Preparation method of hafnium tantalate powder

Preparation of Hf6Ta2O17 powder by one-step oxidation method solves the problem of insufficient phase stability and anti-CMAS corrosion performance of thermal barrier coating materials at high temperatures, as well as the lower capacitance of the electrode active material of supercapacitor and poor cycle stability, achieving high-performance thermal Barrier coating and electrode active material preparation.

CN118877938AInactive Publication Date: 2024-11-01SHANDONG UNIV OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411250865.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing thermal barrier coating materials have insufficient high-temperature phase stability, thermal shock resistance and CMAS corrosion resistance, and the low specific capacitance of the electrode active materials of supercapacitors and poor cycle stability.

Method used

(Hf,Ta)(C,N) carbon nitride is used as the precursor, and Hf6Ta2O17 powder is prepared by one-step oxidation method, simplifying the production process, reducing energy consumption, avoiding the use of organic solvents, and improving environmental protection and production safety.

Benefits of technology

The preparation of high-performance thermal barrier coatings and supercapacitor electrode active materials is realized, with high melting point, excellent high temperature stability, excellent thermodynamic and mechanical properties, and significantly improves the cyclic stability and energy density of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention provides a preparation method of hafnium tantalate (Hf6Ta2O17) powder, and belongs to the technical field of ceramic powder preparation. (Hf, Ta) (C, N) carbonitride is used as a precursor, and hafnium tantalate powder is generated through one-step oxidation reaction. Specifically, the method comprises the following steps: placing a precursor in a furnace, heating the precursor to 1000-1500 DEG C at a heating rate of 5 DEG C / min in an air atmosphere, calcining the precursor for 1-5 hours, and cooling the precursor to room temperature to obtain the Hf6Ta2O17 powder. The preparation method is simple, does not need to use an organic solvent, and is suitable for batch production. The Hf6Ta2O17 powder shows wide application potential in the aspects of high-performance thermal barrier coatings and electrode active materials of supercapacitors. The defects of an existing thermal barrier coating material in high-temperature phase stability, mechanical performance and volcanic ash (CMAS) corrosion resistance are overcome, and the challenges of a supercapacitor electrode material in the aspects of specific capacitance and cycling stability are overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing hafnium tantalate powder, which is suitable for high-performance thermal barrier coatings and electrode active materials of supercapacitors. Background Art

[0002] Thermal barrier coatings (TBCs) play a vital role in modern aircraft engines and gas turbines. Their main function is to improve the operating temperature and service life of high-temperature alloys and ceramic materials. Although the current thermal barrier coating technology has made significant progress, the existing materials still have problems with high-temperature phase stability and insufficient thermal shock resistance. 7-8wt% yttria (Y2O3) partially stabilized zirconium oxide (ZrO2) (abbreviated as 8YSZ) has become the most widely used thermal barrier coating ceramic material because of its high melting point, low thermal conductivity and good chemical inertness. However, in an operating environment exceeding 1200°C, 8YSZ will undergo a phase transition from tetragonal to monoclinic phase, which is accompanied by volume expansion and internal stress accumulation, leading to cracking and peeling of the coating, significantly reducing the service life of the coating. This defect makes 8YSZ unable to meet the service requirements of advanced aircraft engine hot end components at higher temperatures. In addition, during operation, aircraft engines may inhale siliceous minerals including air dust, sand, fly ash, volcanic ash, airport runway debris, and fuel residues. These substances will form molten calcium magnesium aluminum silicate (CMAS: CaO-MgO-AlO 1.5 -SiO2) and deposited on the surface of TBCs, and then continuously penetrated and dissolved its structure. The CMAS corrosion phenomenon reduces the strain tolerance of the coating, significantly shortens the service life of the coating, and becomes the main factor accelerating the spalling of TBCs. This highly corrosive use environment poses a severe challenge to the performance of TBCs materials. In particular, 8YSZ has poor resistance to molten CMAS corrosion. In view of this, there is an urgent need to develop a new type of thermal barrier coating material that should have good high-temperature phase stability, superior mechanical properties and excellent resistance to CMAS corrosion to meet the needs of future aero engines and gas turbines in extreme environments.

[0003] Hafnium tantalate (Hf6Ta2O 17 ) has great application potential in the field of high-performance thermal barrier coating materials due to its excellent thermomechanical properties and resistance to CMAS corrosion. 17 Belongs to A6B2O 17 The unique superstructure and excellent physical properties of this material make it have outstanding performance in extreme environments. The crystal structure of this material belongs to the orthorhombic system, and the lattice parameters are a= 4.941 Å, b= 86.71 Å, c= 5.264 Å, α=90o , β = 90 o , γ=90 o . This structure is composed of a series of asymmetric oxygen polyhedral units centered on cations, including [TaO6] distorted octahedrons, [HfO7] capped triangular prisms, and [TaO8] distorted double-capped triangular prisms periodically arranged along the

[100] direction. Among them, the [TaO6] octahedron is located on the two-fold axis parallel to the a-axis, while the [TaO8] double-pointed triangular prism is located at the midpoint of the [TaO6] octahedron, maintaining mirror symmetry. In addition, due to the similarity of the atomic radii of Hf and Ta, the cation sublattice forms a modulation structure with a modulation wave vector q=(0.125, 0, 0), resulting in a superstructure with a multiplicity of 8. These complex crystal properties are the key to the Hf6Ta2O 17 It provides excellent performance foundation in high temperature applications. In terms of performance, Hf6Ta2O 17 It exhibits a room temperature hardness of 18.45 GPa and a low thermal conductivity (2.89 W•m -1 •K -1 ) and low thermal expansion coefficient (9.59×10 -6 K -1 ). It has no phase transition from room temperature to the melting point of 2450°C, which ensures volume stability in high-temperature applications, far exceeding the phase transition temperature of 8YSZ (1200°C). In addition, Hf6Ta2O 17 The bonded shoe has excellent corrosion resistance to molten CMAS in the temperature range of 1523-1673 K, and has significant high-temperature chemical stability and can effectively resist water vapor erosion. In addition, its fracture toughness ranges from 3.8 MPa•m in the range of 25°C to 1600°C. 1 / 2 Reduced to 0.6 MPa•m 1 / 2 , better than La2Zr2O7 (about 1.5 MPa•m 1 / 2 ) and YTaO4 (2~3 MPa•m 1 / 2 ), and close to 8YSZ (4.41~1.01 MPa•m 1 / 2 ). Under the same conditions, Hf6Ta2O 17 The creep resistance of Hf6Ta2O is better than that of 8YSZ, with a stress index of 2~3 and an activation energy of 600~620 kJ / mol. 17 With its high melting point, excellent thermal stability, low oxygen mobility, and outstanding thermodynamic and mechanical properties, it is expected to become an ideal material for the next generation of high-performance thermal barrier coatings.

[0004] In addition, Hf6Ta2O 17It can also be used as an electrode active material for supercapacitors, mainly due to its unique ultra-large crystal structure and large gaps, which provide excellent channels for the transmission of ions and charges in the lattice. In addition, its inherent anion vacancies can be used as effective energy storage sites. With the rapid development of renewable energy such as wind power and photovoltaic power generation, although these forms of energy are environmentally friendly, they are limited by factors such as land resources and intermittent output. Efficient and stable energy storage equipment is needed to improve energy utilization efficiency in order to achieve the purpose of stable supply. In this context, supercapacitors have advantages in applications of short-term energy absorption or release due to their high power density, fast charging and discharging capabilities and long cycle life, making them an ideal choice for solving the above challenges. The basic structure of a supercapacitor includes electrodes, electrolytes, non-conductive diaphragms and current collectors, among which the electrode active material is the core component. The electrode is usually composed of an electrode active material, a conductive agent and a binder, and the choice of the electrode active material directly affects the performance of the supercapacitor. At present, there are three main types of commonly used electrode active materials: carbon-based materials, metal oxides and hydroxide materials, and conductive polymers. Carbon-based materials are widely used due to their good cycle stability, simple process and low cost, but their specific capacity is low. Metal oxide and hydroxide materials provide higher specific capacity, but they are expensive, short-lived and may be toxic. Conductive polymer materials have good electronic conductivity, low internal resistance and high specific capacity, but their cycle stability is poor. Hf6Ta2O 17 It is a promising electrode active material. The material shows better electrochemical performance than single metal oxides such as HfO2 and Ta2O5. -1 At a current density of 394.6 F g -1 The specific capacitance of Hf6Ta2O is 2V, and it has a wide voltage window of 2V. More importantly, 17 After 5,000 charge and discharge cycles, it can maintain 87.5% of its initial specific capacitance, showing excellent cycle stability. 17 Type composite metal oxide Hf6Ta2O 17 It shows great potential in improving the energy density and performance of supercapacitors and is expected to become a key electrode material for future high-efficiency supercapacitors.

[0005] According to the phase diagram of HfO2-Ta2O5, Hf6Ta2O 17 It can stably exist and maintain the same crystal phase in a larger synthesis range. 17 The powder is mainly produced by solid phase method and sol-gel method. The solid phase method uses HfO2 and Ta2O5 powder as raw materials, mixes them by ball milling and calcines them at high temperature to obtain Hf6Ta2O 17Powder. Zheng et al. in the paper “High-temperature compressive creep behavior and mechanism of Hf6Ta2O 17 In the study, Hf6Ta2O was successfully prepared by mixing HfO2 and Ta2O5 in a molar ratio of 7.33:1 and then subjecting them to a high-temperature solid-phase reaction at 1600°C for 20 hours. 17 Subsequently, the powder was cold pressed into blocks and sintered at normal pressure (first heated to 800°C for 2 hours and then heated to 1600°C for 20 hours). The average grain size of the sample was 2.1 μm and the volume density was 10.15 g / cm 3 , Hf6Ta2O with a relative density of 95.9% 17 Ceramics. Hf6Ta2O 17 The ceramic exhibits excellent creep resistance in the temperature range of 1100℃ to 1300℃, with a creep strain rate of 2×10 -7 s -1 ~1.8×10 -4 s -1 In contrast, the creep strain rate of 8YSZ ceramics in the temperature range of 1000℃ to 1200℃ is 8.3×10 -7 s -1 ~7.5×10 -4 s -1 Although this method is simple to operate and easy to industrialize, it may be difficult to prepare pure phase Hf6Ta2O due to uneven mixing of raw material powders, which may easily introduce impurities. 17 Another effective technology for preparing ceramic powders is the sol-gel method; for example, Hao et al. 17 In the process of "ceramics fabricated by solvothermal and pressure-less sintering", hafnium chloride (HfCl4) and tantalum chloride (TaCl5) were used as raw materials, and acetylacetone was selected as a chelating agent. Through the sol-gel combined with solvothermal esterification reaction and low-temperature heat treatment (1000°C), a single-phase Hf6Ta2O with an average particle size of about 2μm was successfully synthesized. 17 Subsequently, the powder was subjected to cold isostatic pressing and pressureless sintering at 1400°C~1700°C (keeping temperature for 1 hour) to prepare Hf6Ta2O 17The density of the ceramic is significantly improved. Especially after sintering at 1700°C, the relative density of the obtained ceramic block reaches 96.30%, and the density is 10.19 g / cm 3 It is worth noting that as the temperature increases, Hf6Ta2O 17 The thermal conductivity of ceramics decreases and the coefficient of thermal expansion increases; these properties stabilize at high temperatures. At 1500°C, Hf6Ta2O 17 The thermal conductivity of Hf6Ta2O is only 1.62 W / (m⋅K), which is much lower than that of traditional 8YSZ ceramics. 17 The material has great potential as a high-performance thermal barrier coating. Although the sol-gel method can synthesize high-purity powders, the gel is prone to agglomeration, which may lead to inhomogeneity in the size and morphology of the ceramic particles. Summary of the invention

[0006] In summary, Hf6Ta2O 17 The excellent properties of the powder have attracted wide attention due to its potential application in high-performance thermal barrier coatings and supercapacitor electrode active materials. 17 The method uses (Hf,Ta)(C,N) carbonitride as a precursor to directly prepare Hf6Ta2O by a one-step oxidation method. 17 This preparation technology not only simplifies the production process, reduces energy consumption, but also avoids the use of organic solvents, significantly improving environmental protection and production safety. In addition, the simplicity of this method also makes mass production possible, further improving the feasibility of industrial application. 17 Powders have broad application prospects in the fields of high-performance thermal barrier coatings and supercapacitors.

[0007] In order to overcome the limitations of existing thermal barrier coating materials in terms of high temperature phase stability, thermal shock resistance, CMAS corrosion resistance and service life, and to solve the problems of low specific capacitance and poor cycle stability of electrode active materials of supercapacitors, the present invention proposes a Hf6Ta2O 17 Powder preparation method. This method uses (Hf, Ta) (C, N) carbonitride powder as raw material and successfully prepares Hf6Ta2O by a one-step oxidation method. 17 Powder. Its technical route mainly includes the following two steps:

[0008] (1) With (Hf x Ta 1-x )(C y N 1-y) (x=0.5~0.8, y=0.78~0.84) carbonitride as the precursor. The precursor is placed in a furnace, heated to 1000℃~1500℃ at a heating rate of 5℃ / min in an air atmosphere and kept at this temperature for 1~5 hours to perform an oxidation reaction. After the reaction is completed, the product is naturally cooled to room temperature with the furnace to obtain Hf6Ta2O 17 Powder.

[0009] (2) The preparation method of (Hf,Ta)(C,N) precursor is as follows: HfC and TaC powders are used as raw materials, and metal Co powder is selected as flux; (1) HfC and TaC powders are accurately weighed according to the molar ratio of (1-4):1; at the same time, the mass ratio of the total mass of carbide to the mass of metal Co is maintained at 3:7, and they are thoroughly mixed; (2) The mixed powder is pressed into a mold, and then moved into a furnace, and heated to 1500-1700℃ at a heating rate of 5-10℃ / min in a nitrogen environment, and kept warm for 1-8h. After the heat treatment is completed, the product is cooled to room temperature with the furnace to obtain a (Hf,Ta)(C,N) / Co metal-based ceramic block; (3) The block is immersed in a 7.2mol / L dilute nitric acid solution to dissolve and corrode the Co alloy matrix therein; (4) After the corrosion is completed, it is filtered, washed multiple times and dried to obtain (Hf,Ta)(C,N) carbonitride powder.

[0010] The working principle of the present invention is: the selected (Hf x Ta 1-x )(C y N 1-y ) (x=0.5~0.8, y=0.78~0.84) carbonitride raw material has a NaCl type crystal structure, belongs to the cubic system, and has a space group of Fm3m. In this crystal structure, Hf and Ta atoms are evenly distributed at the vertices and body center positions of the lattice according to the corresponding molar ratio, while C and N atoms are evenly distributed at the midpoints of the edges and the center positions of the faces. This arrangement structure is conducive to the common diffusion of Hf and Ta atoms, thereby improving the uniformity and efficiency of the oxidation reaction. During the oxidation process, since the internal migration distance of Hf and Ta atoms in the dense octahedral coordination crystal structure is short, the speed of the oxidation reaction is accelerated, so that the entire oxidation process is completed in a shorter time, the preparation efficiency is improved, and the energy consumption is reduced. Therefore, the present invention realizes a simplified preparation process by using (Hf, Ta) (C, N) carbonitride as a precursor, which can efficiently promote the uniform reaction of oxygen atoms with Hf and Ta atoms in the crystal structure. Finally, this efficient oxidation reaction forms Hf6Ta2O 17Oxide. In the traditional solid phase reaction, unevenness may occur during the mixing process of HfO2 and Ta2O5 powder raw materials, resulting in an increase in the diffusion distance between Hf and Ta atoms, which usually requires a higher reaction temperature and a longer insulation time to obtain the desired oxide. In contrast, although the sol-gel method can implement the oxidation reaction at a lower temperature, its process is complicated. The process often uses a variety of organic solvents, and agglomeration is prone to occur, making it difficult to control the morphological uniformity of the product. The method of the present invention ensures high-quality Hf6Ta2O by taking advantage of the uniformity of the elements in the precursor and the advantages of the crystal structure. 17 The formation of oxides significantly shortens the preparation cycle, simplifies the process flow, and has outstanding industrial application potential.

[0011] The present invention has the following advantages:

[0012] (1) The preparation process of the present invention is simple, the preparation cycle is short, and energy saving is achieved; no organic solvent is required, and the preparation process is safe and environmentally friendly, providing conditions for industrial-scale production.

[0013] (2) Hf6Ta2O prepared by the present invention 17 With its high melting point, excellent high-temperature stability, outstanding thermodynamics, mechanical properties, and excellent energy storage and cycle stability, it is expected to become an ideal thermal barrier coating material and electrode active material for supercapacitors, demonstrating its great potential in high-performance applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is Hf6Ta2O prepared in Example 1 17 XRD pattern of powder.

[0015] Figure 2 It is Hf6Ta2O prepared in Example 2 17 XRD pattern of powder.

[0016] Figure 3 It is Hf6Ta2O prepared in Example 2 17 SEM image of powder.

[0017] Figure 4 It is Hf6Ta2O prepared in Example 2 17 EDS spectrum of powder.

[0018] Figure 5 It is Hf6Ta2O prepared in Example 3 17 XRD pattern of powder.

[0019] Figure 6 It is Hf6Ta2O prepared in Example 3 17SEM image of powder.

[0020] Figure 7 It is Hf6Ta2O prepared in Example 3 17 EDS spectrum of powder.

[0021] Figure 8 It is Hf6Ta2O prepared in Example 4 17 XRD pattern of powder.

[0022] Fig. 9 It is Hf6Ta2O prepared in Example 5 17 XRD pattern of powder.

[0023] Fig.10 It is Hf6Ta2O prepared in Example 5 17 SEM image of powder.

[0024] Fig.11 It is Hf6Ta2O prepared in Example 5 17 EDS spectrum of powder.

[0025] Fig.12 It is Hf6Ta2O prepared in Example 6 17 XRD pattern of powder.

[0026] Fig.13 It is Hf6Ta2O prepared in Example 6 17 SEM image of powder.

[0027] Fig.14 It is Hf6Ta2O prepared in Example 6 17 EDS spectrum of powder.

[0028] Fig.15 It is Hf6Ta2O prepared in Example 7 17 XRD pattern of powder.

[0029] Fig.16 It is Hf6Ta2O prepared in Example 8 17 XRD pattern of powder.

[0030] Fig.17 It is Hf6Ta2O prepared in Example 9 17 XRD pattern of powder.

[0031] Fig.18 It is Hf6Ta2O prepared in Example 9 17 SEM image of powder.

[0032] Fig.19It is Hf6Ta2O prepared in Example 10 17 XRD pattern of powder.

[0033] Fig. 20 It is Hf6Ta2O prepared in Example 10 17 SEM image of powder.

[0034] Fig.21 It is Hf6Ta2O prepared in Example 11 17 XRD pattern of powder.

[0035] Fig. 22 It is Hf6Ta2O prepared in Example 11 17 SEM image of powder.

[0036] Fig.23 It is Hf6Ta2O prepared in Example 12 17 XRD pattern of powder.

[0037] Fig.24 It is Hf6Ta2O prepared in Example 12 17 SEM image of powder. DETAILED DESCRIPTION

[0038] The technical solution of the present invention is not limited to the specific embodiments listed below, but also includes any combination of the specific implementation modes.

[0039] Example 1

[0040] In this embodiment, Hf6Ta2O 17 The preparation method of the powder is as follows: 0.8 Ta 0.2 )(C 0.84 N 0.16 ) carbonitride as a precursor. The precursor is placed in a furnace, heated to 1400°C at a heating rate of 5°C / min in an air atmosphere, and kept warm for 2 hours to perform an oxidation reaction. After the reaction is completed, the product is naturally cooled to room temperature with the furnace to obtain Hf6Ta2O 17 Powder.

[0041] The (Hf 0.8 Ta 0.2 )(C 0.84 N 0.16) precursor preparation method is as follows: HfC and TaC powders are used as raw materials, and metal Co powder is used as flux; (1) HfC and TaC powders are accurately weighed according to a molar ratio of 4:1; at the same time, the mass ratio of the total mass of carbide to the mass of metal Co is maintained at 3:7 and mixed until uniform; (2) After the mixed powder is pressed into shape using a mold, it is moved into a furnace and heated to 1700℃ at a heating rate of 10℃ / min in a nitrogen environment and kept at this temperature for 1h. After the heat treatment is completed, the product is cooled to room temperature with the furnace to obtain (Hf 0.8 Ta 0.2 )(C 0.84 N 0.16 ) / Co metal-based ceramic block; (3) immersing the obtained ceramic block in a 7.2 mol / L dilute nitric acid solution to dissolve and corrode the Co alloy matrix therein; (4) after the corrosion is completed, filtering, washing and drying for multiple times to obtain (Hf 0.8 Ta 0.2 )(C 0.84 N 0.16 )Carbonitride powder.

[0042] The prepared Hf6Ta2O 17 The powder was subjected to X-ray diffraction phase analysis (XRD), and the test results are as follows: Figure 1 In the obtained XRD spectrum, each characteristic peak is clear and sharp, corresponding to the orthorhombic Hf6Ta2O 17 Specifically, the strong diffraction peaks at 30.4°, 34.1°, 35.2°, 50.6° and 51.5° correspond to the (1171), (002), (0340), (202) and (2340) crystal planes, respectively, indicating that the sample has good crystallinity, confirming the successful preparation of Hf6Ta2O 17 Oxide.

[0043] Example 2

[0044] In this embodiment, Hf6Ta2O 17 The preparation method of the powder is as follows: 0.8 Ta 0.2 )(C 0.84 N 0.16 ) carbonitride as a precursor. The precursor is placed in a furnace, heated to 1200°C at a heating rate of 5°C / min in an air atmosphere, and kept warm for 2 hours to perform an oxidation reaction. After the reaction is completed, the product is cooled to room temperature with the furnace to obtain Hf6Ta2O 17 Powder. Among them, (Hf 0.8 Ta 0.2 )(C 0.84 N 0.16) The preparation method of the powder is the same as that in Example 1.

[0045] The prepared Hf6Ta2O 17 The powder was subjected to X-ray diffraction phase analysis (XRD), and the test results are as follows: Figure 2 In the obtained XRD spectrum, each characteristic peak is clear and sharp, corresponding to the orthorhombic Hf6Ta2O 17 Specifically, the strong diffraction peaks at 30.4°, 34.1°, 35.2°, 50.6° and 51.5° correspond to the (1171), (002), (0340), (202) and (2340) crystal planes, respectively, indicating that the sample has good crystallinity, confirming the successful preparation of Hf6Ta2O 17 Oxide.

[0046] Figure 3 Hf6Ta2O 17 Scanning electron microscope (SEM) image of the powder. Figure 3 (a) The oxidation products are shown to be in the shape of exploded firecrackers and irregular shapes, with a size of about 0.9 to 2.5 µm, which helps to increase the specific surface area of ​​the material; Figure 3 (b) shows that the surface of the oxidation product is composed of obvious and compact nanoparticles with a particle size of about 60-140 nm. The compact nanoparticle structure not only increases the surface active sites of the material, but also may enhance the density of the material, improve its high temperature phase stability and anti-CMAS corrosion performance.

[0047] The Hf6Ta2O 17 The powders were subjected to energy dispersive X-ray spectroscopy (EDS) point analysis, as Figure 4 EDS results show that the oxidation product contains Hf, Ta, O and C elements, with a molar ratio of Hf:Ta of 3.4:1; further confirming that the prepared sample is Hf6Ta2O 17 powder.

[0048] Example 3

[0049] In this embodiment, Hf6Ta2O 17 The preparation method of the powder is as follows: 0.8 Ta 0.2 )(C 0.84 N 0.16 ) carbonitride as a precursor. The precursor is placed in a furnace, heated to 1000°C at a heating rate of 5°C / min in an air atmosphere, and kept warm for 2 hours to perform an oxidation reaction. After the reaction is completed, the product is cooled to room temperature with the furnace to obtain Hf6Ta2O 17 Powder. Among them, (Hf0.8 Ta 0.2 )(C 0.84 N 0.16 ) The preparation method of the precursor is the same as that in Example 1.

[0050] The prepared Hf6Ta2O 17 The powder was subjected to X-ray diffraction phase analysis (XRD), and the test results are as follows: Figure 5 In the obtained XRD spectrum, each characteristic peak is clear and sharp, corresponding to the orthorhombic Hf6Ta2O 17 Specifically, the strong diffraction peaks at 30.4°, 34.1°, 35.2°, 50.6° and 51.5° correspond to the (1171), (002), (0340), (202) and (2340) crystal planes, respectively, indicating that the sample has good crystallinity, confirming the successful preparation of Hf6Ta2O 17 Oxide.

[0051] Figure 6 Hf6Ta2O 17 Scanning electron microscope (SEM) image of the powder. Figure 6 (a) The oxidation products are shown to be in the shape of exploded firecrackers and irregular shapes, with a size of about 0.7-1.8 µm, which helps to increase the specific surface area of ​​the material; Figure 6 (b) shows that the surface of the oxidation product is composed of obvious and compact nanoparticles with a particle size of about 20-35 nm. The compact nanoparticle structure not only increases the surface active sites of the material, but also may enhance the density of the material, improve its high temperature phase stability and anti-CMAS corrosion performance.

[0052] The Hf6Ta2O 17 The powders were subjected to energy dispersive X-ray spectroscopy (EDS) point analysis, as Figure 7 EDS results show that the oxidation product contains Hf, Ta, O and C elements, with a molar ratio of Hf:Ta of 3.12:1; further confirming that the prepared sample is Hf6Ta2O 17 powder.

[0053] Example 4

[0054] In this embodiment, Hf6Ta2O 17 The preparation method of the powder is as follows: 0.6 Ta 0.4 )(C 0.84 N 0.16) carbonitride as a precursor. The precursor is placed in a furnace, heated to 1400°C at a heating rate of 5°C / min in an air atmosphere, and kept warm for 2 hours to perform an oxidation reaction. After the reaction is completed, the product is cooled to room temperature with the furnace to obtain Hf6Ta2O 17 Powder.

[0055] The (Hf 0.6 Ta 0.4 )(C 0.84 N 0.16 ) precursor preparation method is as follows: HfC and TaC powders are used as raw materials, and metal Co powder is used as flux; (1) HfC and TaC powders are accurately weighed according to a molar ratio of 1.5:1; at the same time, the mass ratio of the total mass of carbide to the mass of metal Co is maintained at 3:7 and mixed until uniform; (2) After the mixed powder is pressed into shape using a mold, it is moved into a furnace and heated to 1700℃ at a heating rate of 10℃ / min in a nitrogen environment and kept at this temperature for 1h. After the heat treatment is completed, the product is cooled to room temperature with the furnace to obtain (Hf 0.6 Ta 0.4 )(C 0.84 N 0.16 ) / Co metal-based ceramic block; (3) immersing the obtained ceramic block in a 7.2 mol / L dilute nitric acid solution to dissolve and corrode the Co alloy matrix therein; (4) after the corrosion is completed, filtering, washing and drying for multiple times to obtain (Hf 0.6 Ta 0.4 )(C 0.84 N 0.16 )Carbonitride powder.

[0056] The prepared Hf6Ta2O 17 The powder was subjected to X-ray diffraction phase analysis (XRD), and the test results are as follows: Figure 8 In the obtained XRD spectrum, each characteristic peak is clear and sharp, corresponding to the orthorhombic Hf6Ta2O 17 Specifically, the strong diffraction peaks at 30.4°, 34.1°, 35.2°, 50.6° and 51.5° correspond to the (1171), (002), (0340), (202) and (2340) crystal planes, respectively, indicating that the sample has good crystallinity, confirming the successful preparation of Hf6Ta2O 17 Oxide.

[0057] Example 5

[0058] In this embodiment, Hf6Ta2O 17 The preparation method of the powder is as follows: 0.6 Ta 04 )(C0.84 N 0.16 ) carbonitride as a precursor. The precursor is placed in a furnace, heated to 1200°C at a heating rate of 5°C / min in an air atmosphere, and kept warm for 2 hours to perform an oxidation reaction. After the reaction is completed, the product is cooled to room temperature with the furnace to obtain Hf6Ta2O 17 Powder. Among them, (Hf 0.6 Ta 04 )(C 0.84 N 0.16 ) The preparation method of the precursor is the same as that in Example 4.

[0059] The prepared Hf6Ta2O 17 The powder was subjected to X-ray diffraction phase analysis (XRD), and the test results are as follows: Fig. 9 In the obtained XRD spectrum, each characteristic peak is clear and sharp, corresponding to orthorhombic Hf6Ta2O 17 Specifically, the strong diffraction peaks at 30.4°, 34.1°, 35.2°, 50.6° and 51.5° correspond to the (1171), (002), (0340), (202) and (2340) crystal planes, respectively, indicating that the sample has good crystallinity, confirming the successful preparation of Hf6Ta2O 17 Oxide.

[0060] Fig.10 Hf6Ta2O 17 Scanning electron microscope (SEM) image of the powder. Fig.10 (a) The oxidation products are shown to be in the shape of exploded firecrackers and irregular shapes, with a size of about 0.8-2.0 µm, which helps to increase the specific surface area of ​​the material; Fig.10 (b) shows that the surface of the oxidation product is composed of obvious and compact nanoparticles with a particle size of about 90~140 nm. The compact nanoparticle structure not only increases the surface active sites of the material, but also may enhance the density of the material, improve its high temperature phase stability and anti-CMAS corrosion performance.

[0061] The Hf6Ta2O 17 The powders were subjected to energy dispersive X-ray spectroscopy (EDS) point analysis, as Fig.11 The EDS results show that the oxidation product contains Hf, Ta, O and C elements, which further confirms that the prepared sample is Hf6Ta2O 17 powder.

[0062] Example 6

[0063] In this embodiment, Hf6Ta2O 17The preparation method of the powder is as follows: 0.6 Ta 04 )(C 0.84 N 0.16 ) carbonitride as a precursor. The precursor is placed in a furnace, heated to 1000°C at a heating rate of 5°C / min in an air atmosphere, and kept warm for 2 hours to perform an oxidation reaction. After the reaction is completed, the product is cooled to room temperature with the furnace to obtain Hf6Ta2O 17 Powder. Among them, (Hf 0.6 Ta 04 )(C 0.84 N 0.16 ) The preparation method of the precursor is the same as that in Example 4.

[0064] The prepared Hf6Ta2O 17 The powder was subjected to X-ray diffraction phase analysis (XRD), and the test results are as follows: Fig.12 In the obtained XRD spectrum, each characteristic peak is clear and sharp, corresponding to orthorhombic Hf6Ta2O 17 Specifically, the strong diffraction peaks at 30.4°, 34.1°, 35.2°, 50.6° and 51.5° correspond to the (1171), (002), (0340), (202) and (2340) crystal planes, respectively, indicating that the sample has good crystallinity, confirming the successful preparation of Hf6Ta2O 17 Oxide.

[0065] Fig.13 Hf6Ta2O 17 Scanning electron microscope (SEM) image of the powder. Fig.13 (a) The oxidation products are shown to be in the shape of exploded firecrackers and irregular shapes, with a size of about 0.9-1.8 µm, which helps to increase the specific surface area of ​​the material; Fig.13 (b) shows that the surface of the oxidation product is composed of obvious and compact nanoparticles with a particle size of about 15-25 nm. The compact nanoparticle structure not only increases the surface active sites of the material, but also may enhance the density of the material, improve its high temperature phase stability and anti-CMAS corrosion performance.

[0066] The Hf6Ta2O 17 The powders were subjected to energy dispersive X-ray spectroscopy (EDS) point analysis, as Fig.14 The EDS results show that the oxidation product contains Hf, Ta, O and C elements, which further confirms that the prepared sample is Hf6Ta2O 17 powder.

[0067] Example 7

[0068] In this embodiment, Hf6Ta2O 17 The preparation method of the powder is as follows: 0.5 Ta 0.5 )(C 0.84 N 0.16 ) carbonitride as a precursor. The precursor is placed in a furnace, heated to 1400°C at a heating rate of 5°C / min in an air atmosphere, and kept warm for 2 hours to perform an oxidation reaction. After the reaction is completed, the product is cooled to room temperature with the furnace to obtain Hf6Ta2O 17 Powder.

[0069] The (Hf 0.5 Ta 0.5 )(C 0.84 N 0.16 ) precursor is prepared as follows: HfC and TaC powders are used as raw materials and metal Co powder is used as flux; (1) HfC and TaC powders are accurately weighed in a molar ratio of 1:1; at the same time, the mass ratio of the total mass of carbide to the mass of metal Co is maintained at 3:7 and mixed until uniform; (2) The mixed powder is pressed into shape using a mold, and then placed in a furnace. In a nitrogen environment, the temperature is raised to 1700°C at a heating rate of 10°C / min and kept at this temperature for 1 hour. After the heat treatment is completed, the product is cooled to room temperature with the furnace to obtain (Hf 0.5 Ta 0.5 )(C 0.84 N 0.16 ) / Co metal-based ceramic block; (3) immersing the obtained ceramic block in a 7.2 mol / L dilute nitric acid solution to dissolve and corrode the Co alloy matrix therein; (4) after the corrosion is completed, filtering, washing and drying for multiple times to obtain (Hf 0.5 Ta 0.5 )(C 0.84 N 0.16 )Carbonitride powder.

[0070] The prepared Hf6Ta2O 17 The powder was subjected to X-ray diffraction phase analysis (XRD), and the test results are as follows: Fig.15 In the obtained XRD spectrum, each characteristic peak is clear and sharp, corresponding to the orthorhombic Hf6Ta2O 17 Specifically, the strong diffraction peaks at 30.4°, 34.1°, 35.2°, 50.6° and 51.5° correspond to the (1171), (002), (0340), (202) and (2340) crystal planes, respectively, indicating that the sample has good crystallinity, confirming the successful preparation of Hf6Ta2O 17 Oxide.

[0071] Example 8

[0072] In this embodiment, Hf6Ta2O 17 The preparation method of the powder is as follows: 0.5 Ta 0.5 )(C 0.78 N 0.22 ) carbonitride as a precursor. The precursor is placed in a furnace, heated to 1400°C at a heating rate of 5°C / min in an air atmosphere, and kept warm for 2 hours to perform an oxidation reaction. After the reaction is completed, the product is cooled to room temperature with the furnace to obtain Hf6Ta2O 17 Powder.

[0073] The (Hf 0.5 Ta 0.5 )(C 0.78 N 0.22 ) precursor preparation method is as follows: HfC and TaC powders are used as raw materials, and metal Co powder is used as flux; (1) HfC and TaC powders are accurately weighed according to a molar ratio of 1:1; at the same time, the mass ratio of the total mass of carbide to the mass of metal Co is maintained at 3:7 and mixed until uniform; (2) After the mixed powder is pressed into shape using a mold, it is moved into a furnace and heated to 1500℃ at a heating rate of 5℃ / min in a nitrogen environment and kept at this temperature for 8h. After the heat treatment is completed, the product is cooled to room temperature with the furnace to obtain (Hf 0.5 Ta 0.5 )(C 0.78 N 0.22 ) / Co metal-based ceramic block; (3) immersing the obtained ceramic block in a 7.2 mol / L dilute nitric acid solution to dissolve and corrode the Co alloy matrix therein; (4) after the corrosion is completed, filtering, washing and drying for multiple times to obtain (Hf 0.5 Ta 0.5 )(C 0.78 N 0.22 )Carbonitride powder.

[0074] The prepared Hf6Ta2O 17 The powder was subjected to X-ray diffraction phase analysis (XRD), and the test results are as follows: Fig.16 In the obtained XRD spectrum, each characteristic peak is clear and sharp, corresponding to the orthorhombic Hf6Ta2O 17 Specifically, the strong diffraction peaks at 30.4°, 34.1°, 35.2°, 50.6° and 51.5° correspond to the (1171), (002), (0340), (202) and (2340) crystal planes, respectively, indicating that the sample has good crystallinity, confirming the successful preparation of Hf6Ta2O 17 Oxide.

[0075] Example 9 In this embodiment, Hf6Ta2O 17 The preparation method of the powder is as follows: 0.5 Ta 0.5 )(C 0.84 N 0.16 ) carbonitride as a precursor. The precursor is placed in a furnace, heated to 1200°C at a heating rate of 5°C / min in an air atmosphere, and kept warm for 2 hours to perform an oxidation reaction. After the reaction is completed, the product is cooled to room temperature with the furnace to obtain Hf6Ta2O 17 Powder. Among them, (Hf 0.5 Ta 0.5 )(C 0.84 N 0.16 ) The preparation method of the precursor is the same as that in Example 7.

[0076] The prepared Hf6Ta2O 17 The powder was subjected to X-ray diffraction phase analysis (XRD), and the test results are as follows: Fig.17 In the obtained XRD spectrum, each characteristic peak is clear and sharp, corresponding to the orthorhombic Hf6Ta2O 17 Specifically, the strong diffraction peaks at 30.4°, 34.1°, 35.2°, 50.6° and 51.5° correspond to the (1171), (002), (0340), (202) and (2340) crystal planes, respectively, indicating that the sample has good crystallinity, confirming the successful preparation of Hf6Ta2O 17 Oxide.

[0077] Fig.18 Hf6Ta2O 17 Scanning electron microscope (SEM) image of the powder. Fig.18 (a) The oxidation products are shown to be in the shape of exploded firecrackers and irregular shapes, with a size of about 1.2 to 2.5 µm, which helps to increase the specific surface area of ​​the material; Fig.18 (b) shows that the surface of the oxidation product is composed of obvious and compact nanoparticles with a particle size of about 60-140 nm. The compact nanoparticle structure not only increases the surface active sites of the material, but also may enhance the density of the material, improve its high temperature phase stability and anti-CMAS corrosion performance.

[0078] Example 10 In this embodiment, Hf6Ta2O 17 The preparation method of the powder is as follows: 0.5 Ta 0.5 )(C 0.78 N 0.22) carbonitride as a precursor. The precursor is placed in a furnace, heated to 1200°C at a heating rate of 5°C / min in an air atmosphere, and kept warm for 2 hours to perform an oxidation reaction. After the reaction is completed, the product is cooled to room temperature with the furnace to obtain Hf6Ta2O 17 Powder. Among them, (Hf 0.5 Ta 0.5 )(C 0.78 N 0.22 ) The preparation method of the precursor is the same as that in Example 8.

[0079] The prepared Hf6Ta2O 17 The powder was subjected to X-ray diffraction phase analysis (XRD), and the test results are as follows: Fig.19 As shown. In the obtained XRD spectrum, each characteristic peak is clear and sharp, corresponding to the orthorhombic Hf6Ta2O 17 Specifically, the strong diffraction peaks at 30.4°, 34.1°, 35.2°, 50.6° and 51.5° correspond to the (1171), (002), (0340), (202) and (2340) crystal planes, respectively, indicating that the sample has good crystallinity, confirming the successful preparation of Hf6Ta2O 17 Oxide.

[0080] Fig. 20 Hf6Ta2O 17 Scanning electron microscope (SEM) image of the powder. Fig. 20 (a) The oxidation products are shown to be in the shape of exploded firecrackers and irregular shapes, with a size of about 0.8 to 2.2 µm, which helps to increase the specific surface area of ​​the material; Fig. 20 (b) shows that the surface of the oxidation product is composed of obvious and compact nanoparticles with a particle size of about 70~150 nm. The compact nanoparticle structure not only increases the surface active sites of the material, but also may enhance the density of the material, improve its high temperature phase stability and anti-CMAS corrosion performance.

[0081] Embodiment 11 In this embodiment, Hf6Ta2O 17 The preparation method of the powder is as follows: 0.5 Ta 0.5 )(C 0.84 N 0.16 ) carbonitride as a precursor. The precursor is placed in a furnace, heated to 1000°C at a heating rate of 5°C / min in an air atmosphere, and kept warm for 2 hours to perform an oxidation reaction. After the reaction is completed, the product is cooled to room temperature with the furnace to obtain Hf6Ta2O 17 Powder. Among them, (Hf 0.5 Ta0.5 )(C 0.84 N 0.16 )The preparation method of the precursor is the same as that in Example 7.

[0082] The prepared Hf6Ta2O 17 The powder was subjected to X-ray diffraction phase analysis (XRD), and the test results are as follows: Fig.21 In the obtained XRD spectrum, each characteristic peak is clear and sharp, corresponding to the orthorhombic Hf6Ta2O 17 Specifically, the strong diffraction peaks at 30.4°, 34.1°, 35.2°, 50.6° and 51.5° correspond to the (1171), (002), (0340), (202) and (2340) crystal planes, respectively, indicating that the sample has good crystallinity, confirming the successful preparation of Hf6Ta2O 17 Oxide.

[0083] Fig. 22 Hf6Ta2O 17 Scanning electron microscope (SEM) image of the powder. Fig. 22 (a) The oxidation products are shown to be in the shape of exploded firecrackers and irregular shapes, with a size of about 0.9-1.9 µm, which helps to increase the specific surface area of ​​the material; Fig. 22 (b) shows that the surface of the oxidation product is composed of obvious and compact nanoparticles with a particle size of about 20-45 nm. The compact nanoparticle structure not only increases the surface active sites of the material, but also may enhance the density of the material, improve its high temperature phase stability and anti-CMAS corrosion performance.

[0084] Example 12 In this embodiment, Hf6Ta2O 17 The preparation method of the powder is as follows: 0.5 Ta 0.5 )(C 0.78 N 0.22 ) carbonitride as a precursor. The precursor is placed in a furnace, heated to 1000°C at a heating rate of 5°C / min in an air atmosphere, and kept warm for 2 hours to perform an oxidation reaction. After the reaction is completed, the product is cooled to room temperature with the furnace to obtain Hf6Ta2O 17 Powder. Among them, (Hf 0.5 Ta 0.5 )(C 0.78 N 0.22 ) The preparation method of the powder is the same as that in Example 8.

[0085] The prepared Hf6Ta2O 17 The powder was subjected to X-ray diffraction phase analysis (XRD), and the test results are as follows: Fig.23 In the obtained XRD spectrum, each characteristic peak is clear and sharp, corresponding to the orthorhombic Hf6Ta2O 17 Specifically, the strong diffraction peaks at 30.4°, 34.1°, 35.2° and 50.6° correspond to the (1171), (002), (0340) and (202) crystal planes, respectively, indicating that the sample has good crystallinity, confirming the successful preparation of Hf6Ta2O 17 Oxide.

[0086] Fig.24 Hf6Ta2O 17 Scanning electron microscope (SEM) image of the powder. Fig.24 (a) The oxidation products are shown to be in the shape of exploded firecrackers and irregular shapes, with a size of about 0.9 to 2.5 µm, which helps to increase the specific surface area of ​​the material; Fig.24 (b) shows that the surface of the oxidation product is composed of obvious and compact nanoparticles with a particle size of about 15-40 nm. The compact nanoparticle structure not only increases the surface active sites of the material, but also may enhance the density of the material, improve its high temperature phase stability and anti-CMAS corrosion performance.

[0087] Embodiment 13 In this embodiment, Hf6Ta2O 17 The preparation method of the powder is as follows: 0.6 Ta 0.4 )(C 0.8 N 0.2 ) carbonitride as a precursor. The precursor is placed in a furnace, heated to 1000°C at a heating rate of 5°C / min in an air atmosphere, and kept warm for 5 hours to perform an oxidation reaction. After the reaction is completed, the product is cooled to room temperature with the furnace to obtain Hf6Ta2O 17 Powder.

[0088] The (Hf 0.6 Ta 0.4 )(C 0.8 N 0.2 ) precursor preparation method is as follows: HfC and TaC powders are used as raw materials, and metal Co powder is used as flux; (1) HfC and TaC powders are accurately weighed according to a molar ratio of 1.5:1; at the same time, the mass ratio of the total mass of carbide to the mass of metal Co is maintained at 3:7 and mixed until uniform; (2) After the mixed powder is pressed into shape using a mold, it is moved into a furnace and heated to 1600℃ at a heating rate of 8℃ / min in a nitrogen environment and kept at this temperature for 4h. After the heat treatment is completed, the product is cooled to room temperature with the furnace to obtain (Hf 0.6 Ta 0.4 )(C0.8 N 0.2 ) / Co metal-based ceramic block; (3) immersing the obtained ceramic block in a 7.2 mol / L dilute nitric acid solution to dissolve and corrode the Co alloy matrix therein; (4) after the corrosion is completed, filtering, washing and drying for multiple times to obtain (Hf 0.6 Ta 0.4 )(C 0.8 N 0.2 )Carbonitride powder.

[0089] Embodiment 14 In this embodiment, Hf6Ta2O 17 The preparation method of the powder is as follows: 0.6 Ta 0.4 )(C 0.8 N 0.2 ) carbonitride as a precursor. The precursor is placed in a furnace, heated to 1500°C at a heating rate of 5°C / min in an air atmosphere, and kept warm for 1 hour to perform an oxidation reaction. After the reaction is completed, the product is cooled to room temperature with the furnace to obtain Hf6Ta2O 17 Powder. Among them, (Hf 0.6 Ta 0.4 )(C 0.8 N 0.2 ) The preparation method of the powder is the same as that in Example 13.

Claims

1. A hafnium tantalate (Hf 6 Ta 2 O 17 ) powder preparation method. The characteristic is: (Hf x Ta 1-x )(C y N 1-y ) (x=0.5~0.8, y=0.78~0.84) carbonitride is used as the precursor. The precursor is placed in a furnace, heated to 1000℃~1500℃ at a heating rate of 5℃ / min in an air atmosphere by a one-step oxidation method, and kept warm for 1~5 hours to carry out the oxidation reaction. After the reaction is completed, the product is cooled to room temperature with the furnace to obtain Hf 6 Ta 2 O 17 Powder.

2. The method according to claim 1, wherein the preparation method of (Hf, Ta) (C, N) powder is as follows: HfC and TaC powders are used as raw materials and metal Co powder is used as flux; (1) HfC and TaC powders are weighed according to a predetermined molar ratio (1-4):1; while ensuring that the total mass of carbide and the mass ratio of metal Co are maintained at 3:7 and mixed until uniform; (2) The mixed powder is pressed into a shape and placed in a furnace, and heated to 1500-1700°C at a heating rate of 5-10°C / min and kept warm for 1-8 hours under a nitrogen environment. After the heat treatment is completed, the product is cooled to room temperature with the furnace to obtain a (Hf, Ta) (C, N) / Co metal-based ceramic block; (3) The obtained ceramic block is immersed in a dilute nitric acid solution to dissolve the Co alloy matrix; (4) After filtering, washing and drying, (Hf, Ta) (C, N) carbonitride powder is obtained.

Citation Information

Cited By

  • Single-phase (Hf, Ta) (C, N) transition metal carbonitride powder as well as preparation method and application thereof

    CN119263840A