing them uniformly in a molar ratio of 1:2, adding anhydrous ethanol in a ratio of the total mass of calcium carbonate and calcium hydrogen phosphate to anhydrous ethanol of 1:2, and ball milling them in a ball mill at a speed of 400 rpm for 4 hours to obtain a mixture A; (2) Mixture A and zirconium oxide microspheres were mixed in a mass ratio of 1:0.6, the average particle size of the zirconium oxide microspheres was 15 μm, and ground for 3 h to obtain mixture B; (3) The mixture B is calcined in a muffle furnace at 1350° C. for 45 min, cooled in the furnace, and then ball-milled in a planetary ball mill at 400 rpm for 5 h. The powder is sieved through a 2000 mesh sieve, and the sieved powder is collected to obtain the uniform twin-phase tricalcium phosphate powder. Example
[0034] (1) Calcium carbonate (CaCO 3 ) and calcium hydrogen phosphate (CaHPO 4 •2H 2 O) mixing them uniformly in a molar ratio of 1:2, adding anhydrous ethanol in a ratio of the total mass of calcium carbonate and calcium hydrogen phosphate to anhydrous ethanol of 1:2, and ball milling them in a ball mill at a speed of 400 rpm for 4 hours to obtain a mixture A; (2) Mixture A and zirconium oxide microspheres were mixed in a mass ratio of 1:0.6, the average particle size of the zirconium oxide microspheres was 15 μm, and ground for 3 h to obtain mixture B; (3) The mixture B is calcined in a muffle furnace at 1350° C. for 45 min, cooled in the furnace, and then ball-milled in a planetary ball mill at 400 rpm for 5 h. The powder is sieved through a 2000 mesh sieve, and the sieved powder is collected to obtain the uniform twin-phase tricalcium phosphate powder. Example
[0035] (1) Calcium carbonate (CaCO 3 ) and calcium hydrogen phosphate (CaHPO 4 •2H 2 O) mixing them uniformly in a molar ratio of 1:2, adding anhydrous ethanol in a ratio of the total mass of calcium carbonate and calcium hydrogen phosphate to anhydrous ethanol of 1:2, and ball milling them in a ball mill at a speed of 400 rpm for 5 hours to obtain a mixture A; (2) Mixture A and aluminum oxide microspheres were mixed at a mass ratio of 1:0.6, the average particle size of the aluminum oxide microspheres was 15 μm, and ground for 3 h to obtain mixture B; (3) The mixture B is calcined in a muffle furnace at 1350° C. for 45 min, cooled in the furnace, and then ball-milled in a planetary ball mill at 400 rpm for 5 h. The powder is sieved through a 2000 mesh sieve, and the sieved powder is collected to obtain the uniform twin-phase tricalcium phosphate powder.
[0036] Comparative Example 1 α-tricalcium phosphate powder (purity>99%) and β-tricalcium phosphate powder (purity>99%) were placed in a planetary ball mill at a mass ratio of 761:239 and ball-milled at 400 rpm for 5 hours. The powder was sieved through a 2000 mesh sieve and the sieved powder was collected to obtain a twin-phase tricalcium phosphate powder.
[0037] Comparative Example 2 (1) Calcium carbonate (CaCO 3 ) and calcium hydrogen phosphate (CaHPO 4 •2H 2 O) mixing them uniformly in a molar ratio of 1:2, adding anhydrous ethanol in a ratio of the total mass of calcium carbonate and calcium hydrogen phosphate to anhydrous ethanol of 1:2, and ball milling them in a ball mill at a speed of 400 rpm for 5 hours to obtain a mixture A; (2) Mixture A and zirconium oxide microspheres were mixed in a mass ratio of 1:1, the average particle size of the zirconium oxide microspheres was 15 μm, and ground for 3 h to obtain mixture B; (3) The mixture B was calcined in a muffle furnace at 1350°C for 45 min, cooled in the furnace, and then ball-milled in a planetary ball mill at 400 rpm for 5 h. The powder was sieved through a 2000 mesh sieve and the sieved powder was collected to obtain a twin-phase tricalcium phosphate powder.
[0038] Comparative Example 3 (1) Calcium carbonate (CaCO 3 ) and calcium hydrogen phosphate (CaHPO 4 •2H 2 O) mixing them uniformly in a molar ratio of 1:2, adding anhydrous ethanol in a ratio of the total mass of calcium carbonate and calcium hydrogen phosphate to anhydrous ethanol of 1:2, and ball milling them in a ball mill at a speed of 400 rpm for 5 hours to obtain a mixture A; (2) Mixture A and zirconium oxide microspheres were mixed in a mass ratio of 1:0.2, the average particle size of the zirconium oxide microspheres was 15 μm, and ground for 3 h to obtain mixture B; (3) The mixture B was calcined in a muffle furnace at 1350°C for 45 min, cooled in the furnace, and then ball-milled in a planetary ball mill at 400 rpm for 5 h. The powder was sieved through a 2000 mesh sieve and the sieved powder was collected to obtain a twin-phase tricalcium phosphate powder.
[0039] Comparative Example 4 (1) Calcium carbonate (CaCO 3 ) and calcium hydrogen phosphate (CaHPO 4 •2H 2 O) mixing them uniformly in a molar ratio of 1:2, adding anhydrous ethanol in a ratio of the total mass of calcium carbonate and calcium hydrogen phosphate to anhydrous ethanol of 1:2, and ball milling them in a ball mill at a speed of 400 rpm for 5 hours to obtain a mixture A; (2) Mixture A was calcined in a muffle furnace at 1350° C. for 45 min, cooled in the furnace, and then ball-milled in a planetary ball mill at 400 rpm for 5 h. The powder was sieved through a 2000 mesh sieve and the sieved powder was collected to obtain a twin-phase tricalcium phosphate powder.
[0040] Comparative Example 5 (1) Calcium carbonate (CaCO 3 ) and calcium hydrogen phosphate (CaHPO 4 •2H 2 O) mixing them uniformly in a molar ratio of 1:2, adding anhydrous ethanol in a ratio of the total mass of calcium carbonate and calcium hydrogen phosphate to anhydrous ethanol of 1:2, and ball milling them in a ball mill at a speed of 400 rpm for 5 hours to obtain a mixture A; (2) Mixture A and zirconium oxide microspheres were mixed in a mass ratio of 1:0.6, and the average particle size of aluminum oxide microspheres was 500 μm, and the mixture was ground for 3 h to obtain mixture B; (3) The mixture B was calcined in a muffle furnace at 1350°C for 45 min, cooled in the furnace, and then ball-milled in a planetary ball mill at 400 rpm for 5 h. The powder was sieved through a 2000 mesh sieve and the sieved powder was collected to obtain a twin-phase tricalcium phosphate powder.
[0041] Experimental example: 1. Phase analysis: The tricalcium phosphate powders prepared in Examples 1-5 and Comparative Examples 2-4 were analyzed by X-ray diffractometer, and the phase compositions of α-tricalcium phosphate and β-tricalcium phosphate in the products were calculated using easy quantitative analysis in JADE6.5. The results are shown in Table 1.
[0042] Table 1: Phase composition data of tricalcium phosphate Group Microsphere Type Mass ratio of mixture A to microspheres Calcination time (min) α-tricalcium phosphate (%) β-tricalcium phosphate (%) Example 1 Zirconia 1:0.6 45 76.1 23.9 Example 2 Zirconia 1:0.8 60 85.9 14.1 Example 3 Zirconia 1:0.3 30 63.8 36.2 Example 4 Zirconia 1:0.6 30 67.2 32.8 Example 5 Zirconia 1:0.6 60 82.4 17.6 Example 6 Aluminum oxide 1:0.6 45 74.2 25.8 Comparative Example 2 Zirconia 1:1 45 78.3 21.7 Comparative Example 3 Zirconia 1:0.2 45 73.3 26.7 Comparative Example 4 Zirconia / 45 71.6 28.4 Comparative Example 5 Zirconia 1:0.6 45 70.2 29.8 It can be seen from Table 1 that the mass ratio of mixture A to ground microspheres affects the composition of α-tricalcium phosphate and β-tricalcium phosphate of the calcined products. This is mainly due to the delayed cooling characteristics of the ground microspheres and the adjustable distribution of the heat transfer medium, which can control the crystal phase transformation of α-tricalcium phosphate and β-tricalcium phosphate during the calcination process.
[0043] 2. Aperture The tricalcium phosphate powders prepared in Examples 1-5 and Comparative Examples 1-4 were mixed with water at a solid-liquid ratio of 2:1 to form a cylinder about 3.0 mm high. The cylinder was dried, and gold was sprayed on the surface of the cylinder using a vacuum coating apparatus and then evacuated. The microstructure of the surface of the cylinder was observed using a scanning electron microscope, the pore size was measured, and the average value was calculated to obtain the average pore size. The results are shown in Table 2.
[0044] 3. Porosity Porosity detection method: The tricalcium phosphate powders prepared in Examples 1-5 and Comparative Examples 1-4 were mixed with water at a solid-liquid ratio of 2:1 to form a cylinder about 3.0 mm high. Anhydrous ethanol was used as the liquid medium. The porosity of the sample was determined by a specific gravity balance according to the Archimedes drainage method. The results are shown in Table 2.
[0045] 4. Determination of compressive strength The solid phase powder of tricalcium phosphate prepared in Examples 1-5 and Comparative Examples 1-4 and the solidifying liquid citric acid solution were mixed in proportion, blended with a medicine spoon for 30 seconds to form a uniform bone cement slurry, filled into a stainless steel cylindrical mold with a diameter of 6 mm and a height of 12 mm and compacted under a pressure of 0.7 MPa. The prepared cylindrical sample was inserted into a glass tube with a diameter of 6.5 mm and a height of 13 mm, and then placed in an environment with a temperature of 37° C. and a relative humidity of 100% for curing for 3 days. The compressive strength of the sample was tested by a universal material testing machine at a loading rate of 1 mm / min, and the average value was calculated. The results are shown in Table 2.
[0046] Table 2 Test results Group Pore size (μm) Porosity (%) Compressive strength (MPa) Example 1 326.2±12.2 62.1 24.3±0.3 Example 2 275.1±21.6 57.8 22.9±0.9 Example 3 224.9±14.4 52.6 23.1±0.4 Example 4 379.4±13.9 57.3 21.2±1.1 Example 5 201.3±14.6 56.2 20.5±1.3 Example 6 301.58±26.92 61.4 23.5±2.5 Comparative Example 1 124.6±11.4 41.6 14.9±0.9 Comparative Example 2 116.2±11.7 48.7 16.7±1.2 Comparative Example 3 124.9±12.5 47.6 17.8±0.7 Comparative Example 4 68.9±2.3 44.9 15.6±1.3 Comparative Example 5 69.2±2.9 47.2 16.4±1.8 It can be seen from Table 2 that the bicrystalline tricalcium phosphate bone cement prepared by the preparation method of the present invention can obtain a porosity and pore size suitable for the crawling of osteoblasts, which is beneficial to the growth of new bones.
[0047] The present invention adopts a high temperature curing reaction to prepare a bicrystalline phase tricalcium phosphate powder, and controls the mass ratio of the starting material to alumina and the calcining temperature to control the distribution and ratio of α-tricalcium phosphate and β-tricalcium phosphate in the bicrystalline phase powder. In the bicrystalline phase tricalcium phosphate powder, α-tricalcium phosphate can be hydrated when it meets water to generate calcium-deficient hydroxyapatite, and the degradation rate of β-tricalcium phosphate is faster than that of calcium-deficient hydroxyapatite. The degradation of β-tricalcium phosphate can further form a through aperture to promote the growth of osteoblasts. The uniformly distributed bicrystalline phase tricalcium phosphate powder formed by calcination can improve the compressive strength of bone cement.
[0048] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing uniform twin-phase tricalcium phosphate powder, characterized in that: The following steps are involved: 1) Calcium carbonate and calcium hydrogen phosphate are mixed in a molar ratio of 1:(1.95-2.05), and ball-milled to obtain a mixture A; 2) Mixing mixture A and grinding microspheres at a mass ratio of 1:(0.3-0.8), and grinding to obtain mixture B; 3) The mixture B is placed in a muffle furnace for calcination, grinding, and sieving to obtain the uniform twin-phase tricalcium phosphate powder.
2. The method for preparing a uniform twin-phase tricalcium phosphate powder according to claim 1, characterized in that: In the step 1), before the ball milling, an anhydrous volatile solvent is added for mixing.
3. The method for preparing a uniform twin-phase tricalcium phosphate powder according to claim 1, characterized in that: In the step 1), the ball milling is carried out in a ball mill at a speed of 200 rpm-500 rpm and a ball milling time of 4-6 hours.
4. The method for preparing a uniform twin-phase tricalcium phosphate powder according to claim 2, characterized in that: In the step 1), the mass ratio of the total mass of the calcium carbonate and calcium hydrogen phosphate to the mass ratio of the anhydrous volatile solvent is 1:1-3.
5. The method for preparing a uniform twin-phase tricalcium phosphate powder as claimed in claim 2, characterized in that: In the step 1), the anhydrous volatile solvent is ethanol.
6. The method for preparing a uniform twin-phase tricalcium phosphate powder according to claim 1, characterized in that: In the step 2), the grinding microspheres are selected from one or more of aluminum oxide microspheres, zirconium oxide microspheres, silicon carbide microspheres, and silicon nitride microspheres.
7. The method for preparing a uniform twin-phase tricalcium phosphate powder according to claim 1, characterized in that: In the step 2), the particle size of the grinding microspheres is 10-20 μm; and the grinding time is 2-4 hours.
8. The method for preparing a uniform twin-phase tricalcium phosphate powder according to claim 1, characterized in that: In the step 3), the grinding is performed using a planetary ball mill. The mixture B is placed in the planetary ball mill at a grinding speed of 200 rpm-500 rpm and a grinding time of 4-6 hours.
9. The method for preparing a uniform twin-phase tricalcium phosphate powder according to claim 1, characterized in that: In the step 3), the aperture of the sieve used for sieving is smaller than the particle size of the ground microspheres.
10. The method for preparing a uniform twin-phase tricalcium phosphate powder according to claim 1, characterized in that: In the step 3), the calcination temperature in the muffle furnace is 1300-1400° C. and the calcination time is 0.5-1 h.
Citation Information
Patent Citations
PROCESS FOR OBTAINING TWO-PHASE BIOCERAMICS BASED ON CALCIUM PHOSPHATE FROM MARBLE WASTE
BR102019001412A2
Biphase calcium phosphate (BCP) composite powder synthesized by high-temperature solid phase reaction and preparation method thereof
CN107176832A
Biphase tricalcium phosphate white phosphor as well as in-situ synthesis method and application thereof
CN109054836A
Alpha-tricalcium phosphate and preparation method thereof
CN110562945A
Hydraulic cement based on calcium phosphate for surgical use
US20070186818A1
Cited By
Silicon-regulated in-situ biphase TCP high-strength porous artificial bone filling material and application thereof
CN122516436A