Low-cost low-carbon-emission silicon carbide ceramic-based composite material and preparation method thereof
Through the impregnation-curing-pyrolysis-sintering cycle process using polycarbosilane as the precursor, the problems of high preparation cost and complex process of silicon carbide ceramic composite materials are solved, and the preparation of high performance, low cost and low carbon emissions are achieved Methods, improve the strength and consistency of the material.
Patent Information
- Application Number
- CN202411139215.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-20
AI Technical Summary
The existing preparation methods for silicon carbide ceramic matrix composites are costly, complex in processes and difficult to guarantee performance consistency, which limits their large-scale commercial applications.
Polycarbosilane is used as the precursor to prepare silicon carbide ceramic-based composite materials through impregnation-curing-pyrolysis-sintering cycle process, improving the mechanical properties and thermal stability of the material, reducing material costs, and simplifying the process flow.
It significantly improves the strength and fracture strain of composite materials, reduces cost and carbon emissions, shortens manufacturing cycle and energy consumption, and improves performance consistency.
Abstract
Description
Technical Field
[0001] The invention relates to a ceramic-based composite material and a preparation method thereof, and in particular to a low-cost and low-carbon emission silicon carbide ceramic-based composite material and a preparation method thereof. Background Art
[0002] Silicon carbide ceramic matrix composites are known for their high hardness, low density, good oxidation resistance and high temperature resistance, and show broad application prospects in aerospace, automotive industry, national defense security, energy and electronic devices. Traditional preparation methods are usually costly and complex, which to some extent limits their large-scale commercial application. Therefore, exploring a low-cost and efficient preparation method for silicon carbide ceramic matrix composites has important theoretical and practical value.
[0003] Existing technologies and their limitations: Currently, the technologies used to prepare silicon carbide ceramic-based composites mainly include precursor organic polymer infiltration and pyrolysis (PIP), chemical vapor infiltration (CVI), reactive melt infiltration (RMI), etc. These technologies have their own characteristics, but also have certain limitations.
[0004] PIP is an organic precursor-based impregnation-curing-pyrolysis process that can effectively prepare composite materials with complex shapes and structures. This method is easy to operate and suitable for large-scale production, but because it requires multiple cycles of treatment, the entire preparation process is long and the material cost is relatively high.
[0005] CVI deposits silicon carbide ceramic materials in porous preforms through chemical vapor reaction, which can precisely control the microstructure of the material. However, the CVI process usually takes a long time to complete and has high requirements for equipment, resulting in increased costs.
[0006] RMI uses liquid silicon metal as an intermediate medium to react the metal with the ceramic fiber preform at high temperature to generate the required composite material. This method can complete the preparation in a relatively short time, but due to the high siliconization temperature of 1400-1600℃, it causes great damage to the silicon carbide fiber and the overall cost is still high.
[0007] Although the above technologies have made some progress in the preparation of silicon carbide ceramic matrix composites, they still face some key challenges:
[0008] Cost issue: Existing preparation methods usually require the use of expensive raw materials and complex equipment, resulting in high cost of finished products.
[0009] Process complexity: Some technologies such as CVI require a long deposition process, which increases the manufacturing cycle and energy consumption.
[0010] Performance consistency: How to maintain the consistency and reliability of material performance while reducing costs is also an important issue. Summary of the invention
[0011] In view of the above background, the present invention aims to propose a PIP technology using polycarbosilane as a precursor to prepare high-performance, low-cost silicon carbide ceramic-based composites through a cyclic process of impregnation-curing-pyrolysis-sintering. This method can not only reduce material costs, but also improve the mechanical properties and thermal stability of the material, providing a new way for the industrial production of high-performance composite materials.
[0012] The invention is characterized in that the fiber in the composite material accounts for 50-90% of the total volume, the silicon carbide matrix accounts for 7-45% of the total volume, the tensile strength is 300-400MPa, and the fracture strain is 0.5-1.5%.
[0013] The present invention is characterized in that the preparation method of the composite material adopts polycarbosilane as a precursor and prepares a high-performance silicon carbide ceramic-based composite material through a cycle process of impregnation-curing-pyrolysis-sintering. The preparation method comprises the following steps in order: (1) impregnating the precursor polycarbosilane into a preform; (2) curing and cross-linking treatment at 200-400°C for 1-5 hours; (3) pyrolysis at 600-1000°C for 1-5 hours; (4) repeating steps (1)(2)(3) for 1-5 short cycles; (5) sintering at 1000-1250°C for 1-3 hours; (6) repeating steps (1)(2)(3)(4)(5) for 1-6 long cycles to obtain a low-cost and low-carbon emission silicon carbide ceramic-based composite material.
[0014] Compared with existing materials and technologies, the present invention has the following beneficial effects: (1) The fiber volume fraction is high, the strength of the composite material is increased by 150-200%, and the fracture strain is increased by 200-300%; (2) The fiber volume fraction is high, the amount of polycarbosilane used is reduced, and the cost of the composite material is reduced by 30-50%; (3) The fiber volume fraction is high, and the performance consistency of the composite material is improved; (4) The number of cycles of impregnation-curing-pyrolysis-sintering is small, the high-temperature damage of the fiber is small, and the fiber performance is maintained; (5) The total number and total time used for high-temperature sintering of the composite material are shortened by more than 75%, the manufacturing cycle is shortened by 30-60%, the energy consumption cost is reduced by more than 50%, and the carbon emission is reduced by more than 25%, which is a low-carbon emission preparation method. DETAILED DESCRIPTION
[0015] The present invention is further explained below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art are all within the scope of the claims attached to this application.
[0016] Example 1 Bearing pipe material and preparation
[0017] The silicon carbide fiber pipe preform has an inner diameter of 100 mm, an outer diameter of 135 mm, and a length of 100 mm. The inside and outside are fixed with graphite molds. The volume fraction of silicon carbide fiber is 90%, and it is tightly wound by fine fiber cloth. The preform is first placed in a polycarbosilane solution, (1) impregnated with a pressure of 3 MPa for 2 hours; (2) then cured at 300°C for 2 hours; (3) then pyrolyzed at 600°C for 1 hour; (4) the above impregnation-curing-pyrolysis process is repeated for one cycle; then (5) sintered at 1150°C for 2 hours; (6) the above steps (1)(2)(3)(4)(5) are repeated for one cycle to obtain a low-cost composite material. The sintering temperature of the second step (5) is 1200°C and maintained for 3 hours. After the first step (5) is completed, demoulding is performed, and the preform is rough-machined to obtain the required surface size; after the step (6) is completed, the surface is finely machined to obtain the required bearing pipe. The composite material has a tensile strength of 380 MPa and a fracture strain of 1.5%.
[0018] Example 2 Brake disc materials and preparation
[0019] The carbon fiber non-woven fabric has an inner diameter of 200 mm, an outer diameter of 300 mm, and a thickness of 20 mm. The inside and outside of the non-woven fabric are fixed with graphite molds. The volume fraction of the carbon fiber is 45±5%, and the preform is formed by non-woven bonding and puncture. First, the preform is placed in a polycarbosilane solution, (1) vacuum impregnated for 2 hours; (2) then cured at 400°C for 2 hours; (3) then pyrolyzed at 800°C for 1 hour; (4) the above impregnation-curing-pyrolysis process is repeated for 5 cycles; (5) sintered at 1250°C for 2 hours; (6) the above steps (1)(2)(3)(4)(5) are repeated for 5 cycles to obtain a low-cost composite material. After the third step (5) is completed, the preform is demoulded and processed to obtain the required surface size; after the step (6) is completed, the surface is finely processed to obtain the required brake disc component. The composite material has a tensile strength of 320 MPa and a fracture strain of 0.7%.
[0020] Example 3 Blade materials and preparation
[0021] The silicon carbide fiber blade preform is 80mm long, 50mm wide and 10mm thick. It is fixed with graphite molds inside and outside. The volume fraction of silicon carbide fiber is 60±5%. It is made by three-dimensional four-way weaving of small-tow silicon carbide fiber. The preparation includes 4 long cycles, which are as follows:
[0022] The first long loop:
[0023] (1) Place the preform in a polycarbosilane solution and vacuum impregnate for 1 hour; (2) Then cure at 400°C under normal pressure for 5 hours; (3) Then pyrolyze at 600°C for 1 hour; (4) Repeat the above impregnation-curing-pyrolysis process for 5 short cycles; (5) Sinter at 1000°C for 3 hours; (6) Perform a second long cycle.
[0024] The second long loop:
[0025] (1) After the first long cycle, the preform is placed in a polycarbosilane solution and vacuum impregnated at 1 MPa for 2 hours; (2) then cured at 350°C for 3.5 hours; (3) then pyrolyzed at 700°C for 1.5 hours; (4) the above impregnation-curing-pyrolysis process is repeated for 4 short cycles; (5) sintered at 1100°C for 3 hours; (6) the third long cycle is performed.
[0026] Demolding and rough processing are carried out to process the hard shell on the surface, which is conducive to further impregnation and densification of the interior of the blade.
[0027] The third long loop:
[0028] (1) After the second long cycle, the preform is placed in a polycarbosilane solution and vacuum impregnated at 2 MPa for 3 hours. (2) It is then cured at 300°C for 2 hours. (3) It is then pyrolyzed at 800°C for 1 hour. (4) The above impregnation-curing-pyrolysis process is repeated for 2 short cycles. (5) It is sintered at 1150°C for 2 hours. (6) A fourth long cycle is performed.
[0029] The fourth long loop:
[0030] (1) After the third long cycle, the preform is placed in a polycarbosilane solution and vacuum impregnated at 3 MPa for 4 hours; (2) then cured at 400°C for 1 hour; (3) then pyrolyzed at 900°C for 0.5 hours; (4) the above impregnation-curing-pyrolysis process is repeated for one short cycle; (5) sintered at 1250°C for 2 hours to obtain the desired composite material.
[0031] Finishing and surface CVD silicon carbide coating treatment are performed.
[0032] The composite material has a tensile strength of 350MPa and a fracture strain of 1.0%, reducing costs by 30% and carbon emissions by 25% compared to traditional methods.
Claims
1. A low-cost, low-carbon emission silicon carbide ceramic matrix composite material consisting of fiber and silicon carbide. Features The fiber in the composite material accounts for 50-90% of the total volume of the composite material, the silicon carbide matrix accounts for 7-45% of the total volume, the tensile strength is 300-400MPa, and the fracture strain is 0.5-1.5%.
2. A method for preparing a low-cost, low-carbon emission silicon carbide ceramic-based composite material, using polycarbosilane as a precursor, and preparing a high-performance silicon carbide ceramic-based composite material through an impregnation-curing-pyrolysis-sintering cycle process. Features The method comprises the following steps in order: (1) impregnating the precursor polycarbosilane into the preform by vacuum impregnation and pressure impregnation; (2) curing and cross-linking treatment at 200-400°C for 1-5 hours; (3) pyrolysis at 600-1000°C for 1-5 hours; (4) repeating steps (1)(2)(3) for 1-5 short cycles; (5) sintering at 1000-1250°C for 1-3 hours; (6) repeating steps (1)(2)(3)(4)(5) for 1-6 long cycles to obtain a low-cost and low-carbon emission silicon carbide ceramic-based composite material.
Citation Information
Patent Citations
Low-temperature preparation method of C / SiC ceramic matrix composite material
CN101224988A
SiCf / SiC composite material and preparation method thereof
CN102898171A
Method for preparing self-healing silicon carbide ceramic-based composite material
CN102910927A
Rapid preparation method for C / SiC composite material
CN105016759A
High-strength and high-toughness silicon carbide fiber reinforced silicon carbide ceramic-based composite material preparation method
CN106977217A