Hard carbon material containing closed-pore structure, preparation method and application

By subjecting biomass raw materials to oxidation, acid washing, and carbonization, hard carbon materials with closed-pore structures are prepared, solving the problem of low initial coulombic efficiency of hard carbon materials and improving the electrochemical performance and cost-effectiveness of sodium-ion batteries.

CN118877871AActive Publication Date: 2024-11-01碳一(安徽)钠电材料有限公司 +1

Patent Information

Application Number
CN202410959822.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-01
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

In the existing technology, the low initial coulombic efficiency of hard carbon materials limits their application in sodium-ion batteries.

Method used

Hard carbon materials with closed-pore structures are prepared by treating biomass raw materials through gas-phase and liquid-phase oxidation, combined with acid washing and pre-carbonization carbonization steps. The pore size and pore volume are controlled, and phosphorus, nitrogen or sulfur elements are doped to optimize the graphite microcrystalline structure.

Benefits of technology

It improves the initial coulombic efficiency and electrochemical performance of hard carbon materials, enhances the battery performance of sodium-ion batteries, reduces manufacturing costs, and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118877871A_ABST
    Figure CN118877871A_ABST
Patent Text Reader

Abstract

The invention discloses a hard carbon material containing a closed pore structure, a preparation method and application, the average pore size of the hard carbon material is measured to be 5-6 nm through a gas adsorption method, and the total pore volume of closed pores is 0.12 cm < 3 > / g-0. 30 cm < 3 > / g; through XRD (X-Ray Diffraction) characterization, the crystallite size of the hard carbon material is calculated to be 4.0-5.0 nm in a crystal basal plane direction La, and is 1.00-1.30 nm in a direction vertical to the basal plane direction Lc. In the invention, the hard carbon material with large aperture and large closed pore volume can provide more active sodium storage sites, the initial coulombic efficiency of the hard carbon material is improved, the graphite microcrystalline structure in the hard carbon material is narrower and longer, and the realization of large aperture and large closed pore volume of the hard carbon material is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of secondary battery negative electrode materials, and in particular to a hard carbon material containing a closed-pore structure, a preparation method and an application thereof. Background Art

[0002] With the development of the new energy industry, lithium-ion batteries have been widely used in industries such as electric vehicles, but their further development is restricted by a series of key issues such as lithium resource reserves and lithium-ion battery costs. Sodium-ion batteries have the advantages of low cost, abundant sodium reserves and wide distribution, and are expected to be a substitute for lithium-ion batteries.

[0003] As the negative electrode material of sodium ion batteries, hard carbon has a disordered amorphous structure that allows more defects and micropores in hard carbon materials to provide more active sodium storage sites, which is beneficial to improving the electrical performance of sodium ion batteries. The existing technology uses biomass as a raw material to prepare hard carbon materials. Plant biomass is rich in a large amount of cellulose, hemicellulose, lignin and other substances, and is the most abundant renewable resource on the earth. However, the electrochemical performance of hard carbon prepared by direct carbonization of plant biomass is not ideal. One of the main reasons is that the inherent low initial Coulomb efficiency of hard carbon materials restricts their application range. How to improve the initial Coulomb efficiency of hard carbon materials has become an urgent problem to be solved.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The purpose of the present invention is to provide a hard carbon material containing a closed-pore structure, a preparation method and an application thereof, thereby improving the problem of low initial Coulomb efficiency of the hard carbon material.

[0006] The present invention is achieved in that:

[0007] In a first aspect, the present invention provides a hard carbon material, wherein the average pore size of the hard carbon material is 5nm-6nm and the total pore volume of the closed pores is 0.12cm 3 / g-0.30cm 3 / g;

[0008] Through XRD characterization, it is calculated that the crystallite size of the hard carbon material is 4.0nm-5.0nm in the crystal basal plane direction La and 1.00nm-1.30nm in the direction perpendicular to the basal plane Lc.

[0009] In an optional embodiment, the hard carbon material satisfies at least one of the following (1)-(7):

[0010] (1) The hard carbon crystal interlayer spacing d(002) in the hard carbon material is 0.390 nm to 0.400 nm;

[0011] (2) The specific surface area of ​​the hard carbon material is 4 cm 2 / g-8cm 2 / g;

[0012] (3) I of the hard carbon material D / I G 1.7-1.8;

[0013] (4) The hard carbon material is doped with at least one of phosphorus, nitrogen or sulfur, and the content of the doped element is ≥ 3wt%, preferably 4wt%-10wt%;

[0014] (5) The hard carbon material comprises biomass-based hard carbon;

[0015] (6) The reversible discharge specific capacity of the hard carbon material is greater than 340 mAh / g;

[0016] (7) The initial efficiency of the hard carbon material is greater than 87%.

[0017] In a second aspect, the present invention provides a method for preparing the hard carbon material according to the aforementioned embodiment, comprising the following steps:

[0018] performing oxidation treatment on the biomass raw material to obtain an oxidation product;

[0019] washing the oxidation product with an acid solution to obtain a purified product;

[0020] The purified product is sequentially pre-carbonized and carbonized to obtain the hard carbon material.

[0021] In an optional embodiment, the preparation method further satisfies at least one of the following conditions ac:

[0022] a. The cellulose content in the biomass raw material is ≥35wt%, and the lignin content is ≥15wt%; preferably, the cellulose content in the biomass raw material is 35wt%-45wt%, and the lignin content is 17wt%-40wt%; more preferably, the cellulose content in the biomass raw material is 35wt%-45wt%, and the lignin content is 30wt%-40wt%;

[0023] b. The biomass raw material comprises a plant biomass raw material; further preferably, the plant biomass raw material is selected from at least one of bagasse, straw, corn cob, paper pulp and wood;

[0024] c. The oxygen content in the biomass raw material is W1, the oxygen content in the oxidation product is W2, (W1-W2) / W1≥65%; preferably, (W1-W2) / W1 is 90%-200%.

[0025] In an optional embodiment, the oxidation treatment includes gas phase oxidation and / or liquid phase oxidation.

[0026] In an optional embodiment, the oxidation reaction further satisfies at least one of the following (1)-(8):

[0027] (1) The gas phase oxidation is specifically a heating treatment in an oxygen-containing atmosphere, with a gas flow rate of 1 L / min-3 L / min;

[0028] (2) the oxygen-containing gas used for the gas-phase oxidation comprises at least one of air, oxygen or carbon dioxide;

[0029] (3) The heating temperature of the gas phase oxidation is 200° C.-400° C., and the time is 6 h-12 h;

[0030] (4) The liquid phase oxidation specifically includes treating the biomass raw material in a solution containing an oxidant;

[0031] (5) the oxidant used in the liquid phase oxidation comprises at least one of hydrogen peroxide, peracetic acid, sodium dichromate, chromic acid, nitric acid, potassium permanganate or ammonium persulfate;

[0032] (6) adding an oxidizing agent during the liquid phase oxidation treatment; further preferably, the oxidizing agent comprises ferrous sulfate; further preferably, the mass ratio of ferrous sulfate to biomass is 1:(2-10);

[0033] (7) The treatment temperature of the liquid phase oxidation is 30°C-50°C, and the treatment time is 10min-60min;

[0034] (8) The ratio of the biomass raw material used in the liquid phase oxidation to the oxidant is 1 g: (0.003-0.13) mol.

[0035] In an optional embodiment, the acid solution includes a group containing a doping element, and the group containing a doping element is selected from at least one of a phosphoric acid group, a carboxylic acid group and a sulfuric acid group;

[0036] Preferably, the acid solution comprises phosphoric acid and / or phytic acid; more preferably, the concentration of phytic acid in the acid solution is 20wt%-30wt%, and the concentration of phosphoric acid is 15wt%-20wt%;

[0037] Preferably, in the pickling step, the pickling time is 4h-8h;

[0038] Preferably, the oxidation product is washed with water before and after the acid washing.

[0039] In an optional embodiment, the pre-carbonization temperature is 700°C-1000°C, and the pre-carbonization time is 2h-4h;

[0040] And / or, the carbonization temperature is 1200° C.-1400° C., and the carbonization time is 1 h-4 h;

[0041] And / or, the pre-carbonized product is crushed before the carbonization step; preferably, the crushing method is ball milling, the ball milling speed is 100r / min-400r / min, and the ball milling time is 4h-10h.

[0042] In a third aspect, the present invention provides a negative electrode plate, comprising the hard carbon material described in the aforementioned embodiment or a hard carbon material prepared by any one of the methods of the aforementioned embodiment.

[0043] In a fourth aspect, the present invention provides a secondary battery comprising the negative electrode sheet described in the aforementioned embodiment.

[0044] In a fifth aspect, the present invention provides an electrical device, comprising the secondary battery described in the aforementioned embodiment.

[0045] The present invention has the following beneficial effects:

[0046] In the embodiment of the present invention, the hard carbon material with large pore size and large closed pore volume can provide more active sodium storage sites, which is beneficial to improve the initial coulombic efficiency of the hard carbon material. The graphite microcrystalline structure in the hard carbon material is narrower and longer, which is beneficial to the realization of large pore size and large closed pore volume of the hard carbon material. The hard carbon composite material prepared by the present invention has an excellent closed-pore structure, a low specific surface area, and has better reversible discharge specific capacity and first coulombic efficiency. At the same time, the pore structure of the hard carbon material can be effectively improved by regulating the oxygen content in the precursor after oxidation treatment, thereby enhancing the electrochemical performance of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0048] Figure 1 is a SEM image of the hard carbon material prepared in Example 1 of the present invention, and its magnification is 5000×;

[0049] Figure 2 yes Figure 1 A local enlarged image with a magnification of 50000×. DETAILED DESCRIPTION

[0050] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially, and the biomass used is dried and has a water content of less than 1wt%.

[0051] The embodiment of the present invention provides a hard carbon material, wherein the average pore size of the hard carbon material is 5nm-6nm and the total pore volume of the closed pores is 0.12cm 3 / g-0.30cm 3 / g;

[0052] Through XRD characterization, it is calculated that the crystallite size of the hard carbon material is 4.0nm-5.0nm in the crystal basal plane direction La and 1.00nm-1.30nm in the direction perpendicular to the basal plane Lc.

[0053] In the embodiment of the present invention, the average pore size of the hard carbon material is 5nm-6nm as measured by gas (such as nitrogen) adsorption method, and specifically can be 5nm, 5.2nm, 5.4nm, 5.6nm, 5.8nm, 6nm or any value between 5nm and 6nm; the total pore volume of the closed pores is 0.12cm 3 / g-0.30cm 3 / g, specifically 0.12cm 3 / g, 0.15cm 3 / g, 0.18cm 3 / g, 0.21cm 3 / g, 0.24cm 3 / g, 0.27cm 3 / g, 0.30cm 3 / g or 0.12cm 3 / g-0.30cm 3 / g. Hard carbon materials with suitable mesopore diameter and higher closed pore volume can provide more active sodium storage sites, which is beneficial to improve the initial Coulombic efficiency of hard carbon materials.

[0054] In the embodiment of the present invention, the crystallite size La of the hard carbon material in the crystal basal plane direction is 4.0nm-5.0nm, specifically 4.0nm, 4.1nm, 4.2nm, 4.3nm, 4.4nm, 4.5nm, 4.6nm, 4.7nm, 4.8nm, 4.9nm, 5.0nm or any value between 4.0nm-5.0nm; the vertical direction Lc in the basal plane direction is 1.00nm-1.30nm, specifically 1.00nm, 1.05nm, 1.10nm, 1.15nm, 1.2nm, 1.25nm, 1.30nm or any value between 1.00nm-1.30nm. The graphite crystal structure in the hard carbon material is narrower and longer, which is conducive to the realization of large pore size and large closed pore volume of the hard carbon material.

[0055] In an optional embodiment, the hard carbon material satisfies at least one of the following (1)-(7):

[0056] (1) The interlayer spacing d(002) of the hard carbon crystals in the hard carbon material is 0.390nm-0.400nm, specifically, it can be 0.390nm, 0.395nm, 0.400nm or any value between 0.390nm and 0.400nm. The larger interlayer spacing is beneficial to the diffusion of sodium ions and improves the stability of the hard carbon material during the sodiumation / de-sodiumation process.

[0057] (2) The specific surface area of ​​the hard carbon material is 4 cm 2 / g-8cm 2 / g, specifically 4cm 2 / g, 5cm 2 / g, 6cm 2 / g, 7cm 2 / g, 8cm 2 / g or 4cm 2 / g-8cm 2 / g; a certain specific surface area is beneficial to increase the provision of active sodium storage sites, but if the specific surface area is too large, defects and closed pores will be reduced, which will lead to a decrease in capacity and initial efficiency.

[0058] (3) I of the hard carbon material D / I G is 1.7-1.8, specifically can be 1.7, 1.72, 1.74, 1.76, 1.78, 1.8 or any value between 1.7 and 1.8;

[0059] (4) The hard carbon material is doped with at least one of phosphorus, nitrogen or sulfur, and the content of the doped element is ≥3wt%, specifically 3wt%, 5wt%, 7wt%, 9wt%, 11wt%, 13wt%, or any value ≥3wt%, preferably 4wt%-10wt%; the presence of the doping element is beneficial to improving the capacity and first coulombic efficiency of the hard carbon material.

[0060] (5) The hard carbon material includes biomass-based hard carbon.

[0061] (6) The reversible discharge specific capacity of the hard carbon material is greater than 340 mAh / g; more preferably, the reversible discharge specific capacity is greater than 360 mAh / g.

[0062] (7) The first efficiency of the hard carbon material is greater than 87%; more preferably, the first efficiency is greater than 91%.

[0063] The present invention also provides a method for preparing the hard carbon material described in the above embodiment, comprising the following steps:

[0064] performing oxidation treatment on the biomass raw material to obtain an oxidation product;

[0065] washing the oxidation product with an acid solution to obtain a purified product;

[0066] The purified product is sequentially pre-carbonized and carbonized to obtain the hard carbon material.

[0067] During the oxidation treatment step, cellulose glycosidic bonds undergo oxidative cleavage, inducing cross-linking of molecules and molecular chains. The oxidative cross-linking process of cellulose will produce more C=O and retain more CO, which is beneficial to the subsequent pre-carbonization and carbonization pyrolysis process, and will produce narrower and longer graphite microcrystalline structures, thereby forming larger and more closed pores.

[0068] On the one hand, the pickling step can remove the ash in the oxidation product. On the other hand, part of the acid solution reacts with the oxidation product to obtain a wood precursor containing doped elements. After pre-carbonization and carbonization, the doped hard carbon material is obtained, which is more conducive to improving the capacity and first coulomb efficiency of the hard carbon material. Pre-carbonization is conducive to reducing the oxygen content in the material. Without pre-carbonization treatment, the oxygen content in the purified product is too high, the structural stability is poor during the carbonization process, and the pore structure is difficult to shrink, which will lead to an excessively large specific surface area and a reduction in defects.

[0069] The embodiment of the present invention uses biomass as raw material to prepare hard carbon materials. The raw materials are widely available and inexpensive, which reduces environmental pollution and can effectively control the preparation cost. In addition, the biomass raw materials are rich in cellulose and lignin. Through oxidative cross-linking, the C=O structure is increased. After acid washing, not only the impurity content can be reduced, but also the element doping can be achieved. The material prepared after carbonization has good conductivity, which is conducive to improving the performance of the finished battery. In an optional embodiment, the preparation method also satisfies at least one of the following ac:

[0070] a. The cellulose content in the biomass raw material is ≥35wt%, and the lignin content is 15wt%; preferably, the cellulose content in the biomass raw material is 35wt%-45wt%, and the lignin content is 17wt%-40wt%; more preferably, the cellulose content in the biomass raw material is 35wt%-45wt%, and the lignin content is 30wt%-40wt%; it is difficult to achieve doping by acid washing after cellulose oxidation, so if the cellulose content is too high and the lignin content is low, the effect of oxidation acid washing on improving the electrical properties of hard carbon materials is limited.

[0071] b. The biomass raw material includes plant biomass raw materials; further preferably, the plant biomass raw material is selected from at least one of bagasse, straw, corn cob, paper pulp, and wood; the raw materials are widely available and inexpensive, which reduces environmental pollution and can effectively control the preparation cost.

[0072] c. The oxygen content in the biomass raw material is W1, the oxygen content in the oxidation product is W2, (W1-W2) / W1≥65%, specifically, it can be 65%, 100%, 150%, 200%, 250% or any value ≥65%; preferably, (W1-W2) / W1 is 90%-200%. The increase in the degree of oxidation is conducive to the production of narrower and longer graphite microcrystalline structures, thereby forming larger and more closed pores.

[0073] In an optional embodiment, the oxidation treatment includes gas phase oxidation and / or liquid phase oxidation, preferably liquid phase oxidation.

[0074] In an optional embodiment, the gas phase oxidation further satisfies at least one of the following (1)-(3):

[0075] (1) The gas phase oxidation is specifically a heating treatment in an oxygen-containing atmosphere, with a gas flow rate of 1 L / min-3 L / min;

[0076] (2) the oxygen-containing gas used for the gas-phase oxidation comprises at least one of air, oxygen or carbon dioxide;

[0077] (3) The heating temperature of the gas phase oxidation is 200°C-400°C, and the heating time is 6h-12h.

[0078] In an optional embodiment, the liquid phase oxidation further satisfies at least one of the following (1)-(5):

[0079] (1) The liquid phase oxidation specifically comprises treating the biomass raw material in a solution containing an oxidant, wherein the concentration of the oxidant in the solution is 20wt%-50wt%;

[0080] (2) the oxidant used in the liquid phase oxidation comprises at least one of hydrogen peroxide, peracetic acid, sodium dichromate, chromic acid, nitric acid, potassium permanganate or ammonium persulfate;

[0081] (3) adding an oxidizing agent during the liquid phase oxidation treatment; further preferably, the oxidizing agent includes a reducing metal ion such as ferrous sulfate; further preferably, the mass ratio of ferrous sulfate to biomass is 1:(2-10);

[0082] (4) The treatment temperature of the liquid phase oxidation is 30°C-50°C, and the treatment time is 10min-60min;

[0083] (5) The ratio of the biomass raw material used in the liquid phase oxidation to the oxidant is 1 g: (0.003-0.13) mol.

[0084] The specific steps of liquid phase oxidation include: mixing a reducing metal salt solution such as a ferrous sulfate solution with a biomass raw material for 0.5h-2h, and then separating the solid and the liquid to obtain a solid phase, which is the biomass raw material adsorbed with reducing metal ions; preferably, the mass ratio of ferrous ions in the ferrous sulfate solution to the biomass raw material is 1:(14-50); then mixing the biomass raw material adsorbed with reducing metal ions with an oxidant in a liquid phase to react, to obtain an oxidation product.

[0085] In the liquid phase oxidation step, ferrous ions are mainly used to embed into the fibers of biomass, and the subsequently added oxidants react with them to produce hydroxyl radicals, inducing cellulose bond breaking and cross-linking. In gas phase oxidation, the weight loss ranges of lignin and cellulose are different, which makes it difficult to control the oxidation temperature and degree of oxidation; hydrothermal pre-oxidation is cumbersome to operate and difficult to industrialize. Compared with gas phase oxidation and hydrothermal oxidation, liquid phase oxidation is simple to operate, has strong oxidizing properties, and is easy to control.

[0086] In an optional embodiment, the acid solution includes a group containing a doping element, and the group containing the doping element is selected from at least one of a phosphoric acid group, a carboxylic acid group and a sulfate group; during the pickling process, an esterification reaction occurs between the hydroxyl group of lignin and the group containing the doping element to form a bridge, thereby forming a wood precursor rich in the doping element.

[0087] Preferably, the acid solution includes phosphoric acid and / or phytic acid; more preferably, the concentration of phytic acid in the acid solution is 20wt%-30wt%, and the concentration of phosphoric acid is 15wt%-20wt%; using a mixed acid for pickling can increase the types of impurities removed, effectively improve the ash removal effect, and thus help improve the primary efficiency.

[0088] Preferably, in the pickling step, the pickling time is 4h-8h, and the pickling is performed until the washing solution is neutral or nearly neutral.

[0089] Preferably, the oxidation product is washed with water before and after the acid washing.

[0090] In an optional embodiment, the pre-carbonization temperature is 700°C-1000°C, specifically 700°C, 800°C, 900°C, 1000°C or any value between 700°C-1000°C, and the pre-carbonization time is 2h-4h, specifically 2h, 3h, 4h or any value between 2h-4h; pre-carbonization is carried out at a lower temperature, which is beneficial to reducing the oxygen content in the purified product and to maintaining the stability of the material structure and the shrinkage of the pore structure during the carbonization process.

[0091] In an optional embodiment, the carbonization temperature is 1200°C-1400°C, specifically 1200°C, 1250°C, 1300°C, 1350°C, 1400°C or any value between 1200°C-1400°C, and the carbonization time is 1h-4h, specifically 1h, 2h, 3h, 4h or any value between 1h-4h; the carbonization temperature will affect the specific surface area and interlayer spacing of the material. Too low a carbonization temperature will result in an excessively large specific surface area and reduced defects.

[0092] In an optional embodiment, the pre-carbonized product is crushed before the carbonization step; preferably, the crushing method is ball milling, the ball milling speed is 100r / min-400r / min, and the ball milling time is 4h-10h. Crushing can effectively destroy the original structure of the material, which is conducive to the shrinkage of the pore structure in the subsequent carbonization process and improves its surface defects.

[0093] An embodiment of the present invention further provides a negative electrode plate, comprising the hard carbon material described in the aforementioned embodiment or a hard carbon material prepared by any one of the methods of the aforementioned embodiment.

[0094] An embodiment of the present invention further provides a secondary battery, comprising the negative electrode sheet described in the above embodiment.

[0095] An embodiment of the present invention further provides an electrical device, comprising the secondary battery described in the above embodiment.

[0096] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0097] Example 1

[0098] This embodiment provides a method for preparing a hard carbon material, which specifically includes the following steps:

[0099] Take 30g of paper pulp (paper pulp from softwood kraft paper of a paper mill, with a cellulose content of 41.2wt% and a lignin content of 35.65wt%), 8g of ferrous sulfate heptahydrate, add them to 300mL of deionized water, stir for 1h, then add 30% concentration of hydrogen peroxide solution (the molar ratio of H2O2 to ferrous sulfate is 1:2), stir at 45°C for 40min, discard the solution, and obtain the oxidized precursor.

[0100] The precursor was pickled with a mixed acid of phytic acid (mass concentration of 50%) and phosphoric acid (mass concentration of 35%) in a volume ratio of 1:1 for 6 hours, washed with water and dried, and then pre-carbonized at 800°C for 3 hours to obtain a phosphorus-rich biomass precursor. After ball milling at 300 r / min for 10 hours, it was carbonized and cooled at 1300°C to obtain a hard carbon material. The SEM image is shown in FIG. Figure 1 and Figure 2 shown.

[0101] Example 2

[0102] This embodiment provides a method for preparing a hard carbon material, which specifically includes the following steps:

[0103] Take 30g of sugarcane bagasse (cellulose content 43.1wt%, lignin content 25wt%) and 10g of ferrous sulfate, add them to 300mL of deionized water, stir for 1.5h, then add hydrogen peroxide solution (the molar ratio of H2O2 to ferrous sulfate is 1:1.5), stir for 30min at 45°C, discard the solution, and obtain the oxidized precursor.

[0104] The precursor was pickled with a mixed acid of phytic acid (mass concentration of 50%) and phosphoric acid (mass concentration of 35%) in a volume ratio of 1:1 for 4.5 hours, washed with water and dried, and then pre-carbonized at 800°C for 3 hours to obtain a phosphorus-rich biomass precursor. After ball milling at 300 r / min for 10 hours, it was carbonized and cooled at 1300°C to obtain a hard carbon material.

[0105] Example 3

[0106] This embodiment provides a method for preparing a hard carbon material, which specifically includes the following steps:

[0107] Take 30g corn cob (cellulose content 39.7wt%, lignin content 17.8wt%), 5g ferrous sulfate, add to 300mL deionized water, stir for 1h, then add hydrogen peroxide solution (the molar ratio of H2O2 to ferrous sulfate is 1:1), stir at 45°C for 35min, discard the supernatant, and place the bottom product in a vacuum drying oven at 85°C for drying to obtain the oxidized precursor.

[0108] The precursor was pickled with a mixed acid of phytic acid (mass concentration of 50%) and phosphoric acid (mass concentration of 35%) in a volume ratio of 1:1 for 7 hours, washed with water and dried, and then pre-carbonized at 800°C for 3 hours to obtain a phosphorus-rich biomass precursor. After ball milling at 300 r / min for 10 hours, it was carbonized and cooled at 1300°C to obtain a hard carbon material.

[0109] Example 4

[0110] This embodiment provides a method for preparing a hard carbon material, which is mainly different from that of Embodiment 1 in that a different mixed acid is used for pickling, and specifically comprises the following steps:

[0111] Take 30g of paper pulp (paper pulp from softwood kraft paper of a paper mill, with a cellulose content of 41.2wt% and a lignin content of 35.65wt%), 8g of ferrous sulfate heptahydrate, add them to 300mL of deionized water, stir for 1h, then add hydrogen peroxide solution (the molar ratio of H2O2 to ferrous sulfate is 1:2), stir at 45°C for 30min, discard the solution, and obtain an oxidized precursor.

[0112] The precursor was pickled with a mixed acid of phytic acid (mass concentration of 50%) and phosphoric acid (mass concentration of 35%) in a volume ratio of 1:1 for 6 hours, and then pre-carbonized at 800°C for 3 hours to obtain a phosphorus-rich biomass precursor. After ball milling at 300 r / min for 10 hours, it was carbonized and cooled at 1300°C to obtain a hard carbon material.

[0113] Example 5

[0114] This embodiment provides a method for preparing a hard carbon material, which is mainly different from Embodiment 1 in that the pre-carbonization temperature is lowered, and specifically comprises the following steps:

[0115] Take 30g of paper pulp (paper pulp from softwood kraft paper of a paper mill, with a cellulose content of 41.2wt% and a lignin content of 35.65wt%), 8g of ferrous sulfate heptahydrate, add them to 300mL of deionized water, stir for 1h, then add hydrogen peroxide solution (the molar ratio of H2O2 to ferrous sulfate is 1:2), stir at 45°C for 30min, discard the solution, and obtain an oxidized precursor.

[0116] The precursor was pickled with a mixed acid of phytic acid (mass concentration of 50%) and phosphoric acid (mass concentration of 35%) in a volume ratio of 1:1 for 6 hours, washed with water and dried, and then pre-carbonized at 600°C for 3 hours to obtain a phosphorus-rich biomass precursor. After ball milling at 300 r / min for 10 hours, it was carbonized and cooled at 1300°C to obtain a hard carbon material.

[0117] Example 6

[0118] This embodiment provides a method for preparing a hard carbon material, which is mainly different from Embodiment 1 in that the ball milling speed is reduced, and specifically comprises the following steps:

[0119] Take 30g of paper pulp (paper pulp from softwood kraft paper of a paper mill, with a cellulose content of 41.2wt% and a lignin content of 35.65wt%), 8g of ferrous sulfate heptahydrate, add them to 300mL of deionized water, stir for 1h, then add hydrogen peroxide solution (the molar ratio of H2O2 to ferrous sulfate is 1:2), stir at 45°C for 40min, discard the solution, and obtain an oxidized precursor.

[0120] The precursor was pickled with a mixed acid of phytic acid (mass concentration of 50%) and phosphoric acid (mass concentration of 35%) in a volume ratio of 1:1 for 6 hours, washed with water and dried, and then pre-carbonized at 800°C for 3 hours to obtain a phosphorus-rich biomass precursor. After ball milling at 100 r / min for 6 hours, it was carbonized and cooled at 1300°C to obtain a hard carbon material.

[0121] Example 7

[0122] This embodiment provides a method for preparing a hard carbon material, which is mainly different from Embodiment 1 in that the carbonization temperature is lowered, and specifically comprises the following steps:

[0123] Take 30g of paper pulp (paper pulp from softwood kraft paper of a paper mill, with a cellulose content of 41.2wt% and a lignin content of 35.65wt%), 8g of ferrous sulfate heptahydrate, add them to 300mL of deionized water, stir for 1h, then add hydrogen peroxide solution (the molar ratio of H2O2 to ferrous sulfate is 1:2), stir at 45°C for 40min, discard the solution, and obtain an oxidized precursor.

[0124] The precursor was pickled with a mixed acid of phytic acid (mass concentration of 50%) and phosphoric acid (mass concentration of 35%) in a volume ratio of 1:1 for 6 hours, washed with water and dried, and then pre-carbonized at 800°C to obtain a phosphorus-rich biomass precursor. After ball milling at 300 r / min for 10 hours, it was carbonized and cooled at 1200°C to obtain a hard carbon material.

[0125] Example 8

[0126] This embodiment provides a method for preparing a hard carbon material, which is mainly different from Embodiment 7 in that the amount of ferrous sulfate used is reduced, and specifically comprises the following steps:

[0127] Take 30g of paper pulp (paper pulp from softwood kraft paper of a paper mill, with a cellulose content of 41.2wt% and a lignin content of 35.65wt%), 5g of ferrous sulfate heptahydrate, add them to 300mL of deionized water, stir for 1h, then add hydrogen peroxide solution (the molar ratio of H2O2 to ferrous sulfate is 1:2), stir at 45°C for 40min, discard the solution, and obtain an oxidized precursor.

[0128] The precursor was pickled with a mixed acid of phytic acid (mass concentration of 50%) and phosphoric acid (mass concentration of 35%) in a volume ratio of 1:1 for 6 hours, washed with water and dried, and then pre-carbonized at 800°C to obtain a phosphorus-rich biomass precursor. After ball milling at 300 r / min for 10 hours, it was carbonized and cooled at 1200°C to obtain a hard carbon material.

[0129] Example 9

[0130] This embodiment provides a method for preparing a hard carbon material, which is mainly different from Embodiment 7 in that the amount of ferrous sulfate used is increased, and specifically comprises the following steps:

[0131] Take 30g of paper pulp (paper pulp from softwood kraft paper of a paper mill, with a cellulose content of 41.2wt% and a lignin content of 35.65wt%), 15g of ferrous sulfate heptahydrate, add them to 300mL of deionized water, stir for 1h, then add hydrogen peroxide solution (the molar ratio of H2O2 to ferrous sulfate is 1:2), stir at 45°C for 40min, discard the solution, and obtain an oxidized precursor.

[0132] The precursor was pickled with a mixed acid of phytic acid (mass concentration of 50%) and phosphoric acid (mass concentration of 35%) in a volume ratio of 1:1 for 6 hours, washed with water and dried, and then pre-carbonized at 800°C to obtain a phosphorus-rich biomass precursor. After ball milling at 300 r / min for 10 hours, it was carbonized and cooled at 1200°C to obtain a hard carbon material.

[0133] Example 10

[0134] This embodiment provides a method for preparing a hard carbon material, which is different from Embodiment 7 mainly in that the oxidation method is different, and specifically includes the following steps:

[0135] Take 30g of paper pulp (paper pulp from softwood kraft paper of a paper mill, with a cellulose content of 41.2wt% and a lignin content of 35.65wt%), place it in a nitrogen atmosphere, let air in, and heat to 300°C for 9 hours with an air flow rate of 2L / min to obtain an oxidized precursor.

[0136] The precursor was pickled with a mixed acid of phytic acid (mass concentration of 50%) and phosphoric acid (mass concentration of 35%) in a volume ratio of 1:1 for 6 hours, washed with water and dried, and then pre-carbonized at 800°C to obtain a phosphorus-rich biomass precursor. After ball milling at 300 r / min for 10 hours, it was carbonized and cooled at 1200°C to obtain a hard carbon material.

[0137] Comparative Example 1

[0138] This embodiment provides a method for preparing a hard carbon material. The remaining operations are the same as those in Embodiment 1, except that the raw material used is microcrystalline cellulose.

[0139] Comparative Example 2

[0140] This embodiment provides a method for preparing a hard carbon material. The remaining operations are the same as those in Embodiment 1, except that ferrous sulfate heptahydrate is not added.

[0141] Comparative Example 3

[0142] This embodiment provides a method for preparing a hard carbon material. The remaining operations are consistent with those in Embodiment 1, except that no mixed acid is added for treatment.

[0143] Comparative Example 4

[0144] This embodiment provides a method for preparing a hard carbon material. The remaining operations are the same as those in Embodiment 1, except that no pre-carbonization is performed, and carbonization is performed directly after ball milling.

[0145] Comparative Example 5

[0146] This embodiment provides a method for preparing a hard carbon material. The remaining operations are the same as those in Embodiment 1, except that the carbonization is performed directly without ball milling after pre-carbonization.

[0147] Comparative Example 6

[0148] This embodiment provides a method for preparing a hard carbon material. The remaining operations are the same as those in Embodiment 1, except that high-temperature carbonization is performed at 1000°C.

[0149] Application Examples

[0150] The hard carbon materials of each embodiment and comparative example were subjected to N2 adsorption and desorption to detect the specific surface area. The specific surface area and pore structure were determined by gas adsorption method, and the interlayer spacing was calculated by XRD. The wavelength of the incident light was The intensity of the typical D peak and G peak was measured by Raman spectroscopy. D / I G The calculation results are shown in Table 1:

[0151] Table 1

[0152]

[0153]

[0154] From the analysis of Table 1: In the present invention, the oxidation of hydroxyl radicals generated by the reaction of ferrous sulfate and hydrogen peroxide can effectively oxidize the cellulose in the raw material, oxidatively cleave the cellulose glycosidic bonds, and induce molecular cross-linking and molecular chain cross-linking. The cellulose oxidation cross-linking process will produce more C=O and retain more CO, so that the precursor O content increases, and in the carbonization pyrolysis process, a narrower and longer graphite microcrystalline structure will be produced, thereby forming larger closed pores. The raw material that has not been oxidized by hydroxyl radicals has a smaller pore volume and average pore size.

[0155] Treatment with phosphoric acid and phytic acid can effectively remove the ash, and the esterification reaction between the hydroxyl groups of lignin and the phosphate groups in the mixed acid of phytic acid and phosphoric acid forms a bridge, thereby forming a phosphorus-rich wood precursor, which can effectively improve the interlayer spacing, reversible discharge specific capacity, and first coulombic efficiency of the subsequently prepared hard carbon.

[0156] The oxygen content before carbonization is significantly lower than that of the sample after pre-oxidation treatment, which is beneficial to structural stability and the shrinkage of the pore structure. The oxygen content of the sample without pre-carbonization is too high, and the subsequent carbonization after ball milling is not conducive to structural stability and the shrinkage of the pore structure, resulting in a larger specific surface area and fewer defects.

[0157] During the preparation process, adding ball milling can effectively destroy its original structure, which is conducive to the shrinkage of the pore structure and the improvement of its surface defects in the subsequent carbonization process. The precursor without ball milling treatment has significantly poorer specific surface area, reversible discharge specific capacity and first coulombic efficiency after carbonization.

[0158] During the carbonization process, the carbonization temperature controls the specific surface area and interlayer spacing. A lower carbonization temperature can maintain the interlayer spacing, but it causes the carbonized product to have a larger specific surface area, and poor reversible discharge specific capacity and first coulombic efficiency.

[0159] The negative electrode materials obtained in each embodiment and comparative example were used to prepare sodium ion batteries according to the following methods.

[0160] A method for preparing a button-type sodium ion battery comprises the following steps:

[0161] According to the ratio of active material: SP: CMC: SBR = 94:2:1.5:2.5, the negative electrode material, SP, CMC, and SBR were weighed respectively and mixed evenly in deionized water to form a slurry; the evenly mixed slurry was coated on the aluminum foil current collector, baked in an oven at 80°C for 1h, and then cooled to room temperature.

[0162] Adjust the rolling distance to roll the pole piece. Cut the rolled pole piece into a small disc with a diameter of 14 mm and weigh it as m1. Similarly, cut the aluminum foil current collector into a small disc with a diameter of 14 mm and weigh it as m2. (m1-m2)*0.94 is the mass of the active material, recorded as m3. The weighed small disc is then placed in an 80℃ oven and vacuum-dried for 12 hours.

[0163] The vacuum-dried small disc was transferred to a glove box, and a sodium ion button cell was assembled in a glove box with oxygen and water contents less than 0.01 ppm, using a sodium sheet as a counter electrode and an auxiliary electrode, an electrolyte of 1 M NaPF6 / EC:DMC:DEC=2:2:1, and a glass fiber separator as a separator;

[0164] The assembled button-type sodium ion battery was left to stand for 12 hours. The electrochemical performance of the button-type sodium ion battery was tested at a constant current on the Wuhan Blue Electric Battery Test System. The test results are shown in Table 2.

[0165] Table 2

[0166]

[0167] From the examples and comparative examples 1-6 in Table 2, it can be seen that the hard carbon prepared by using raw materials rich in cellulose and lignin has the best reversible discharge specific capacity and first coulombic efficiency. 2+ Embedded in cellulose, it reacts with the added hydrogen peroxide, and the strong oxidizing effect of the generated hydroxyl radicals oxidizes the cellulose, which is conducive to the generation of more C=O structures. After being treated with a mixed acid of phosphoric acid and phytic acid, it not only removes impurities, but also can cross-link with lignin at the same time. In the subsequent pre-carbonization process, the in-situ generation of CO and PO bonds on the surface can effectively increase the specific capacity and the first coulomb efficiency. After ball milling, the defects on its surface are increased, which is conducive to the contraction of the pore structure in the subsequent carbonization process. The prepared hard carbon has a low specific surface area, excellent reversible discharge specific capacity and first coulomb efficiency. And further, by regulating the oxygen content in the precursor after oxidation treatment, the pore structure of the hard carbon material can be effectively improved, and the electrochemical performance of the product can be enhanced.

[0168] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0169] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

[0170] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A hard carbon material, characterized in that: The average pore size of the hard carbon material measured by gas adsorption method is 5nm-6nm, and the total pore volume of the closed pores is 0.12cm 3 / g-0.30cm 3 / g; Through XRD characterization, it is calculated that the crystallite size of the hard carbon material is 4.0nm-5.0nm in the crystal basal plane direction La and 1.00nm-1.30nm in the direction perpendicular to the basal plane Lc.

2. The hard carbon material according to claim 1, characterized in that The hard carbon material satisfies at least one of the following (1) to (7): (1) The hard carbon crystal interlayer spacing d(002) in the hard carbon material is 0.390 nm to 0.400 nm; (2) The specific surface area of ​​the hard carbon material is 4 cm 2 / g-8cm 2 / g; (3) I of the hard carbon material D / I G 1.7-1.8; (4) The hard carbon material is doped with at least one of phosphorus, nitrogen or sulfur, and the content of the doped element is ≥ 3wt%, preferably 4wt%-10wt%; (5) The hard carbon material comprises biomass-based hard carbon; (6) The reversible discharge specific capacity of the hard carbon material is greater than 340 mAh / g; (7) The initial efficiency of the hard carbon material is greater than 87%.

3. A method for preparing the hard carbon material according to claim 1, characterized in that: The following steps are involved: performing oxidation treatment on the biomass raw material to obtain an oxidation product; washing the oxidation product with an acid solution to obtain a purified product; The purified product is sequentially pre-carbonized and carbonized to obtain the hard carbon material.

4. The method for preparing a hard carbon material according to claim 3, characterized in that: The preparation method also satisfies at least one of the following ac: a. The cellulose content in the biomass raw material is ≥35wt%, and the lignin content is ≥15wt%; preferably, the cellulose content in the biomass raw material is 35wt%-45wt%, and the lignin content is 17wt%-40wt%; more preferably, the cellulose content in the biomass raw material is 35wt%-45wt%, and the lignin content is 30wt%-40wt%; b. The biomass raw material comprises a plant biomass raw material; more preferably, the plant biomass raw material is selected from at least one of bagasse, straw, corn cob, paper pulp and wood; c. The oxygen content in the biomass raw material is W1, the oxygen content in the oxidation product is W2, (W1-W2) / W1≥65%; preferably, (W1-W2) / W1 is 90%-200%.

5. The method for preparing a hard carbon material according to claim 3, characterized in that: The oxidation treatment includes gas phase oxidation and / or liquid phase oxidation.

6. The method for preparing a hard carbon material according to claim 5, characterized in that: The oxidation treatment further satisfies at least one of the following (1) to (8): (1) The gas phase oxidation is specifically a heating treatment in an oxygen-containing atmosphere, with a gas flow rate of 1 L / min-3 L / min; (2) the oxygen-containing gas used for the gas-phase oxidation comprises at least one of air, oxygen or carbon dioxide; (3) The heating temperature of the gas phase oxidation is 200° C.-400° C., and the time is 6 h-12 h; (4) The liquid phase oxidation specifically includes treating the biomass raw material in a solution containing an oxidant; (5) the oxidant used in the liquid phase oxidation comprises at least one of hydrogen peroxide, peracetic acid, sodium dichromate, chromic acid, nitric acid, potassium permanganate or ammonium persulfate; (6) adding an oxidizing agent during the liquid phase oxidation treatment; more preferably, the oxidizing agent comprises ferrous sulfate; more preferably, the mass ratio of ferrous sulfate to biomass is 1:(2-10); (7) The treatment temperature of the liquid phase oxidation is 30°C-50°C, and the treatment time is 10min-60min; (8) The ratio of the biomass raw material used in the liquid phase oxidation to the oxidant is 1 g: (0.003-0.13) mol.

7. The method for preparing a hard carbon material according to claim 3, characterized in that: The acid solution includes a group containing a doping element, and the group containing the doping element is selected from at least one of a phosphoric acid group, a carboxylic acid group and a sulfuric acid group; Preferably, the acid solution comprises phosphoric acid and / or phytic acid; more preferably, the concentration of phytic acid in the acid solution is 20wt%-30wt%, and the concentration of phosphoric acid is 15wt%-20wt%; Preferably, in the pickling step, the pickling time is 4h-8h; Preferably, the oxidation product is washed with water before and after the acid washing.

8. The method for preparing a hard carbon material according to claim 3, characterized in that: The pre-carbonization temperature is 700℃-1000℃, and the pre-carbonization time is 2h-4h; And / or, the carbonization temperature is 1200° C.-1400° C., and the carbonization time is 1 h-4 h; And / or, the pre-carbonized product is crushed before the carbonization step; preferably, the crushing method is ball milling, the ball milling speed is 100r / min-400r / min, and the ball milling time is 4h-10h.

9. A negative electrode plate, characterized in that: The invention comprises the hard carbon material according to claim 1 or 2 or the hard carbon material prepared by any one of the methods of claims 3-8.

10. A secondary battery, characterized in that: Including the negative electrode sheet as described in claim 9.

Citation Information

Patent Citations

  • Lignin-based compound carbon fiber and preparation method thereof

    CN107326477A

  • Method for preparing high-capacity hard carbon negative electrode material of lithium ion battery

    CN109921020A

  • Hard carbon negative electrode material of sodium-ion battery based on shell biomass and preparation method of hard carbon negative electrode material

    CN113666356A

  • Biomass hard carbon based on low crystalline cellulose content and preparation method and application thereof

    CN115064667A

  • Sodium-ion battery hard carbon negative electrode material and preparation method and application thereof

    CN116253306A

Cited By

  • Hard carbon paper negative electrode material based on papermaking process regulation and control as well as preparation method and application of hard carbon paper negative electrode material

    CN121626964A

  • Hard carbon paper negative electrode material based on papermaking process regulation and preparation method and application thereof

    CN121626964B

  • Hard carbon paper negative electrode material based on TEMPO oxidation modification and preparation method and application thereof

    CN121757839A