Durable concrete-based anti-corrosion and anti-fouling material and preparation method thereof

By constructing a hydrophobic antifouling coating on a concrete substrate, and utilizing plasma-modified and nano-titanium dioxide antifouling coatings, the problems of low antifouling efficiency and environmental pollution in marine facilities have been solved, achieving durable and environmentally friendly antifouling effects.

CN118878348APending Publication Date: 2024-11-01MINDONG HYDROPOWER DEV CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411091251.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing technologies for preventing marine organisms from attaching to marine facilities are inefficient and cause environmental pollution, especially when applied to concrete substrates, where research is limited.

Method used

By plasma-modifying the surface of a concrete substrate, an epoxy asphalt anti-corrosion coating and a mixed nano-titanium dioxide and methacrylate block copolymer antifouling coating are applied, constructing a hydrophobic surface and a dynamic micro-nano elastomer protrusion structure to form an antifouling coating.

Benefits of technology

It achieves long-term prevention of marine organism attachment in marine environments, has good coating durability, is environmentally friendly and non-toxic, and reduces the risk of facility corrosion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878348A_ABST
    Figure CN118878348A_ABST
Patent Text Reader

Abstract

The invention relates to a durable concrete-based anti-corrosion and anti-fouling material and a preparation method thereof.The preparation method comprises the following specific steps that firstly, a plasma technology is used for etching the surface of concrete, the binding force of a coating and the concrete is improved, then epoxy asphalt is used for coating the surface of the concrete, drying is conducted, and the concrete has a waterproof function; then carrying out plasma treatment on the surface; and finally, coating the surface of the concrete base material with a mixture of the methacrylate block copolymer, the nano titanium dioxide and the graphene, and drying. The cured coating has low surface energy, marine organisms are difficult to attach to the surface of the coating, and the coating easily falls off under the action of water flow or other external forces even if the marine organisms are not firmly attached to the surface of the coating. Nanoscale titanium dioxide can greatly improve the performance of the coating, titanium dioxide has very strong oxidation ability under illumination conditions, can decompose a lot of organic pollutants, and can destroy the tissues of marine organisms to achieve the purpose of preventing and removing marine organisms. The antifouling paint can be applied to long-acting antifouling of marine facilities such as ship bottoms, offshore platforms, navigation marks, hydraulic steel gates and the like, and is used for preventing marine organism fouling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This technical solution involves the technical field of surface modification of concrete materials, and its application mainly involves the field of preventing biological attachment of marine facilities. Background Art

[0002] Seawater pumped storage technology uses the ocean as an upper or lower reservoir, with a small water level fluctuation, which reduces the construction of reservoirs and their investment costs, and solves the problems of freshwater resource utilization and environmental damage in traditional pumped storage power stations. China has extremely rich marine resources and has great potential in the development and utilization of seawater pumped storage technology. However, seawater is rich in nutrients, and marine organisms grow vigorously and are very easy to grow and attach to various equipment and facilities in power stations, causing boarding and corrosion to the facilities, thereby affecting the operation of the facilities and even damaging the equipment in severe cases. Therefore, it is necessary to carry out anti-fouling treatment on the infrastructure materials of seawater pumped storage power stations.

[0003] At present, the main anti-fouling methods include mechanical methods, chemical methods and physical methods. Mechanical methods generally refer to manual removal, which is time-consuming, labor-intensive and inefficient. Chemical methods mainly involve anti-fouling coating treatment on the outer surface of the equipment. Traditional chemical anti-fouling coatings are gradually being eliminated due to the release of toxic substances. Physical methods mainly use materials with low surface energy and self-cleaning functions to resist the attachment of fouling organisms, but the long-term anti-fouling effect is not good. At present, anti-fouling and anti-attachment coatings are mostly applied to metal ship surfaces, and there is little research on their application on concrete substrates. Summary of the invention

[0004] The purpose of the present invention is to provide a physical antifouling technology that is easy to operate, low in cost, non-toxic and pollution-free, and to prepare a durable concrete-based anticorrosion and antifouling material. The preparation process is environmentally friendly and harmless, and the preparation process is simple.

[0005] In order to achieve the above-mentioned purpose, the present invention provides the following technical solutions: a durable concrete-based anticorrosion and antifouling material and preparation method, firstly treating the surface of the concrete substrate, modifying the surface by plasma technology, improving the substrate and the coating, and then coating the concrete surface with epoxy asphalt to make the concrete have anticorrosion function, and finally coating the methacrylate block copolymer and nano titanium dioxide mixture on the surface of the concrete substrate, and then drying to obtain the anticorrosion and antifouling concrete material, which is specifically as follows: 1) Surface treatment of concrete materials, selecting concrete materials in accordance with the standard requirements of GB50204-2015 "Concrete Structure Engineering Construction Quality Acceptance Code", first removing the oil, soluble salt, floating ash, moisture and other dirt on the surface of the concrete material, and then treating it by high-pressure water gun, shot blasting, sand blasting, grinding and other methods, and the surface roughness is not less than 50 μm. 2) Plasma treatment of concrete, plasma surface modification treatment of concrete under the conditions of 200 W discharge power, oxygen atmosphere and 90 s, 120 s and 150 s treatment time to improve the bonding strength between the coating and the concrete. 3) Anti-corrosion treatment of concrete materials: apply the epoxy asphalt anti-corrosion coating on the surface of the concrete material by brushing, dry it at 50°C for 24 hours, repeat the operation 2 to 3 times, obtain an anti-corrosion structure, and the coating thickness is 300 to 400 μm. 4) Plasma treatment of the anti-corrosion layer: plasma treat the anti-corrosion layer with the same parameters as in step 2). 5) Preparation of anti-corrosion and anti-fouling concrete materials: mix 10 to 15 wt.% nano titanium dioxide and methacrylate block copolymer, apply the mixed anti-fouling coating on the surface of the anti-corrosion coating by brushing, dry it at 50°C for 24 hours, repeat the operation again, and the coating thickness is 100 to 200 μm, so that the concrete material has an anti-fouling effect. Furthermore, the type of the concrete material can be cement concrete, asphalt concrete, etc.

[0006] The outer layer of the present invention constructs a hydrophobic surface, and at the same time constructs a micro-nano elastomer protrusion structure of different forms. The protrusion structure swings with the action of water flow, forming a dynamic surface on the surface of the substrate. For marine organisms close to its surface, it actively bounces off, which has a "camouflage and misleading" effect on the organisms, preventing them from attaching to the surface. The cured coating has low surface energy, and it is difficult for marine organisms to attach to its surface. Even if they attach, they are not firm and can easily fall off under the action of water flow or other external forces. Nano-scale titanium dioxide can greatly improve the performance of the coating. Since titanium dioxide has a strong oxidation ability under light conditions, it can decompose many organic pollutants. For marine organisms, it can destroy their tissues and achieve the purpose of preventing and removing marine organisms. It can be applied to the long-term anti-fouling of marine facilities such as ship bottoms, offshore platforms, navigation marks, hydraulic steel gates, etc., to prevent marine organisms from fouling. BRIEF DESCRIPTION OF THE DRAWINGS

[0007] Figure 1Shows a structural diagram of the present invention; In the accompanying drawings: 1-concrete material, 2-anti-corrosion coating, 3-anti-fouling coating. DETAILED DESCRIPTION

[0008] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail in conjunction with the embodiments below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In view of the problems existing in the prior art, the present invention provides a method for preparing a durable concrete-based anticorrosion and antifouling material, and the present invention is described in detail in conjunction with the accompanying drawings below.

[0009] Example 1: Figure 1 As shown, the method for preparing the durable concrete-based anticorrosion and antifouling material provided in the embodiment of the present invention comprises: S1: Select concrete that meets the requirements of GB50204-2015 "Concrete Structure Engineering Construction Quality Acceptance Code", first remove oil, soluble salt, floating dust, moisture and other contaminants on the surface, and then use high-pressure water gun, shot blasting, sand blasting, grinding and other methods to make its surface roughness not less than 50 μm.

[0010] S2: Plasma surface modification treatment was performed under the conditions of a discharge power of 200 W, an oxygen atmosphere, and a treatment time of 120 s.

[0011] S3: Apply the epoxy asphalt anti-corrosion coating on the surface of the concrete material by brushing, dry it at 50℃ for 24 hours, and repeat the operation 2 to 3 times to obtain an anti-corrosion structure with a coating thickness of 300 to 400 μm.

[0012] S4: Plasma treatment of the anti-corrosion layer is performed using the same parameters as in step S2.

[0013] S5: Mix 13 wt.% nano titanium dioxide and methacrylate block copolymer, apply the mixed antifouling coating on the surface of the anticorrosive coating by brushing, dry at 50℃ for 24 h, and repeat the operation. The coating thickness is 100~200μm, so that the concrete material has an antifouling effect.

[0014] Example 2: Figure 1 As shown, the method for preparing the durable concrete-based anticorrosion and antifouling material provided in the embodiment of the present invention comprises: S1: Select concrete that meets the requirements of GB50204-2015 "Concrete Structure Engineering Construction Quality Acceptance Code", first remove oil, soluble salt, floating dust, moisture and other contaminants on the surface, and then use high-pressure water gun, shot blasting, sand blasting, grinding and other methods to make its surface roughness not less than 50 μm.

[0015] S2: Plasma surface modification treatment was performed under the conditions of a discharge power of 200 W, an oxygen atmosphere, and a treatment time of 90 s.

[0016] S3: Apply the epoxy asphalt anti-corrosion coating on the surface of the concrete material by brushing, dry it at 50℃ for 24 hours, and repeat the operation 2 to 3 times to obtain an anti-corrosion structure with a coating thickness of 300 to 400 μm.

[0017] S4: Plasma treatment of the anti-corrosion layer is performed using the same parameters as in step S2.

[0018] S5: Mix 10 wt.% nano titanium dioxide and methacrylate block copolymer, apply the mixed antifouling coating on the surface of the anticorrosive coating by brushing, dry at 50℃ for 24 h, and repeat the operation. The coating thickness is 100~200μm, so that the concrete material has an antifouling effect.

[0019] Example 3: Figure 1 As shown, the method for preparing the durable concrete-based anticorrosion and antifouling material provided in the embodiment of the present invention comprises: S1: Select concrete that meets the requirements of GB50204-2015 "Concrete Structure Engineering Construction Quality Acceptance Code", first remove oil, soluble salt, floating dust, moisture and other contaminants on the surface, and then use high-pressure water gun, shot blasting, sand blasting, grinding and other methods to make its surface roughness not less than 50 μm.

[0020] S2: Plasma surface modification treatment was performed under the conditions of a discharge power of 200 W, an oxygen atmosphere, and a treatment time of 150 s.

[0021] S3: Apply the epoxy asphalt anti-corrosion coating on the surface of the concrete material by brushing, dry it at 50℃ for 24 hours, and repeat the operation 2 to 3 times to obtain an anti-corrosion structure with a coating thickness of 300 to 400 μm.

[0022] S4: Plasma treatment of the anti-corrosion layer is performed using the same parameters as in step S2.

[0023] S5: Mix 15 wt.% nano titanium dioxide and methacrylate block copolymer, apply the mixed antifouling coating on the surface of the anticorrosion coating by brushing, dry at 50℃ for 24 h, and repeat the operation. The coating thickness is 100~200μm, so that the concrete material has an antifouling effect.

[0024] Effect verification: 1. Different sample blocks prepared by the process of Examples 1-3 were tested, referring to GB / T 10834-2008, using slightly saturated sodium chloride solution, setting the temperature at 37°C, and testing the salt water resistance of the coating for 2000 h.

[0025] 2. Select standard specimens of each sample for coating adhesion test, refer to GB / T 5210-2006, and use adhesion tester to test the pull-off adhesion of coating on concrete.

[0026] 3. Prepare concrete samples with reference to the antifouling method of shallow sea immersion of antifouling paint samples in GB / T 5370-2007. Hang the prepared hanging plate samples under the raft and immerse them in the sea. Regularly inspect and take photos to evaluate the antifouling performance.

[0027] The test samples and the comparison samples were tested according to the above test method, and the test results are shown in Table 1; Table 1 Salt water resistance test Pull-off Adhesion Test Antifouling performance test Example 1 After 2000 hours, the paint film is intact without blistering, peeling or corrosion. 6.73 MPa After 12 months of seawater immersion, there is still no marine organism attachment or paint peeling. Example 2 After 2000 hours, the paint film is intact without blistering, peeling or corrosion. 4.29 MPa The antifouling period is 6-7 months. A small amount of shellfish began to attach around October. Among them, only a small amount of organisms attached to the net knots on the FWD sample, and there was no increase in the number of organisms. Example 3 After 2000 hours, the paint film is intact without blistering, peeling or corrosion. 5.56 MPa After 12 months of seawater immersion, only a small amount of tiny algae attached and no shellfish grew It can be seen from the above table that the sample coating prepared in Example 1 has strong salt water resistance, strong coating adhesion, and good marine antifouling performance, and is a preferred embodiment of the present invention; The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a durable concrete-based anticorrosion and antifouling material, characterized in that: The following steps are involved: 1) Surface treatment of concrete materials: first remove the oil, soluble salt, floating ash, moisture and other dirt on the surface of the concrete material, and then treat it by high-pressure water gun, shot blasting, sand blasting, grinding and other methods. 2) Plasma treatment of concrete: plasma surface modification of concrete is carried out under different discharge power, gas composition and treatment time conditions to improve the bonding strength between the coating and concrete. 3) Anti-corrosion treatment of concrete materials: the anti-corrosion coating is applied to the surface of the concrete material by brushing, dried at 50℃ for 24 hours, and then repeated 2 to 3 times to obtain an anti-corrosion structure. 4) Plasma treatment of anti-corrosion layer: plasma treatment of the anti-corrosion layer with the same parameters in step 2). 5) Preparation of anti-corrosion and anti-fouling concrete materials: the mixed anti-fouling coating is applied to the surface of the anti-corrosion coating by brushing, dried at 50℃ for 24 hours, and then repeated once to make the concrete material produce an anti-fouling effect.

2. The method for preparing a durable concrete-based anticorrosion and antifouling material according to claim 1, characterized in that: In step 1), the type of concrete material may be, but is not limited to, cement concrete, asphalt concrete, etc.

3. The method for preparing a durable concrete-based anticorrosion and antifouling material according to claim 1, characterized in that: In step 1), the concrete material complies with the standard requirements of GB50204-2015 "Concrete Structure Engineering Construction Quality Acceptance Code".

4. The method for preparing a durable concrete-based anticorrosion and antifouling material according to claim 1, characterized in that: In step 1), the surface roughness of the concrete material after grinding is not less than 50 μm.

5. The method for preparing a durable concrete-based anticorrosion and antifouling material according to claim 1, characterized in that: In step 2), the discharge power is 200 W, the treatment time is 90 s, 120 s and 150 s, and the mixed gas is oxygen.

6. The method for preparing a durable concrete-based anticorrosion and antifouling material according to claim 1, characterized in that: In step 2), the equipment used to observe and measure the surface morphology and surface free energy of the concrete after plasma treatment is: an electron scanning microscope and a contact angle meter.

7. The method for preparing a durable concrete-based anticorrosion and antifouling material according to claim 1, characterized in that: In step 3), the concrete material anti-corrosion coating is an epoxy asphalt coating.

8. The method for preparing a durable concrete-based anticorrosion and antifouling material according to claim 1, characterized in that: In step 3), the thickness of the anti-corrosion coating on the concrete material is 300-400 μm.

9. The method for preparing a durable concrete-based anticorrosion and antifouling material according to claim 1, characterized in that: In step 5), the antifouling coating of the concrete material is a mixture of nano titanium dioxide and methacrylate block copolymer.

10. The method for preparing a durable concrete-based anticorrosion and antifouling material according to claim 1, characterized in that: In step 5), the content of nano titanium dioxide in the antifouling coating of the concrete material is 10-15 wt.%.

11. The method for preparing a durable concrete-based anticorrosion and antifouling material according to claim 1, characterized in that: In step 5), the thickness of the antifouling coating on the concrete material is 100-200 μm.

12. The concrete-based anticorrosion and antifouling material obtained according to the preparation method according to any one of claims 1 to 10.