Acrylate polymer, acrylate polymer solution, cross-linked resin, preparation method and application

By copolymerizing acrylate compounds, oxazolinyl compounds and hydrophilic group compounds in a specific proportion, combined with free radical polymerization in water and pH adjustment, the stretching and crossing of acrylate polymer crosslinking resins in the prior art are solved. The problem of insufficient linking performance has achieved high-performance crosslinking resin preparation, which is suitable for a variety of applications and meets environmental standards.

CN118878731APending Publication Date: 2024-11-01SHANGHAI LANGYI FUNCTIONAL MATERIALS
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410914949.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The crosslinking resins made of existing aqueous acrylate polymers and acid-containing proton resins have poor tensile properties and crosslinking properties, and the use of organic solvents leads to environmental protection and cost problems.

Method used

Copolymerization is carried out using acrylate compounds, oxazolinyl compounds and hydrophilic group compounds in a specific proportion, and the pH value is adjusted and the initiator is used to prepare excellent mechanical properties and solvent resistance. and crosslinked with acid-containing proton resin.

Benefits of technology

It significantly improves the tensile properties and solvent resistance of crosslinking resins, improves crosslinking degree, is suitable for coatings, adhesives and biological materials, and has no VOC and meets environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878731A_ABST
    Figure CN118878731A_ABST
Patent Text Reader

Abstract

The invention relates to an acrylate polymer, an acrylate polymer solution, cross-linked resin, a preparation method and application. The acrylate polymer comprises a repetitive unit I, a repetitive unit II and a repetitive unit III, the mass percent of the repetitive unit I is 15%-45%, the mass percent of the repetitive unit II is 25%-45%, and the mass percent of the repetitive unit III is 20%-45%. The acrylate polymer can be used as a cross-linking agent containing acidic proton resin. The acrylate polymer disclosed by the invention has relatively proper glass transition temperature Tg, molecular weight and molecular weight distribution index and good water solubility. And the polymer solution has relatively low viscosity and relatively high storage stability. The cross-linked resin formed by cross-linking the acrylate polymer and the acidic proton-containing resin has excellent tensile property and solvent resistance, has higher cross-linking degree, and has wide application prospects in the aspects of coatings, adhesives, biological materials and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an acrylate polymer, an acrylate polymer solution, a cross-linked resin, a preparation method and an application. Background Art

[0002] Acrylate polymers are copolymers composed of methacrylate, acrylate, and olefin monomers. Compared to other synthetic polymer resins, acrylate polymers offer distinct advantages, including lightfastness, weather resistance, durability, and heat resistance. They exhibit no discoloration at 230°C, excellent acid and alkali corrosion resistance, and possess excellent properties such as transparency and hardness. They are increasingly used in automobiles, home appliances, construction, and plastic products.

[0003] Patent application CN 113906061 A uses a copolymer obtained by copolymerizing a (meth)acrylic acid monomer with an oxazoline-containing monomer as a modifier. When a thermoplastic resin containing acidic protons is used as the thermoplastic resin, the copolymer can be modified while suppressing or preventing degradation of various properties of the thermoplastic resin. However, this technology uses an organic solvent for polymerization, which increases costs, pollutes the environment, and incurs high costs for solvent separation and recovery.

[0004] Patent application CN 106604943 A (meth) acrylic acid C 1-20 The invention involves polymerizing a monoethylenically unsaturated hydrophilic monomer containing at least one sulfonic acid group (-SO3M) (monomer b), and a monoethylenically unsaturated monomer containing at least one oxazoline group (monomer c). However, the resulting polymer exhibits poor tensile and crosslinking properties. Summary of the Invention

[0005] To overcome the technical shortcomings of prior art cross-linked resins made from water-based acrylate polymers and acidic proton-containing resins, such as poor tensile and cross-linking properties, the present invention provides an acrylate polymer, an acrylate polymer solution, a cross-linked resin, a preparation method, and applications. Cross-linking the acrylate polymer and the acidic proton-containing resin of the present invention significantly enhances mechanical properties and significantly improves solvent resistance of the resulting cross-linked resin.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides an acrylate polymer comprising a repeating unit I, a repeating unit II, and a repeating unit III; based on the total mass of the acrylate polymer, the mass percentage of the repeating unit I is 15%-45%, the mass percentage of the repeating unit II is 25%-45%, and the mass percentage of the repeating unit III is 20%-45%;

[0008] The repeating unit I is a repeating unit corresponding to an acrylate compound;

[0009] The repeating unit II is a repeating unit corresponding to an olefinic compound containing at least one oxazoline group;

[0010] The repeating unit III is a repeating unit corresponding to an olefinic compound containing at least one hydrophilic group other than an oxazoline group.

[0011] In the present invention, the structure of the repeating unit I can be shown as formula (I):

[0012]

[0013] In each repeating unit I,

[0014] R1, R2, and R3 are each independently hydrogen, methyl, or ethyl;

[0015] R4 are each independently C1-C 30 of hydrocarbon groups.

[0016] In each repeating unit I, R4 can be independently C1-C 10 an alkyl or cycloalkyl group.

[0017] In certain specific embodiments, in each repeating unit I, R1 and R2 are hydrogen; R3 and R4 are methyl.

[0018] In certain specific embodiments, in each repeating unit I, R1 and R2 are hydrogen; R3 is methyl; and R4 is 1,7,7-trimethylbicyclo[2.2.1]hept-2-yl.

[0019] In the present invention, the structure of the repeating unit II can be shown as formula (II):

[0020]

[0021] In each repeating unit II,

[0022] R5 are each independently hydrogen or methyl;

[0023] R6, R7, R8, and R9 are each independently hydrogen, halogen, C 1-20 Alkyl, C 2-20Alkenyl, C 6-20 Aryl, C 7-32 Arylalkyl, C 1-20 Hydroxyalkyl, C 1-20 aminoalkyl or C 1-20 alkyl halide;

[0024] In each repeating unit II, R6, R7, R8, and R9 can each independently be hydrogen, methyl, or ethyl.

[0025] In certain specific embodiments, in each repeating unit II, R5 is methyl; and R6, R7, R8, and R9 are hydrogen.

[0026] In the present invention, the structure of the repeating unit III can be shown as formula (III):

[0027]

[0028] In each repeating unit III,

[0029] R 10 are each independently hydrogen or methyl;

[0030] Each X group is independently -COONa, -CONH2, -CN, -PhSO3Na or the following groups:

[0031]

[0032] In each X group,

[0033] R 11 、R 12 are each independently hydrogen or methyl;

[0034] n is each independently 1-100;

[0035] In each repeating unit III, n can be independently 6-50.

[0036] In the present invention, in the acrylic ester polymer, the repeating unit I, the repeating unit II and the repeating unit III may be randomly distributed.

[0037] In the present invention, the number average molecular weight of the acrylate polymer may be 5000-70000 g / mol, preferably 10000-40000 g / mol, more preferably 18000-28000 g / mol, for example, 18101 g / mol, 19547 g / mol, 19568 g / mol, 19886 g / mol, 20356 g / mol, 21520 g / mol, 22013 g / mol, 24635 g / mol, 24851 g / mol, 25436 g / mol, 26710 g / mol or 27604 g / mol.

[0038] In the present invention, the molecular weight distribution index (PDI) of the acrylic ester polymer may be less than 1.70, preferably 1.4-1.7, for example, 1.50, 1.52, 1.53, 1.54, 1.55, 1.56, 1.57, 1.63 or 1.68.

[0039] In the present invention, the glass transition temperature Tg of the acrylic ester polymer may be 5-85°C, preferably 40-70°C.

[0040] In the present invention, “in each ..., ... are each independently ...” means that in the molecular chain of the acrylic ester polymer, in different repeating units represented by the same general formula, the groups represented by the same symbol may be the same or different.

[0041] For example, "In each repeating unit I, R1 is independently hydrogen, methyl, or ethyl" means that in the molecular chain of the acrylate polymer, R1 in different repeating units I represented by formula (I) may be the same or different. Similarly, each repeating unit II and each repeating unit III has the same meaning.

[0042] For example, it is necessary to explain that "in each X group, R 11 Each independently represents hydrogen or methyl, and n is independently 1-100. "means that in the molecular chain of the acrylate polymer, in different repeating units III represented by formula (I), "n" in each X group may be the same or different; n In, R 11 It can be the same or different.

[0043] In the present invention, the acrylic ester polymer described herein is known to those skilled in the art to inevitably include some residual impurities in the preparation process, such as initiators, chain transfer agents, pH regulators, etc., due to some auxiliary materials used in the preparation process.

[0044] In a second aspect, the present invention provides an acrylate polymer solution comprising water and the acrylate polymer as described above, wherein the solid content of the acrylate polymer solution is 40%-55%, where the percentage is the ratio of the mass of the acrylate polymer to the mass of the acrylate polymer solution, and the pH of the acrylate polymer solution is 7-9.

[0045] In the present invention, the pH of the acrylate polymer solution may be 7.0, 7.4, 7.5, 7.6, 7.9, 8.0, 8.1, 8.2 or 9.0.

[0046] In the present invention, the viscosity of the acrylate polymer solution may be 60-90 mPa·s, for example, 60 mPa·s, 62 mPa·s, 68 mPa·s, 71 mPa·s, 72 mPa·s, 78 mPa·s, 80 mPa·s, 83 mPa·s or 87 mPa·s.

[0047] In a third aspect, the present invention provides a method for preparing an acrylate polymer solution, comprising the following steps:

[0048] S1. In a protective atmosphere, in the presence of an initiator and a chain transfer agent, subjecting raw materials to a free radical polymerization reaction in water; wherein the raw materials include polymerizable monomers, and the polymerizable monomers include monomer A, monomer B, and monomer C; based on the total mass of the polymerizable monomers, the mass percentage of monomer A is 15%-45%; the mass percentage of monomer B is 25%-45%, and the mass percentage of monomer C is 20%-45%; the monomer A is an acrylate compound; the monomer B is an olefinic compound containing at least one oxazoline group; and the monomer C is an olefinic compound containing at least one hydrophilic group other than an oxazoline group;

[0049] S2. Adjust the pH of the reaction system to 7.0-9.0.

[0050] In the present invention, the monomer A may be one or more compounds represented by formula (M-1):

[0051]

[0052] In each type of monomer A, R1, R2, R3 and R4 are independently the same as R1, R2, R3 and R4 as described above.

[0053] In the present invention, the monomer A may be one or more of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-propyl acrylate, n-propyl methacrylate, isopropyl acrylate, isopropyl methacrylate, n-butyl acrylate, n-butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, tert-butyl acrylate, tert-butyl methacrylate, sec-butyl acrylate, sec-butyl methacrylate, n-octyl acrylate, n-octyl methacrylate, tridecyl acrylate, tridecyl methacrylate, dodecyl acrylate, dodecyl methacrylate, stearyl acrylate, stearyl methacrylate, isobornyl acrylate, isobornyl methacrylate, cyclohexyl acrylate, cyclohexyl methacrylate, tert-butylcyclohexyl acrylate, tert-butylcyclohexyl methacrylate, cyclododecyl acrylate and cyclododecyl methacrylate.

[0054] In the present invention, if the content of monomer A is too low, the resistance of the polymer will be reduced; if it is too high, the proportion of monomer B and monomer C that can be polymerized and added cannot be guaranteed, resulting in reduced crosslinking or hydrophilicity.

[0055] In certain specific embodiments of the present invention, the mass percentage of the monomer A is 30%-40%.

[0056] In the present invention, the monomer B may be one or more compounds represented by formula (M-2):

[0057]

[0058] In each type of monomer A, R5, R6, R7, R8 and R9 are independently R5, R6, R7, R8 and R9 as described above;

[0059] In the present invention, the monomer B can be 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-vinyl-4-ethyl-2-oxazoline, 2-vinyl-4,4-dimethyl-2-oxazoline, 2-vinyl-5,5-dimethyl-2-oxazoline, 2-vinyl-4,4,5,5-tetramethyl-2-oxazoline, 2-isopropenyl-2-oxazoline, One or more of oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, 2-isopropenyl-5-methyl-2-oxazoline, 2-isopropenyl-4-ethyl-2-oxazoline, 2-isopropenyl-5-ethyl-2-oxazoline, 2-isopropenyl-4,4-dimethyl-2-oxazoline, 2-isopropenyl-5,5-dimethyl-2-oxazoline and 2-isopropenyl-4,4,5,5-tetramethyl-2-oxazoline.

[0060] In the present invention, if the content of monomer B is too low, the subsequent crosslinking property cannot be guaranteed and sufficient crosslinking cannot be performed; if it is too high, the content of other monomers will be reduced, which will have an adverse effect on water resistance, solvent resistance, etc.

[0061] In certain specific embodiments of the present invention, the mass percentage of the monomer B is 30%-40%.

[0062] In the present invention, the monomer C may be one or more compounds represented by formula (M-3):

[0063]

[0064] In various monomers A, X and R 10 are independently X and R as described above 10 .

[0065] In the present invention, the monomer C may be one or more of acrylic acid and its salts, methacrylic acid and its salts, methoxy polyethylene glycol acrylate, monoesters of acrylic acid and polyethylene glycol, acrylamide, methacrylamide, methacrylonitrile, and sodium styrene sulfonate. The acrylic acid salt may be sodium acrylate or ammonium acrylate. The methacrylic acid salt may be sodium methacrylate or ammonium methacrylate.

[0066] In the present invention, if the content of monomer C is too low, the hydrophilicity of the polymer may be reduced; if it is too low, the content of oxazoline that can undergo addition polymerization cannot be guaranteed.

[0067] In certain specific embodiments of the present invention, the mass percentage of the monomer C is 20%-40%.

[0068] In the present invention, the initiator can be compounded with the reducing agent to form a composite initiator.

[0069] In the present invention, the initiator may be a water-soluble polymerization initiator or an oil-soluble polymerization initiator. The water-soluble polymerization initiator may be a persulfate, such as lithium persulfate, potassium persulfate, sodium persulfate, or ammonium persulfate. The oil-soluble polymerization initiator may be an organic peroxide, such as cumene hydroperoxide, benzoyl peroxide, tert-butyl hydroperoxide, acetyl peroxide, or diisopropylbenzene hydroperoxide.

[0070] In the present invention, the mass of the initiator may be 0.05%-0.8%, for example, 0.6%-1.6%, of the total mass of the polymerization monomers.

[0071] In the present invention, the initiator can be added dropwise into the reaction system in the form of an initiator solution.

[0072] In the present invention, the chain transfer agent may be an alkyl mercaptan, a xanthate compound, a phenolic compound, an allyl compound, a halogenated hydrocarbon compound, a vinyl ether, triphenylethane, pentaphenylethane, acrolein, methacrolein, thioglycolic acid, mercaptosuccinic acid, terpinolene, or α-methylstyrene dimer. The alkyl mercaptan may be n-hexyl mercaptan, n-octyl mercaptan, tert-octyl mercaptan, n-dodecyl mercaptan, tert-dodecyl mercaptan, or n-octadecyl mercaptan. The xanthate compound may be dimethyl xanthate disulfide or diisopropyl xanthate disulfide. The phenolic compound may be 2,6-di-tert-butyl-4-methylphenol or styrenated phenol. The allyl compound may be allyl alcohol. The halogenated hydrocarbon compound may be dichloromethane, dibromomethane, or tetrabromomethane. The vinyl ether may be α-benzyloxystyrene, α-benzyloxyacrylonitrile, or α-benzyloxyacrylamide.

[0073] In the present invention, the mass of the chain transfer agent may be 0.1%-1.0%, for example, 0.3%-0.4%, of the total mass of the polymerizable monomers.

[0074] In the present invention, according to conventional selection in the art, the raw materials may further include one or both of a reducing agent and an emulsifier.

[0075] The reducing agent may be a reducing inorganic acid salt, a reducing carboxylic acid and its salt, a reducing sugar, or an amine. The reducing inorganic acid salt may be a sulfite, a bisulfite, a pyrosulfite, a dithionite, a dithionite, a thiosulfate, a formaldehyde sulfonate, or a benzaldehyde sulfonate. The reducing carboxylic acid may be L-ascorbic acid, isoascorbic acid, tartaric acid, or citric acid. The reducing sugar may be dextrose or sucrose. The amine may be dimethylaniline or triethanolamine.

[0076] The emulsifier is a conventional surfactant, such as an anionic surfactant or a nonionic surfactant. The nonionic surfactant may be a polyethylene glycol alkyl ester, a polyethylene glycol alkylphenyl ether, or a polyethylene glycol alkyl ether. The anionic surfactant may be a sulfate salt of a higher alcohol, an alkylbenzene sulfonate, an alkyldiphenyl oxide disulfonate, an aliphatic sulfonate, an aliphatic carboxylate, a dehydroabietic acid salt, a formalin condensate of naphthalenesulfonic acid, or a sulfate salt of the nonionic surfactant.

[0077] In the present invention, the mass of the water may be 100%-120% of the total mass of the polymerizable monomers.

[0078] In the present invention, the free radical polymerization reaction can be carried out according to conventional operations and conditions of such reactions in the art.

[0079] In the present invention, the protective atmosphere refers to an atmosphere that does not react with the reactants, such as an inert gas or nitrogen.

[0080] In the present invention, the temperature of the free radical polymerization reaction may be 35-95°C, preferably 50-70°C, such as 50°C, 60°C or 70°C.

[0081] In the present invention, the method of adding the raw materials is not particularly limited, and can be collective addition, batch addition, continuous addition or power feed addition.

[0082] Wherein, when adding in batches, the initiator can be added in three batches.

[0083] In certain specific embodiments of the present invention, the mass ratio of the first batch of initiators, the second batch of initiators and the third batch of initiators may be 1:0.1:0.5 or 1:0.2:0.4.

[0084] Wherein, when adding in batches, the monomers can be added in two batches.

[0085] In certain specific embodiments of the present invention, the mass ratio of the first batch of monomers to the second batch of monomers may be 1:2, 1:3 or 1:5.

[0086] Wherein, when adding in batches, the chain transfer agent can be added in two batches.

[0087] In certain specific embodiments of the present invention, the mass ratio of the first batch of chain transfer agent to the second batch of chain transfer agent may be 1:1 or 1:2.

[0088] When adding in batches, the temperature of the free radical polymerization reaction of each batch of raw materials may be the same or different.

[0089] In the present invention, the pH adjustment can be performed using a pH adjuster. The pH adjuster can be a conventional alkaline substance, such as sodium hydroxide, potassium hydroxide, aqueous ammonia, sodium bicarbonate, or sodium carbonate. The pH adjuster can be used in an amount of 0.5% to 2.5% of the total mass of the polymerizable monomers, such as 0.5%, 1%, 2%, or 2.5%.

[0090] In the present invention, the pH of the reaction system can be adjusted to 7.0, 7.4, 7.5, 7.6, 7.9, 8.0, 8.1, 8.2 or 9.0.

[0091] In a fourth aspect, the present invention provides an acrylate polymer prepared by the above-mentioned method for preparing an acrylate polymer.

[0092] In a fifth aspect, the present invention provides a method for preparing an acrylate polymer, comprising the following steps: drying the acrylate polymer solution as described above.

[0093] In a sixth aspect, the present invention provides an acrylate polymer prepared by the above-mentioned preparation method of the acrylate polymer.

[0094] In a seventh aspect, the present invention provides a use of the above-mentioned acrylate polymer as a cross-linking agent for an acidic proton-containing resin.

[0095] In the present invention, the acidic proton-containing resin may be a polyarylacetylene resin (PAA resin) or a waterborne polyurethane resin (PU resin).

[0096] In an eighth aspect, the present invention provides a cross-linked resin, the raw materials of which include an acidic proton-containing resin and the acrylate polymer described above.

[0097] In the present invention, the acidic proton-containing resin may be a polyarylacetylene resin (PAA resin) or a waterborne polyurethane resin (PU resin).

[0098] In the present invention, the mass ratio of the acidic proton-containing resin to the acrylate polymer may be (50-100):(2-6).

[0099] In the present invention, the cross-linking degree of the cross-linked resin may be greater than 88%, for example, 89%, 90%, 91% or 92%.

[0100] In the present invention, the elongation at break of the cross-linked resin may be greater than 800%, for example, 850%, 860%, 868%, 880%, 883%, 885%, 891%, 895%, 897%, 901%, 910% or 951%.

[0101] In the present invention, the tensile strength of the cross-linked resin may be greater than 35 MPa, for example, 38.3 MPa, 38.4 MPa, 39.0 MPa, 39.1 MPa, 39.4 MPa, 39.5 MPa, 40.1 MPa, 40.2 MPa, 40.5 MPa, 41.0 MPa or 42.6 MPa.

[0102] In a ninth aspect, the present invention provides an application of the cross-linked resin described above in the field of coatings, adhesives or biomaterials.

[0103] Without violating the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain preferred embodiments of the present invention.

[0104] The reagents and raw materials used in the present invention are commercially available.

[0105] The positive progress effect of the present invention is:

[0106] (1) The acrylate polymer of the present invention has a relatively suitable glass transition temperature Tg, a relatively suitable molecular weight and molecular weight distribution index, and good water solubility;

[0107] (2) The acrylate polymer of the present invention has a low viscosity and a high storage stability in the polymer solution (can be stored at 50° C. for at least 7 days);

[0108] (3) The acrylic acid ester polymer of the present invention is VOC-free during preparation, thus meeting the requirements of environmental protection development;

[0109] (4) The cross-linked resin formed by cross-linking the acrylic ester polymer of the present invention and the acidic proton-containing resin has excellent tensile properties and solvent resistance, and has a high degree of cross-linking, and has broad application prospects in coatings, adhesives, biomaterials, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0110] Figure 1 This is the GPC spectrum of the polymer prepared in Example 1;

[0111] Figure 2 This is the GPC spectrum of the polymer prepared in Comparative Example 8;

[0112] Figure 3 This is the infrared spectrum of the polymer prepared in Example 1. DETAILED DESCRIPTION

[0113] The present invention is further illustrated by way of examples below, but the present invention is not limited to the scope of the examples. Experimental methods in the following examples where specific conditions are not specified were performed according to conventional methods and conditions, or selected according to the product specifications.

[0114] The reagents or instruments used do not indicate the manufacturer, and are all conventional products that can be purchased through regular channels.

[0115] Methyl methacrylate, isopropenyl oxazoline, sodium acrylate, acrylamide, polyethylene glycol methyl acrylate (Mn-2100), sodium styrene sulfonate, dodecyl mercaptan, potassium persulfate, sodium bicarbonate, and PAA resin (average Mv-450000) in the following examples were all purchased from the Titan Technology Exploration Platform;

[0116] pH meter: Mettler Toledo SevenExcellence S400-Micro

[0117] DSC instrument: Mettler Toledo DSC 3+;

[0118] Rotational viscometer: Shanghai Precision Instrument Co., Ltd. SNB-1

[0119] Gel permeation chromatography (GPC): Agilent 1260 Infinity II

[0120] Examples 1-12 and Comparative Examples 1-9: Preparation of Polymers

[0121] Under an inert gas atmosphere, a polymerization reactor was first charged with 100 g of deionized water and 1.0 g of potassium persulfate and thoroughly stirred. The monomers from Section 1 (Monomer A, Monomer B, and Monomer C) and the other compounds (dodecyl mercaptan and ammonium persulfate) shown in Tables 1-5 were then added all at once, and the polymerization reaction was initiated at 70°C (see Tables 1-5 for specific temperatures).

[0122] After the first stage of polymerization reaction for 2 hours, the monomers from the second stage (Monomer A, Monomer B, and Monomer C) and other compounds (dodecyl mercaptan and ammonium persulfate) shown in Tables 1-5 were added over the next 3 hours. Ammonium persulfate was dissolved in 20g of deionized water and added dropwise simultaneously with the other substances. After the addition was complete, the mixture was maintained at 70°C (specific temperatures are shown in Tables 1-5) for 9 hours to terminate the polymerization reaction.

[0123] After the polymerization reaction is completed, sodium bicarbonate as a pH adjuster shown in Tables 1 to 5 is added, and the mixture is filtered to obtain a polymer solution containing a polymer.

[0124] The raw materials in Examples 1-12 and Comparative Examples 1-9 are shown in Tables 1 to 5 below.

[0125] Table 1 Examples 1-4 Raw materials and amounts (unit: g) and key parameters

[0126]

[0127] Table 2 Examples 5-8 Raw materials and amounts (unit: g) and key parameters

[0128]

[0129] Table 3 Examples 9-12 Raw materials and amounts (unit: g) and key parameters

[0130]

[0131] Table 4 Comparative Examples 1-4 Raw materials and dosage (unit: g) and key parameters

[0132]

[0133] Table 5 Comparative Examples 5-9 Raw materials and dosage (unit: g) and key parameters

[0134]

[0135] The monomer ratios in Examples 1-12 are shown in Table 6 below.

[0136] Table 6 Polymer monomers of Examples 1-12 based on weight percentage of total monomers

[0137]

[0138] Comparative Example 10: Preparation of polymer

[0139] According to the preparation method of P4 polymer in Example 1 in patent application CN 106604943 A (monomers: 104 g n-butyl acrylate, 120 g methyl methacrylate, 32 g 2-acrylamido-2-propanesulfonic acid sodium salt and 64 g isopropenyl oxazoline), a polymer solution containing the polymer was obtained.

[0140] The monomer ratios in Comparative Examples 1-10 are shown in Table 7 below.

[0141] Table 7 Comparative Examples 1-10 Polymer Monomers Based on Total Monomer Weight Percentage

[0142]

[0143] Effect embodiment

[0144] 1. pH determination

[0145] (1) Test objects: polymer solutions obtained in Examples 1-12 and Comparative Examples 1-10.

[0146] (2) Test method: Test in accordance with GB / T 9724-2007.

[0147] (3) Test results: See Table 8-Table 9 for details.

[0148] 2. Conversion rate test

[0149] (1) Test method: Take about 5 g of the polymer solution obtained in Examples 1-12 and Comparative Examples 1-10, record the sample volume as m1, the mass of the clean aluminum foil plate as m2, and dry it at 100°C for 6 hours. Record the mass after drying as m3. Calculate the monomer conversion Y as follows:

[0150] Y=[(m3-m2-m1×W (十二烷基硫醇+过硫酸铵+碳酸氢钠) ) / m1] / W 单体理论固含 ×100%

[0151] Among them, W (十二烷基硫醇+过硫酸铵+碳酸氢钠) =(m 十二烷基硫醇 +m 过硫酸铵 +m 碳酸氢钠 ) / (m a +m b +m c +m 去离子水 +m 十二烷基硫醇 +m 过硫酸铵 +m 碳酸氢钠 )

[0152] W 单体理论固含 =(m a +m b +m c ) / (m a +m b +m c +m 去离子水 +m 十二烷基硫醇 +m 过硫酸铵 +m 碳酸氢钠 )

[0153] (2) Test results:

[0154] Taking Example 1 as an example, the polymer solution obtained by the reaction was taken, and the sample volume was recorded as m1 = 10.0000 g. The mass of the clean aluminum foil plate was m2 = 2.0000 g. The solution was dried at 100°C for 6 hours, and the mass after drying was recorded as m3 = 2.5843 g. The monomer conversion rate Y was calculated as follows:

[0155] W (十二烷基硫醇+过硫酸铵+碳酸氢钠) =(0.1+0.2+0.2+0.4+1) / (30+30+40+100+0.1+0.2+0.2+0.4+1)=0.94%

[0156] W 单体理论固含 =(30+30+40) / (30+30+40+100+0.1+0.2+0.2+0.4+1)=49.53%

[0157] Y 实施例1转化率 =(2.5843-2.0000-10.0000×0.94%) / 49.53%=99%

[0158] The specific results are shown in Tables 8 and 9.

[0159] 3. Viscosity test

[0160] (1) Test objects: polymer solutions obtained in Examples 1-12 and Comparative Examples 1-10.

[0161] (2) Test method: Test in accordance with GB / T 2794-2013.

[0162] (3) Test results: See Table 8-Table 9 for details.

[0163] 4. Tg test

[0164] (1) Test object: Sample obtained by drying during conversion rate test.

[0165] (2) Test method: Test in accordance with GB / T 2794-2013.

[0166] (3) Test results: See Table 8-Table 9 for details.

[0167] 5. Molecular weight and molecular weight distribution index test

[0168] (1) Test object: Sample obtained by drying during conversion rate test.

[0169] (2) Test method: Test in accordance with GB / T 2794-2013.

[0170] (3) Test results: See Tables 8 and 9 for details, where the GPC spectra of the polymers prepared in Example 1 and Comparative Example 8 are shown as follows: Figure 1-2 shown.

[0171] 6. Stability test

[0172] (1) Test method: 10 g of the polymer solutions obtained in Examples 1-12 and Comparative Examples 1-10 were placed in clean, sealed bottles and kept in a 50°C oven for 7 days. After 7 days, the polymer solutions were taken out to check whether stratification or turbidity occurred. If there was no stratification or turbidity, it indicated that the polymer solutions had good stability.

[0173] (2) Test results: See Table 8-Table 9 for details.

[0174] 7. Structural characterization

[0175] (1) Test method: The polymer obtained after drying the polymer solution was tested using the infrared test method commonly used in the art.

[0176] (2) Test results: Figure 3 This is the infrared spectrum of the polymer prepared in Example 1.

[0177] Table 8 Test results of polymer / polymer solution of Examples 1-12

[0178] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 pH 8 7.5 8.2 7.6 7.4 7.9 Conversion rate 99% 99% 99% 99% 98% 99% Viscosity (mPa·s) 78 87 60 71 68 78 Tg(℃) 45 66 55 70 49 48 Number average molecular weight (g / mol) 18101 19568 25436 20356 24851 26710 Molecular weight distribution index 1.50 1.53 1.57 1.68 1.56 1.55 stability Stablize Stablize Stablize Stablize Stablize Stablize Example 7 Example 8 Example 9 Example 10 Example 11 Example 12 pH 8.1 7.5 7.4 7.5 9.0 7.0 Conversion rate 99% 99% 98% 99% 99% 99% Viscosity (mPa·s) 72 83 62 80 72 68 Tg(℃) 45 46 46 80 55 52 Number average molecular weight (g / mol) 19547 27604 24635 21520 19886 22013 Molecular weight distribution index 1.54 1.53 1.54 1.52 1.52 1.63 stability Stablize Stablize Stablize Stablize Stablize Stablize

[0179] Table 9 Comparative Examples 1-10 Polymer / Polymer Solution Test Results

[0180] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 pH 7.7 7.9 8 7.1 6.0 Conversion rate 75% 80% 73% 98% 98% Viscosity (mPa·s) 102 95 87 86 81 Tg(℃) 85 92 100 50 53 Number average molecular weight (g / mol) 30215 25968 28364 27648 31064 Molecular weight distribution index 2.01 2.21 2.13 1.80 2.36 stability turbid turbid turbid Stablize turbid Comparative Example 6 Comparative Example 7 Comparative Example 8 Comparative Example 9 Comparative Example 10 pH 8.2 7.7 7.8 7.1 8.5 Conversion rate 74% 75% 70% 79% 97% Viscosity (mPa·s) 611 593 987 954 109 Tg(℃) 70 69 66 40 71 Number average molecular weight (g / mol) 123650 102543 216796 201244 31254 Molecular weight distribution index 2.13 2.20 1.97 2.16 1.78 stability solidification solidification solidification solidification opaque

[0181] As shown in Table 8, in Examples 1-12, the monomer conversion rate of the polymers was high, and the polymer solutions had good stability and low viscosity.

[0182] As shown in Table 9, in Comparative Examples 1-3, the methyl methacrylate (MMA) content was too high, the monomer conversion rate was low, the water solubility of the polymer was poor, and the polymer solution was unstable.

[0183] As shown in Table 9, in Comparative Example 5, no pH regulator was added, and the pH of the polymer solution was too low, which affected the stability of the polymer solution and reduced its cross-linking effect.

[0184] As shown in Table 9, in Comparative Example 6, the polymerization temperature was too high, resulting in a significant increase in the polymer molecular weight and an increase in the viscosity of the polymer solution.

[0185] As shown in Table 9, in Comparative Example 7, no molecular weight regulator was added, resulting in a significant increase in the molecular weight of the polymer and an increase in the viscosity of the polymer solution.

[0186] As shown in Table 9, in Comparative Example 8, the initiator dosage was too high, resulting in a significant increase in the polymer molecular weight and an increase in the viscosity of the polymer solution.

[0187] As shown in Table 9, in Comparative Example 9, the methyl methacrylate (MMA) content was too low, the monomer conversion rate was low, the water solubility of the polymer was poor, and the polymer solution was unstable.

[0188] As shown in Table 9, in Comparative Example 10, the methyl methacrylate (MMA) content was too high, the water solubility of the polymer was poor, and the polymer solution was not clear and transparent.

[0189] Application Example 1: Crosslinking agent for PAA resin

[0190] Take 50g of PAA resin respectively, add 6g of the polymer solution obtained in Examples 1-12 and Comparative Examples 1-10 respectively, stir and mix evenly, pour into a drying film mold and fill it completely, first keep the temperature at 60°C for 4h, then transfer to a 120°C oven and keep the temperature for 2h to prepare a cross-linked resin.

[0191] Application Example 2: Crosslinking agent for PU-MR871 resin

[0192] 100.0 g of PU-MR871 resin was taken respectively, and 5.0 g of the polymer solution obtained in Examples 1-12 and Comparative Examples 1-10 was added respectively, stirred and mixed evenly, poured into a dumbbell-shaped drying film mold (length 75.0 mm, width 12.5 mm, thickness 2.5 mm) and filled completely. The mixture was dried in a constant temperature and humidity oven (temperature 40°C, humidity >40%) for 48 h to prepare a cross-linked resin.

[0193] Effect application examples

[0194] 1. Cross-linking degree test

[0195] (1) Test method: Weigh about 2g of the cross-linked resin in Application Example 1 and record the weight as W1. Wrap it completely with a 200-mesh filter and place it in water for 24 hours to reflux and dissolve. Weigh the weight of the dried film after dissolution and record it as W2. Calculate its cross-linking degree H.

[0196] H = W2 / W1 × 100%

[0197] (2) Test results:

[0198] Taking Application Example 1 obtained from Example 1 as an example, 50.0 g of PAA resin was taken, 6.0 g of the polymer solution of Example 1 was added, stirred and mixed evenly, poured into a drying mold to be filled completely, first kept at a constant temperature of 60 °C for 4 h, and then transferred to an oven at 120 °C and kept at a constant temperature for 2 h.

[0199] Weigh the weight of the sample W1 = 2.0050 g obtained by the drying treatment in the above steps, wrap it completely with a 200-mesh filter screen, reflux and dissolve it in water for 24 h, weigh the weight of the dried film after dissolution W2 = 1.8051 g, and calculate its crosslinking degree H

[0200] H 实施例1交联度 = 1.8051 / 2.0050 × 100% = 90%

[0201] The specific results are shown in Table 10 - Table 11.

[0202] 2. Solvent resistance test of crosslinked resin

[0203] (1) Test method: Take about 2 g of the crosslinked resin in Application Example 1, record the weight as M1, wrap it completely with a 200-mesh filter screen, reflux and dissolve it in toluene for 24 h, weigh the weight of the dried film after dissolution, record it as M2, and calculate its mass loss rate w

[0204] w = 1 - (M2 / M1 × 100%)

[0205] If w ≤ 5%, it is recorded as √;

[0206] If 5% < w < 90%, it is recorded as O;

[0207] If w ≥ 90%, it is recorded as ×.

[0208] (2) Test results:

[0209] Taking Application Example 1 obtained from Example 1 as an example, take the dried crosslinked sample prepared by the above crosslinking degree test in Application Example 1, with the weight M1 = 2.0015 g, wrap it completely with a 200-mesh filter screen, reflux and dissolve it in toluene for 24 h, weigh the dried film after 24 h of dissolution, with the weight M2 = 0.0401 g, and calculate its mass loss rate w

[0210] Mass loss rate w 实施例1 = 0.0401 / 2.0015 × 100% = 2%, recorded as √

[0211] The specific results are shown in Table 10 - Table 11.

[0212] 3. Elongation at break and tensile strength test

[0213] (1) Test object: the cross-linked resin prepared from the polymer solutions of Examples 1-12 and Comparative Examples 1-10 in Application Example 2.

[0214] (2) Test method: Test in accordance with GB / T528 2009.

[0215] (3) Test results: See Table 10-Table 11 for details.

[0216] Table 10 Test results of cross-linked resins prepared from polymers of Examples 1-12

[0217] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Degree of crosslinking 90% 91% 89% 90% 90% 92% Cross-linked resin resistance √ √ √ √ √ √ Elongation at break 850% 891% 868% 883% 951% 901% Tensile strength MPa 38.3 40.1 39.0 39.4 42.6 40.5 Example 7 Example 8 Example 9 Example 10 Example 11 Example 12 Degree of crosslinking 92% 91% 90% 91% 91% 89% Cross-linked resin resistance √ √ √ √ √ √ Elongation at break 897% 885% 880% 910% 895% 860% Tensile strength MPa 40.2 39.5 39.4 41.0 39.1 38.4

[0218] Table 11 Test results of cross-linked resins prepared from polymers of Comparative Examples 1-10

[0219] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Degree of crosslinking 40% 41% 41% 15% 32% Cross-linked resin resistance O O O × O Elongation at break 702% 710% 715% 615% 639% Tensile strength MPa 27.3 27.8 27.0 21.3 23.8 Comparative Example 6 Comparative Example 7 Comparative Example 8 Comparative Example 9 Comparative Example 10 Degree of crosslinking 12% 16% 9% 7% 84% Cross-linked resin resistance × × × × √ Elongation at break 633% 640% 649% 625% 792% Tensile strength MPa 23.1 24.0 23.7 22.0 34.8

[0220] Among them, the elongation at break of pure PU-MR871 resin is 600% and the tensile strength is 20.9 MPa.

[0221] As shown in Table 10, after the polymers of Examples 1-12 were cross-linked with the acidic proton-containing resin, the mechanical properties were significantly improved, and the solvent resistance of the obtained cross-linked resin was also significantly improved.

[0222] As shown in Table 11, in Comparative Examples 1-3, the methyl methacrylate (MMA) content was too high, and the crosslinking performance of the obtained polymer with the acidic proton resin was significantly lower, that is, the crosslinking degree, solvent resistance and mechanical properties of the obtained crosslinked resin were all reduced.

[0223] As shown in Table 11, in Comparative Example 4, the oxazoline monomer content is too low, and the crosslinking performance of the obtained polymer with the acidic proton-containing resin is significantly lower, that is, the crosslinking degree, solvent resistance and mechanical properties of the prepared crosslinked resin are all reduced.

[0224] As shown in Table 11, in Comparative Example 5, no pH regulator was added, and the crosslinking performance of the obtained polymer with the acidic proton-containing resin was significantly lower, that is, the crosslinking degree, solvent resistance and mechanical properties of the obtained crosslinked resin were all reduced.

[0225] As shown in Table 11, in Comparative Example 6, the polymerization temperature was too high, and the crosslinking performance of the obtained polymer with the acidic proton-containing resin was significantly lower, that is, the crosslinking degree, solvent resistance and mechanical properties of the obtained crosslinked resin were all reduced.

[0226] As shown in Table 11, in Comparative Example 7, no molecular weight regulator was added, and the crosslinking performance of the obtained polymer with the acidic proton-containing resin was significantly lower, that is, the crosslinking degree, solvent resistance and mechanical properties of the obtained crosslinked resin were all reduced.

[0227] As shown in Table 11, in Comparative Example 8, the initiator dosage was too high, and the crosslinking performance of the obtained polymer with the acidic proton-containing resin was significantly lower, that is, the crosslinking degree, solvent resistance and mechanical properties of the obtained crosslinked resin were all reduced.

[0228] As shown in Table 11, in Comparative Example 9, the methyl methacrylate (MMA) content is too low, and the crosslinking performance of the obtained polymer with the acidic proton resin is significantly low, that is, the crosslinking degree, solvent resistance and mechanical properties of the obtained crosslinked resin are all reduced.

[0229] As shown in Table 11, in Comparative Example 10, the methyl methacrylate (MMA) content was too high, and the crosslinking degree and mechanical properties of the obtained polymer and the crosslinked resin prepared from the acidic proton resin were reduced.

Claims

1. An acrylate polymer, characterized in that It comprises a repeating unit I, a repeating unit II and a repeating unit III; based on the total mass of the acrylic ester polymer, the mass percentage of the repeating unit I is 15%-45%, the mass percentage of the repeating unit II is 25%-45%, and the mass percentage of the repeating unit III is 20%-45%; The repeating unit I is a repeating unit corresponding to an acrylate compound; The repeating unit II is a repeating unit corresponding to an olefinic compound containing at least one oxazoline group; The repeating unit III is a repeating unit corresponding to an olefinic compound containing at least one hydrophilic group other than an oxazoline group.

2. The acrylate polymer according to claim 1, characterized in that The structure of the repeating unit I is shown in formula (I): In each repeating unit I, R1, R2, and R3 are each independently hydrogen, methyl, or ethyl; R4 is each independently C1-C 30 The hydrocarbon group; Preferably, in each repeating unit I, R1, R2, R3, and R4 independently satisfy any one of the following conditions ①-③: ① R4 is independently C1-C 10 An alkyl or cycloalkyl group; ②R1 and R2 are hydrogen; R3 and R4 are methyl; ③ R1 and R2 are hydrogen; R3 is methyl; R4 is 1,7,7-trimethylbicyclo[2.2.1]hept-2-yl; And / or, the structure of the repeating unit II is as shown in formula (II): In each repeating unit II, R5 are each independently hydrogen or methyl; R6, R7, R8, and R9 are each independently hydrogen, halogen, C 1-20 Alkyl, C 2-20 Alkenyl, C 6-20 Aryl, C 7-32 Arylalkyl, C 1-20 Hydroxyalkyl, C 1-20 Aminoalkyl or C 1-20 Haloalkyl; Preferably, in each repeating unit II, R5, R6, R7, R8, and R9 satisfy the following conditions ① or ②: ① R6, R7, R8, R9 are each independently hydrogen, methyl or ethyl; ②R5 is methyl; R6, R7, R8, R9 are hydrogen; And / or, the structure of the repeating unit III is as shown in formula (III): In each repeating unit III, R 10 are each independently hydrogen or methyl; The X groups are each independently -COONa, -CONH2, -CN, -PhSO3Na or the following groups: In each X group, R 11 , R 12 are each independently hydrogen or methyl; n is each independently 1-100; Preferably, in each repeating unit III, n is independently 6-50; And / or, in the acrylic ester polymer, the repeating unit I, the repeating unit II and the repeating unit III are randomly distributed; and / or, the number average molecular weight of the acrylate polymer is 5000-70000 g / mol, preferably 10000-40000 g / mol, more preferably 18000-28000 g / mol, for example 18101 g / mol, 19547 g / mol, 19568 g / mol, 19886 g / mol, 20356 g / mol, 21520 g / mol, 22013 g / mol, 24635 g / mol, 24851 g / mol, 25436 g / mol, 26710 g / mol or 27604 g / mol; and / or, the molecular weight distribution index of the acrylate polymer is less than 1.70, preferably 1.4-1.7, for example 1.50, 1.52, 1.53, 1.54, 1.55, 1.56, 1.57, 1.63 or 1.68; And / or, the glass transition temperature Tg of the acrylic ester polymer is 5-85°C, preferably 40-70°C.

3. An acrylate polymer solution, characterized in that It comprises water and the acrylate polymer according to claim 1 or 2, the solid content of the acrylate polymer solution is 40%-55%, the percentage is the ratio of the mass of the acrylate polymer to the mass of the acrylate polymer solution, and the pH of the acrylate polymer solution is 7-9; Preferably, the pH of the acrylate polymer solution is 7.0, 7.4, 7.5, 7.6, 7.9, 8.0, 8.1, 8.2 or 9.0; Preferably, the viscosity of the acrylate polymer solution is 60-90 mPa·s, for example, 60 mPa·s, 62 mPa·s, 68 mPa·s, 71 mPa·s, 72 mPa·s, 78 mPa·s, 80 mPa·s, 83 mPa·s or 87 mPa·s.

4. A method for preparing an acrylate polymer solution, characterized in that: It includes the following steps: S1. In a protective atmosphere, in the presence of an initiator and a chain transfer agent, a raw material is subjected to a free radical polymerization reaction in water; wherein the raw material comprises a polymerizable monomer, and the polymerizable monomer comprises a monomer A, a monomer B and a monomer C; based on the total mass of the polymerizable monomer, the mass percentage of the monomer A is 15%-45%; the mass percentage of the monomer B is 25%-45%, and the mass percentage of the monomer C is 20%-45%; the monomer B is an olefinic compound containing at least one oxazoline group; and the monomer C is an olefinic compound containing at least one hydrophilic group other than the oxazoline group; S2, adjusting the pH of the reaction system to 7.0-9.0; Preferably, the monomer A is one or more of the compounds represented by formula (M-1): In each monomer A, R1, R2, R3 and R4 are each independently as defined in claim 1 or 2; Preferably, the monomer A is one or more of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-propyl acrylate, n-propyl methacrylate, isopropyl acrylate, isopropyl methacrylate, n-butyl acrylate, n-butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, tert-butyl acrylate, tert-butyl methacrylate, sec-butyl acrylate, sec-butyl methacrylate, n-octyl acrylate, n-octyl methacrylate, tridecyl acrylate, tridecyl methacrylate, dodecyl acrylate, dodecyl methacrylate, stearyl acrylate, stearyl methacrylate, isobornyl acrylate, isobornyl methacrylate, cyclohexyl acrylate, cyclohexyl methacrylate, tert-butyl cyclohexyl acrylate, tert-butyl cyclohexyl methacrylate, cyclododecyl acrylate and cyclododecyl methacrylate; Preferably, the mass percentage of the monomer A is 30%-40%; Preferably, the monomer B is one or more compounds represented by formula (M-2): In each type of monomer B, R5, R6, R7, R8 and R9 are each independently as defined in claim 1 or 2; Preferably, the monomer B is 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-vinyl-4-ethyl-2-oxazoline, 2-vinyl-4,4-dimethyl-2-oxazoline, 2-vinyl-5,5-dimethyl-2-oxazoline, 2-vinyl-4,4,5,5-tetramethyl-2-oxazoline, 2-isopropenyl-2-oxazoline One or more of oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, 2-isopropenyl-5-methyl-2-oxazoline, 2-isopropenyl-4-ethyl-2-oxazoline, 2-isopropenyl-5-ethyl-2-oxazoline, 2-isopropenyl-4,4-dimethyl-2-oxazoline, 2-isopropenyl-5,5-dimethyl-2-oxazoline and 2-isopropenyl-4,4,5,5-tetramethyl-2-oxazoline; Preferably, the mass percentage of the monomer B is 30%-40%; Preferably, the monomer C is one or more compounds represented by formula (M-3): In each monomer C, X and R 10 Each independently as defined in claim 1 or 2; Preferably, the monomer C is one or more of acrylic acid and its salts, methacrylic acid and its salts, methoxy polyethylene glycol acrylate, monoester between acrylic acid and polyethylene glycol, acrylamide, methacrylamide, methacrylonitrile and sodium styrene sulfonate; the acrylate is preferably sodium acrylate or ammonium acrylate; the methacrylate is preferably sodium methacrylate or ammonium methacrylate; Preferably, the mass percentage of the monomer C is 20%-40%; Preferably, the initiator is a water-soluble polymerization initiator or an oil-soluble polymerization initiator; the water-soluble polymerization initiator is preferably a persulfate, such as lithium persulfate, potassium persulfate, sodium persulfate or ammonium persulfate; the oil-soluble polymerization initiator is preferably an organic peroxide, such as cumene hydroperoxide, benzoyl peroxide, tert-butyl hydroperoxide, acetyl peroxide or diisopropylbenzene hydroperoxide; Preferably, the mass of the initiator is 0.05%-0.8%, for example 0.6%-1.6%, of the total mass of the polymerization monomers; Preferably, the initiator is added dropwise into the reaction system in the form of an initiator solution; Preferably, the chain transfer agent is an alkyl mercaptan, a xanthate compound, a phenolic compound, an allyl compound, a halogenated hydrocarbon compound, a vinyl ether, triphenylethane, pentaphenylethane, acrolein, methacrolein, thioglycolic acid, mercaptosuccinic acid, terpinolene or α-methylstyrene dimer; the alkyl mercaptan is preferably n-hexyl mercaptan, n-octyl mercaptan, tert-octyl mercaptan, n-dodecyl mercaptan, tert-dodecyl mercaptan or n-octadecyl mercaptan; the xanthate compound is preferably dimethyl xanthate disulfide or diisopropyl xanthate disulfide; the phenolic compound is preferably 2,6-di-tert-butyl-4-methylphenol or styrenated phenol; the allyl compound is preferably allyl alcohol; the halogenated hydrocarbon compound is preferably dichloromethane, dibromomethane or tetrabromomethane; the vinyl ether is preferably α-benzyloxystyrene, α-benzyloxyacrylonitrile or α-benzyloxyacrylamide; Preferably, the mass of the chain transfer agent is 0.1%-1.0%, such as 0.3%-0.4%, of the total mass of the polymerized monomers; Preferably, the raw materials further include one or both of a reducing agent and an emulsifier; the reducing agent is preferably a reducing inorganic acid salt, a reducing carboxylic acid and its salt, a reducing sugar or an amine; the reducing inorganic acid salt is preferably a sulfite, a bisulfite, a pyrosulfite, a dithionite, a dithionite, a thiosulfate, a formaldehyde sulfonate or a benzaldehyde sulfonate; the reducing carboxylic acid is preferably L-ascorbic acid, isoascorbic acid, tartaric acid or citric acid; the reducing sugar is preferably dextrose or sucrose; The amine is preferably dimethylaniline or triethanolamine; the emulsifier is preferably an anionic surfactant or a nonionic surfactant; the nonionic surfactant is preferably polyethylene glycol alkyl ester, polyethylene glycol alkylphenyl ether or polyethylene glycol alkyl ether; the anionic surfactant is preferably a sulfate ester salt of a higher alcohol, alkylbenzene sulfonate, alkyl diphenyl ether disulfonate, aliphatic sulfonate, aliphatic carboxylate, dehydroabietate, formalin condensate of naphthalenesulfonic acid or a sulfate ester salt of the nonionic surfactant; Preferably, the mass of the water is 100%-120% of the total mass of the polymerized monomers; Preferably, the protective atmosphere is an inert gas or nitrogen; Preferably, the temperature of the free radical polymerization reaction is 35-95°C, preferably 50-70°C, such as 50°C, 60°C or 70°C; Preferably, the pH adjustment is performed using a pH adjusting agent; the pH adjusting agent is preferably sodium hydroxide, potassium hydroxide, ammonia water, sodium bicarbonate or sodium carbonate; the amount of the pH adjusting agent is preferably 0.5%-2.5% of the total mass of the polymerized monomer, for example 0.5%, 1%, 2% or 2.5%; Preferably, the pH of the reaction system is adjusted to 7.0, 7.4, 7.5, 7.6, 7.9, 8.0, 8.1, 8.2 or 9.0; Preferably, the raw materials are added by batch addition, continuous addition or power feed addition; when adding in batches, any one of the following conditions ①-④ is preferably satisfied: ① The initiator is added in three batches; the mass ratio of the first batch of initiator, the second batch of initiator and the third batch of initiator is preferably 1:0.1:0.5 or 1:0.2:0.4; ② The monomers are added in two batches; the mass ratio of the first batch of monomers to the second batch of monomers is preferably 1:2, 1:3 or 1:5; ③ The chain transfer agent is added in two batches; the mass ratio of the first batch of chain transfer agent and the second batch of chain transfer agent is preferably 1:1 or 1:2; ④ The temperature of the free radical polymerization reaction of each batch of raw materials is the same or different.

5. An acrylate polymer solution obtained by the method for preparing an acrylate polymer solution according to claim 4.

6. A method for preparing an acrylate polymer, characterized in that: It includes the following steps: The acrylate polymer solution according to claim 3 or 5 is dried.

7. An acrylate polymer obtained by the method for preparing an acrylate polymer as claimed in claim 6.

8. Use of the acrylate polymer according to any one of claims 1, 2 and 7 as a crosslinking agent for an acidic proton-containing resin; Preferably, the acidic proton-containing resin is a polyarylacetylene resin or a waterborne polyurethane resin.

9. A cross-linked resin, characterized in that The raw materials include an acidic proton-containing resin and an acrylate polymer as described in any one of claims 1, 2 and 7; Preferably, the acidic proton-containing resin is a polyarylacetylene resin or a waterborne polyurethane resin; Preferably, the mass ratio of the acidic proton-containing resin to the acrylate polymer is (50-100):(2-6); Preferably, the cross-linking degree of the cross-linked resin is greater than 88%, for example, 89%, 90%, 91% or 92%; Preferably, the elongation at break of the cross-linked resin is greater than 800%, for example, 850%, 860%, 868%, 880%, 883%, 885%, 891%, 895%, 897%, 901%, 910% or 951%; Preferably, the tensile strength of the cross-linked resin is greater than 35 MPa, for example, 38.3 MPa, 38.4 MPa, 39.0 MPa, 39.1 MPa, 39.4 MPa, 39.5 MPa, 40.1 MPa, 40.2 MPa, 40.5 MPa, 41.0 MPa or 42.6 MPa.

10. Use of the cross-linked resin according to claim 9 in the fields of coatings, adhesives or biomaterials.

Citation Information

Cited By

  • Acrylic acid cathode electrophoretic paint raw paint and preparation method and application thereof

    CN119060575A