Method for preparing high-concentration alkali liquor and calcium phosphate through causticization reaction of by-product trisodium phosphate crystal and quicklime
Trisodium phosphate is recovered through waste alkali water treatment produced by baking with rare earth slag and alkali, and reacted with quicklime to produce high-concentration NaOH and high-purity calcium phosphate, which solves the problems of insufficient recycling and complex process, and improves resource recycling Efficiency and reduce production costs.
Patent Information
- Application Number
- CN202411137658.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-01
AI Technical Summary
In the prior art, when treating phosphorus-containing wastewater, calcium phosphate is insufficiently recycled, the process is complicated, and sodium hydroxide is not effectively utilized, resulting in high production costs and low environmental efficiency.
The waste alkali water treatment of rare earth ore or rare earth-containing residues and alkali-calcined residues produced by baking of waste alkali, and caustic reaction with quicklime to produce high-concentration NaOH solution and high-purity calcium phosphate, reducing precipitation method to remove phosphorus The process is complex and comprehensively utilized wastewater elements to produce trisodium phosphate crystals, high-concentration NaOH solution and calcium phosphate.
While achieving phosphorus in phosphorus removal wastewater, high concentration liquid alkali and high purity calcium phosphate by-products are produced, which reduces the complexity of the precipitation method phosphorus removal process, increases the added value of the phosphorus removal environmental protection process, and reduces production costs. And improve the efficiency of resource recycling and utilization.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of phosphorus-containing wastewater recycling and utilization, and particularly relates to a method for preparing high-concentration alkali solution and calcium phosphate by reacting by-product trisodium phosphate crystals with quicklime. Background Art
[0002] At present, the main methods for treating phosphorus-containing wastewater include chemical precipitation method (Rodriguez-LMVallet-Regim. Controlled crystallization of calcium phosphate apatites [J]. ChemMater 2000, 12: 2460-2465), hydrothermal method (Wen Ximei, Guo Jinwu, Zhang Jun, et al. Hydrothermal preparation of hydroxyapatite whiskers assisted by sorbitol [J]. Inorganic Salt Engineering 2008 40 (11): 21-23.), sol-gel method, etc. (Huang Zhiliang, Wang Dawei, Liu Yu, et al. Crystal chemistry FTIR study of hydroxyapatite solid solution replaced by different types of CO2-3 [J]. Journal of Inorganic Chemistry 2002 18 (5): 469-473.). Among them, chemical precipitation is the most widely used due to its simple process. Common chemical reagents used to precipitate phosphorus ("Calcium Method for Treatment of High-Concentration Phosphorus-Containing Wastewater", China Water Supply and Drainage, 2003 Vol. 19, No. 5, p91-92.) include iron salts, aluminum salts, calcium salts, etc. Since hydroxyapatite has the largest equilibrium constant and the most stable properties, most of them use lime to form calcium phosphate precipitation to remove phosphorus.
[0003] The lime removal method currently used to remove phosphorus from wastewater is to add lime milk to phosphorus-containing wastewater to generate calcium phosphate containing more other impurities, remove phosphorus from the wastewater, and the calcium phosphate is not recycled; or in order to obtain high-purity calcium phosphate, the reaction process requires precise control of the solution pH value, which has high operating requirements and complex processes. Moreover, the currently commonly used method does not effectively utilize NaOH due to the low concentration of sodium hydroxide in the treated wastewater. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing high-concentration alkali solution and calcium phosphate by causticizing the by-product trisodium phosphate crystals with quicklime.
[0005] The present invention recovers trisodium phosphate crystals or slurry by treating the waste alkali water generated by alkali roasting of rare earth ore or slag containing a certain amount of rare earth after rare earth separation, and further uses the trisodium phosphate crystals or slurry to perform causticizing reaction with quicklime to generate a high-concentration NaOH solution and a high-purity calcium phosphate byproduct. The present invention produces high-concentration liquid alkali and high-purity calcium phosphate byproducts while removing phosphorus from phosphorus-containing wastewater, reduces the complexity of the precipitation phosphorus removal process, and comprehensively utilizes the elements in the wastewater to produce three byproducts-trisodium phosphate crystals, high-concentration NaOH solution, and high-purity calcium phosphate, thereby increasing the added value of the phosphorus removal environmental protection process and reducing production costs.
[0006] The technical solution adopted by the present invention to solve the technical problem is as follows:
[0007] The present invention provides a method for preparing high-concentration alkali solution and calcium phosphate by producing trisodium phosphate crystals through causticizing reaction with quicklime, which specifically comprises the following steps:
[0008] (1) adding alkali to the rare earth enrichment and roasting it to prepare the slurry, heating the slurry and filtering it into a plate-frame filter press to separate the solid and liquid, and filtering the separated phosphorus-containing waste alkali water into a crystallization tank for water cooling or natural cooling crystallization to generate trisodium phosphate dodecahydrate crystals, and filtering the crystal slurry into a plate-frame filter press to separate the solid and liquid to obtain trisodium phosphate crystals and low-alkalinity waste alkali water, and recycling the low-alkalinity waste alkali water;
[0009] (2) adding trisodium phosphate crystals or crystal slurry to waste alkali water, heating until fully dissolved, adding quicklime to the resulting liquid, and stirring after heat preservation until the reaction is complete to perform causticization reaction;
[0010] (3) The slurry after the causticizing reaction is put into a plate and frame filter press for solid-liquid separation to obtain lime slag cake and high-concentration alkali solution, and the high-concentration alkali solution is recycled;
[0011] (4) After washing the lime slag cake with washing water, the lime slag cake is put into a plate and frame filter press for solid-liquid separation to obtain a calcium phosphate cake as a calcium phosphate byproduct, and the separated filtrate is recycled.
[0012] As a preferred embodiment, in step (1), the rare earth concentrate is alkali-roasted and then slurried, and the slurry is heated to 70-100°C.
[0013] As a preferred embodiment, in step (1), the NaOH concentration in the phosphorus-containing waste alkali water is 1-3 mol / L; the NaOH concentration in the low-alkalinity waste alkali water is 1-3 mol / L.
[0014] As a preferred embodiment, in step (2), the liquid-to-solid ratio of the waste alkali water to trisodium phosphate crystals is 0.5-1.5; and the NaOH concentration in the waste alkali water is 0.5 mol / L-3.5 mol / L.
[0015] As a preferred embodiment, in step (2), trisodium phosphate crystals or slurry are added to waste alkali water and heated to 80°C-100°C to fully dissolve.
[0016] As a preferred embodiment, in step (2), the mass ratio of the trisodium phosphate crystals to quicklime is (1.5-3.1):1.
[0017] As a preferred embodiment, in step (2), the insulation treatment time is 30 min-120 min, and the temperature is 70-100°C.
[0018] As a preferred embodiment, step (2) is replaced by the following steps: adding quicklime to waste alkali water, heating until fully dissolved, adding trisodium phosphate crystals or slurry to the resulting liquid, and stirring after heat treatment until the reaction is complete to carry out causticization reaction.
[0019] As a preferred embodiment, in step (3), the NaOH concentration in the highly concentrated alkali solution is 5 mol / L-9 mol / L; in step (4), the NaOH concentration in the separated filtrate is 1.5 mol / L-3.5 mol / L.
[0020] As a preferred embodiment, in step (4), the liquid-to-solid ratio of the wash water to the lime slag cake is 0.5-2.
[0021] The beneficial effects of the present invention are:
[0022] The invention adopts a self-developed process to recover trisodium phosphate slurry or crystals from a production system, and uses the trisodium phosphate crystals or slurry as a raw material to react with solid lime in alkaline water, thereby removing phosphorus in the waste alkaline water, and generating a high-concentration NaOH solution and high-purity calcium phosphate in the process of converting the by-product trisodium phosphate into calcium phosphate, comprehensively recovering and utilizing sodium hydroxide and calcium phosphate, and improving the efficiency of the environmental protection treatment process. Meanwhile, the invention can generate three by-products, namely, trisodium phosphate crystals, calcium phosphate crystals and high-concentration NaOH solution, and reduce the cost of the environmental protection process. DETAILED DESCRIPTION
[0023] The present invention provides a method for preparing high-concentration alkali solution and calcium phosphate by producing trisodium phosphate crystals through causticizing reaction with quicklime, which can achieve the following purposes and functions:
[0024] (1) The present invention controls the alkalinity and temperature of phosphorus-containing waste alkali water to cool and crystallize to produce trisodium phosphate crystals.
[0025] (2) Conversion of trisodium phosphate to NaOH. The present invention utilizes trisodium phosphate and quicklime for causticization reaction to generate a highly concentrated NaOH solution, thereby converting waste alkaline water into highly concentrated alkaline water.
[0026] (3) Wastewater treatment. The fluorine and phosphorus in the waste alkaline water are causticized and enter the calcium phosphate cake, so that the phosphorus content in the produced high-concentration alkaline water can be reduced to below 0.01g / L.
[0027] (4) Recovery of sodium, phosphorus and fluorine resources. The present invention can convert the sodium, phosphorus and fluorine in the waste alkaline water and the generated trisodium phosphate crystals into NaOH and calcium phosphate and calcium fluoride for recycling.
[0028] (5) The lime slag after causticization is washed with water, and the NaOH adsorbed by the lime slag is recovered and further used for causticizing bottom water.
[0029] The present invention provides a method for preparing high-concentration alkali solution and calcium phosphate by producing trisodium phosphate crystals through causticizing reaction with quicklime, which specifically comprises the following steps:
[0030] (1) Rare earth enriched alkali (rare earth ore or slag containing a certain amount of rare earth after rare earth separation) is roasted and slurried, the slurry is heated to 70-100° C. and then filtered into a plate-frame filter press for solid-liquid separation, the separated phosphorus-containing waste alkali water (NaOH concentration is 1-3 mol / L) is pumped into a crystallization tank for water cooling or natural cooling crystallization to generate trisodium phosphate dodecahydrate crystals, the crystal slurry is pumped into a plate-frame filter press for solid-liquid separation to obtain trisodium phosphate crystals and low-alkalinity waste alkali water (NaOH concentration is 1-3 mol / L), and the low-alkalinity waste alkali water is recycled.
[0031] In step (1), the slurry of the alkali roasted enrichment should be heated to above 70°C and the NaOH concentration should be controlled to a certain level. When the concentration is low, the solution is not saturated and trisodium phosphate crystals cannot be precipitated subsequently.
[0032] (2) adding trisodium phosphate crystals to waste alkali water at a ratio of 0.5-1.5 in the liquid-to-solid ratio of waste alkali water (NaOH concentration of 0.5 mol / L-3.5 mol / L) to trisodium phosphate crystals, heating to 80°C-100°C to fully dissolve, adding quicklime to the resulting liquid at a mass ratio of trisodium phosphate crystals to quicklime (1.5-3.1):1, heat-insulating treatment (time of 30 min-120 min, temperature of 70-100°C), and stirring until the reaction is complete to carry out causticizing reaction.
[0033] Among them, the insulation reaction time and temperature need to be adjusted according to the amount of trisodium phosphate crystals to be processed.
[0034] Alternatively, the above step (2) is replaced by the following steps: quicklime is added to waste alkali water, heated until fully dissolved, trisodium phosphate crystals are added to the resulting liquid, and after heat treatment, the mixture is stirred until the reaction is complete to carry out causticization reaction.
[0035] Among them, quicklime can be added gradually in several steps or all at once. It is necessary to ensure that the quicklime is in a local excess state during the reaction to increase the causticization rate.
[0036] Among them, the stirring speed after heat preservation treatment is kept at medium and high speed. The general laboratory electric stirring speed is 700-1500 rpm. In actual production, the stirring speed needs to be adjusted accordingly according to the material processing volume.
[0037] (3) The slurry after the causticizing reaction is sent into a plate and frame filter press for solid-liquid separation to obtain lime slag cake and high-concentration alkali solution (NaOH concentration is 5 mol / L-9 mol / L), and the high-concentration alkali solution is recycled.
[0038] (4) washing the lime slag cake with washing water in a ratio of 0.5-2 in terms of liquid-solid ratio of washing water to lime slag cake, and then filtering the lime slag cake in a plate-frame filter press for solid-liquid separation to obtain a calcium phosphate cake as a calcium phosphate byproduct, and recycling the separated filtrate (with a NaOH concentration of 1.5 mol / L-3.5 mol / L).
[0039] The washing water may be the low alkalinity waste water or sand filtered water obtained in step (1).
[0040] The present invention provides a method for preparing high-concentration alkali solution and calcium phosphate by producing trisodium phosphate crystals through causticizing reaction with quicklime, and the main process principle is:
[0041] (1) Preparation process principle of trisodium phosphate crystals
[0042] The rare earth enriched material is alkali roasted and then slurried. The slurry is heated to above 70°C, the solid and liquid are separated, and the separated alkaline water is cooled and crystallized to produce trisodium phosphate crystals, thereby reducing the phosphorus content in the alkaline water to meet environmental protection requirements. At the same time, the phosphorus and sodium in the waste alkaline water are recovered and converted into trisodium phosphate crystals as a by-product, or as a raw material for causticization reaction to produce a high-concentration NaOH solution for production, and a by-product of calcium phosphate is produced.
[0043] (2) Causticization reaction produces high-concentration alkaline water and calcium phosphate
[0044] a. The reaction equation is as follows:
[0045] CaO+H 2 O=Ca(OH) 2
[0046] 3Ca(OH) 2 +2Na 3 PO 4 =Ca 3 (PO 4 ) 2 +6NaOH
[0047] b. Process principle: Use quicklime and low-alkalinity waste alkali water and trisodium phosphate generated by the production system to carry out high-temperature causticization reaction to generate high-concentration NaOH solution and calcium phosphate. Use low-alkalinity waste alkali water or sand-filtered water generated by the production system to wash the NaOH adsorbed by calcium phosphate to produce medium- and low-concentration alkali water, which is further used for high-temperature causticization reaction. The washed calcium phosphate is used as a by-product, thereby converting trisodium phosphate and low-alkalinity waste alkali water generated by the production system into high-concentration NaOH solution for production, and producing by-product calcium phosphate, while reducing the phosphorus and fluorine content in the waste alkali water.
[0048] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0049] Example 1
[0050] (1) Take trisodium phosphate crystals prepared from the washing water of the alkali roasting enrichment on the production line, waste alkali water, and 85% pure quicklime. Pour 800ml of low-concentration alkali water (NaOH1.5mol / L) into a 2000ml beaker. Add 656g of trisodium phosphate, stir and heat to above 85°C, rotate at 800rpm, pour 285g of lime at one time, start stirring, the initial liquid level is about 1500ml, flush with water during the causticization process to maintain this liquid level until the reaction is completed, and the insulation time is 60min. After the reaction is completed, use a circulating water vacuum pump to filter and separate the solid and liquid. The filtrate is a high-concentration alkali water with a NaOH concentration of 5.04mol / L and a phosphate content of 0.028g / L. Add 1000ml of water to the filter residue, stir and wash, and vacuum filter to obtain a NaOH solution (NaOH1.55mol / L).
[0051] Example 2
[0052] (2) Take trisodium phosphate crystals prepared from the washing water of the alkaline roasting enrichment on the production line, waste alkali water, and 85% pure quicklime. Pour 400ml of low-concentration alkaline water (NaOH 0.8mol / L) into a 1000ml beaker, add 328g of trisodium phosphate, heat to above 80°C, add 150g of quicklime, and stir to react for 60min. After the reaction is completed, filter with a circulating water vacuum pump to separate the solid and liquid. The filtrate is high-concentration alkaline water with a NaOH concentration of 5.56mol / L. Add 500ml of water to the filter residue, stir and wash, and vacuum filter to obtain a NaOH solution (NaOH 1.94mol / L). The calcium residue after washing and vacuum filtration has a phosphate content of 19.06%, a calcium oxide content of 42.25%, and a water content of 32.09%.
[0053] Example 3
[0054] (3) Take trisodium phosphate crystals prepared from the washing water of the alkali roasting enrichment on the production line, waste alkali water, and 85% pure quicklime. Pour 400ml of low-concentration alkaline water (NaOH2.11mol / L) into a 1000ml beaker, add 150g of quicklime, stir for 10 minutes, and mix evenly. Heat to above 80°C, add 328g of trisodium phosphate, and stir to react for 60min. After the reaction is completed, filter with a circulating water vacuum pump to separate the solid and liquid. The filtrate is high-concentration alkaline water with a NaOH concentration of 8.08mol / L. Add 500ml of water to the filter residue, stir and wash, and vacuum filter to obtain a NaOH solution (NaOH3.41mol / L).
[0055] The present invention discloses a method for preparing high-concentration alkali solution and calcium phosphate by reacting trisodium phosphate crystals with quicklime for causticization. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the method. It is particularly important to point out that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The product of the present invention has been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the product described herein without departing from the content, spirit and scope of the present invention to realize and apply the technology of the present invention.
Claims
1. A method for producing trisodium phosphate crystals as by-products and reacting with quicklime to prepare highly concentrated alkali solution and calcium phosphate, It is characterized in that The following steps are involved: (1) adding alkali to the rare earth enrichment and roasting it to prepare the slurry, heating the slurry and filtering it into a plate-frame filter press to separate the solid and liquid, and filtering the separated phosphorus-containing waste alkali water into a crystallization tank for water cooling or natural cooling crystallization to generate trisodium phosphate dodecahydrate crystals, and filtering the crystal slurry into a plate-frame filter press to separate the solid and liquid to obtain trisodium phosphate crystals and low-alkalinity waste alkali water, and recycling the low-alkalinity waste alkali water; (2) adding trisodium phosphate crystals or crystal slurry to waste alkali water, heating until fully dissolved, adding quicklime to the resulting liquid, and stirring after heat preservation until the reaction is complete to perform causticization reaction; (3) The slurry after the causticizing reaction is put into a plate and frame filter press for solid-liquid separation to obtain lime slag cake and high-concentration alkali solution, and the high-concentration alkali solution is recycled; (4) After washing the lime slag cake with washing water, the lime slag cake is put into a plate and frame filter press for solid-liquid separation to obtain a calcium phosphate cake as a calcium phosphate byproduct, and the separated filtrate is recycled.
2. A method for preparing high-concentration alkali solution and calcium phosphate by causticizing a by-product trisodium phosphate crystal with quicklime according to claim 1, It is characterized in that In step (1), the rare earth concentrate is alkali-roasted and then slurried, and the slurry is heated to 70-100°C.
3. A method for preparing highly concentrated alkali solution and calcium phosphate by producing trisodium phosphate crystals through causticizing reaction with quicklime according to claim 1, It is characterized in that In step (1), the NaOH concentration in the phosphorus-containing waste alkali water is 1-3 mol / L; the NaOH concentration in the low-alkalinity waste alkali water is 1-3 mol / L.
4. The method according to claim 1, wherein the by-product trisodium phosphate crystals are reacted with quicklime to prepare a highly concentrated alkali solution and calcium phosphate, It is characterized in that In step (2), the liquid-to-solid ratio of the waste alkali water to the trisodium phosphate crystals is 0.5-1.5; and the NaOH concentration in the waste alkali water is 0.5 mol / L-3.5 mol / L.
5. A method for preparing high-concentration alkali solution and calcium phosphate by causticizing a by-product trisodium phosphate crystal with quicklime according to claim 1, It is characterized in that In step (2), trisodium phosphate crystals or slurry are added to the waste alkali water and heated to 80°C-100°C to fully dissolve.
6. A method according to claim 1 for preparing highly concentrated alkali solution and calcium phosphate by producing trisodium phosphate crystals through causticizing reaction with quicklime, It is characterized in that In step (2), the mass ratio of the trisodium phosphate crystals to quicklime is (1.5-3.1):
1.
7. The method according to claim 1, wherein the by-product trisodium phosphate crystals are reacted with quicklime to prepare a highly concentrated alkali solution and calcium phosphate, It is characterized in that In step (2), the heat preservation treatment time is 30min-120min, and the temperature is 70-100°C.
8. The method according to claim 1, wherein the by-product trisodium phosphate crystals are reacted with quicklime to prepare a highly concentrated alkali solution and calcium phosphate, It is characterized in that Step (2) is replaced by the following steps: adding quicklime to the waste alkali water, heating until fully dissolved, adding trisodium phosphate crystals or slurry to the resulting liquid, and stirring after heat preservation until the reaction is complete to carry out causticization reaction.
9. The method according to claim 1, wherein the by-product trisodium phosphate crystals are reacted with quicklime to prepare a highly concentrated alkali solution and calcium phosphate, It is characterized in that In step (3), the NaOH concentration in the highly concentrated alkali solution is 5 mol / L-9 mol / L; in step (4), the NaOH concentration in the separated filtrate is 1.5 mol / L-3.5 mol / L.
10. The method according to claim 1, wherein the by-product trisodium phosphate crystals are reacted with quicklime to prepare a highly concentrated alkali solution and calcium phosphate, It is characterized in that In step (4), The liquid-to-solid ratio of the wash water to the lime slag cake described in the claims is 0.5-2.