Polymer modified cyclodextrin MOFs (Metal-Organic Frameworks) material as well as preparation method and capillary electrophoresis chiral separation method thereof

By modifying cyclodextrin MOFs materials with polystyrene, the problems of insufficient multi-level recognition ability and easy decomposition of cyclodextrin MOFs in the field of chiral separation are solved, and the stability and film formation are improved, providing an efficient capillary The electrophoretic chiral separation method overcomes the problem of decomposition and difficulty in modifying the original materials in water.

CN118878748AActive Publication Date: 2024-11-01BEIJING INSTITUTE OF PETROCHEMICAL TECHNOLOGY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311609129.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-11-28
Publication Date
2024-11-01
Estimated Expiration
2043-11-28

AI Technical Summary

Technical Problem

The existing cyclodextrin MOFs materials have problems in the field of chiral separation, such as insufficient multi-level chiral recognition ability, easy to decompose in water, and difficult to modify the inner wall of the capillary, which limits its application in the field of chromatographic separation.

Method used

Polystyrene modified cyclodextrin MOFs material, and the polystyrene and cyclodextrin MOFs are combined through polymerization to form a polymer @ cyclodextrin MOFs composite material, which is modified on the inner wall of the capillary to improve its film-forming and chiral separation. ability.

Benefits of technology

The stability and film formation of cyclodextrin MOFs materials have been improved, and the chiral substances can be effectively separated, which overcomes the problem of decomposition and difficulty in modifying the original materials in water, reduces the separation cost, and provides an efficient capillary electrophoresis hand. Sexual separation method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878748A_ABST
    Figure CN118878748A_ABST
Patent Text Reader

Abstract

The invention discloses a polymer modified cyclodextrin MOFs (Metal-Organic Frameworks) material as well as a preparation method and a capillary electrophoresis chiral separation method thereof. The method comprises the following steps: firstly, dispersing a polymer (such as a styrene monomer) and cyclodextrin MOFs in an organic solvent, and adding an initiator to prepare the polystyrene modified cyclodextrin MOFs material through an ultraviolet irradiation initiation method. The polystyrene modified cyclodextrin MOFs material prepared by the preparation method disclosed by the invention is uniformly dispersed, and the particle size is 200-400nm. Furthermore, the amino acid enantiomers are dispersed in a chloroform solution, the solution is introduced into a capillary tube for coating, and chiral separation of the amino acid enantiomers can be realized by utilizing capillary electrophoresis. The preparation method disclosed by the invention is simple and easy to operate, low in cost and cheap and easily available in raw materials, and has potential application in the field of separation of drug molecules and amino acid biological drugs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of chiral separation, and relates to a polymer-modified cyclodextrin MOFs material and a preparation method thereof and a capillary electrophoresis chiral separation method, and specifically relates to a polymer-modified cyclodextrin MOFs and a preparation method thereof and an application thereof in a capillary electrophoresis chiral separation method, and especially relates to the preparation of a polymer-modified cyclodextrin MOFs material and the application of the material as a coating in capillary electrophoresis to separate amino acid enantiomers. Background Art

[0002] Cyclodextrin MOFs are new porous materials that not only have excellent adsorption properties and catalytic activity, but also have excellent chiral separation performance, chemical stability and pore size distribution. Based on the above excellent properties, cyclodextrin MOFs have broad application prospects in many fields (such as gas adsorption, catalysts, drug separation, water treatment and biosensors, etc.).

[0003] Among these applications, cyclodextrin MOFs have special advantages in chiral separation. Chiral separation refers to the process of separating different chiral structures of a substance. For chiral separation, the most commonly used method is based on stereoselective adsorption, that is, using the stereoselective adsorption of chiral molecules on the surface of chiral materials. Due to their unique structure and surface properties, cyclodextrin MOFs can effectively adsorb and separate substances with different chiral structures, so they have great application potential in chiral separation.

[0004] However, to date, new cyclodextrin MOFs materials with multi-level chiral recognition capabilities have not yet been developed. In addition, when cyclodextrin MOFs are used as chiral separation materials in chromatographic separation, they are easily decomposed by water and are not easy to be modified on the inner wall of the capillary or in the chromatographic separation medium, which greatly limits their separation and analysis applications in the field of chromatography. This may be due to: (1) The currently reported cyclodextrin MOFs have a long synthesis cycle, which takes more than ten days to obtain the product, and the preparation reproducibility of the material is poor; (2) The method of modifying cyclodextrin MOFs on the surface of chromatographic fillers is immature, which limits its wide application. Therefore, the modification of current cyclodextrin MOFs materials is of great research significance.

[0005] Polymer materials have multifunctional reactive groups, and some special polymers have good film-forming properties. At the same time, the flexible structure of the polymer itself can greatly improve the plasticity and ductility of rigid structure cyclodextrin MOFs, making them reprocessable. Therefore, constructing a preparation strategy for rigid and flexible materials and synthesizing polymer-protected cyclodextrin MOFs is a potential research direction. In the future, through further research and development of cyclodextrin MOFs, we can expect to make more progress in the field of chiral separation and contribute to the development of fields such as drug manufacturing, food processing and fine chemicals. Summary of the invention

[0006] In order to improve the above technical problems, the present invention provides a novel polystyrene modified cyclodextrin MOFs chiral separation material and a preparation method thereof and a capillary electrophoresis chiral separation method. The polystyrene modified cyclodextrin MOFs material of the present invention has good film-forming properties and excellent chiral separation ability.

[0007] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0008] A cyclodextrin MOFs composite material comprises cyclodextrin MOFs and a polymer modified on the cyclodextrin MOFs. Preferably, in the composite material, the polymer runs through the cyclodextrin MOFs.

[0009] According to an embodiment of the present invention, the particle size of the composite material is 200-400 nm, for example, 230 nm, 280 nm, 350 nm, 390 nm, 400 nm.

[0010] According to an embodiment of the present invention, the cyclodextrin MOFs are MOFs prepared from γ-cyclodextrin; preferably, the cyclodextrin MOFs are MOFs prepared from γ-cyclodextrin and potassium ions or other metal ions.

[0011] According to an embodiment of the present invention, the polymer is selected from one or a mixture of two or more of polystyrene, polymaleic anhydride, and poly(N-isopropylacrylamide).

[0012] According to an embodiment of the present invention, the composite material is prepared by a polymerization reaction between polymer monomers and cyclodextrin MOFs under the action of an initiator and initiated by light to obtain a polymer-modified cyclodextrin MOFs material.

[0013] According to an embodiment of the present invention, the polymer monomer may be one or a mixture of two or more of styrene, maleic anhydride, and N-isopropylacrylamide.

[0014] According to an embodiment of the present invention, the mass ratio of the polymer monomer to the cyclodextrin MOFs is 1:0.05-1:0.1, exemplified by 1:0.05, 1:0.06, 1:0.07, 1:0.08, 1:0.09, and 1:0.1.

[0015] According to an embodiment of the present invention, the initiator is, for example, azobisisobutyronitrile. Preferably, the amount of the initiator is 1%-3% of the amount of the polymer monomer, exemplified by 1%, 1.5%, 2%, 2.5%, 3%.

[0016] The present invention also provides a method for preparing the composite material, comprising: initiating a polymerization reaction between polymer monomers and cyclodextrin MOFs under the action of an initiator and irradiating light to obtain a polymer-modified cyclodextrin MOFs material.

[0017] According to an embodiment of the present invention, the polymer monomers, cyclodextrin MOFs and initiators are selected and defined as described above.

[0018] According to an embodiment of the present invention, the cyclodextrin MOFs are added to the reaction system in the form of a solution. For example, the cyclodextrin MOFs are first dispersed in an organic solvent to obtain a cyclodextrin MOFs solution, and then mixed with a polymer monomer and an initiator to obtain a reaction solution. For example, the organic solvent is 1,4-dioxane, tetrahydrofuran, etc.

[0019] In one embodiment of the present invention, the concentration of the cyclodextrin MOFs solution is 1 to 10 mg / mL, exemplified by 1 mg / mL, 5 mg / mL, 6 mg / mL, 7 mg / mL, 8 mg / mL, and 10 mg / mL.

[0020] According to an embodiment of the present invention, the polymer monomer is preferably added to the cyclodextrin MOFs solution in a dropwise manner. For example, the polymer monomer is added dropwise to the cyclodextrin MOFs solution under stirring.

[0021] According to an embodiment of the present invention, the preparation method further comprises deoxygenating the reaction solution. For example, oxygen in the reaction solution is removed by a freezing cycle. Exemplarily, the method for removing oxygen is to freeze the reaction solution with liquid nitrogen, evacuate, fill with nitrogen, and repeat the cycle three times.

[0022] According to an embodiment of the present invention, the preparation method further comprises subjecting the deoxygenated reaction solution to ultrasonic treatment. Preferably, the ultrasonic treatment time is 20 to 40 minutes, exemplified by 20 minutes, 30 minutes, and 40 minutes.

[0023] According to an embodiment of the present invention, the illumination is performed by ultraviolet light. For example, ultraviolet light with a wavelength of 254 nm is used for illumination. Preferably, the illumination reaction time is 6-24 hours. Exemplary is 6 hours, 8 hours, 10 hours, 12 hours, 24 hours.

[0024] According to an embodiment of the present invention, the preparation method further comprises, after the reaction is completed, centrifuging, washing and drying to obtain the polymer-modified cyclodextrin MOFs material. Preferably, the drying is natural drying at room temperature or drying at a temperature of 30-50°C.

[0025] According to an embodiment of the present invention, the method for preparing the composite material comprises the following steps:

[0026] (1) dispersing cyclodextrin MOFs material in an organic solvent to obtain a cyclodextrin MOFs solution;

[0027] (2) adding a polymer monomer solution and an initiator to the cyclodextrin MOFs solution of step (1);

[0028] (3) removing oxygen from the reaction solution by a refrigeration cycle method;

[0029] (4) Ultrasound and ultraviolet light to induce polymer reaction;

[0030] (5) After the reaction is completed, centrifuge, wash and dry to obtain the target product.

[0031] During the reaction process: after ultrasonic dispersion, the polymer monomers are first dispersed inside the pores of cyclodextrin MOFs. After the initiator is added, the polymer monomers in the pores are polymerized with the polymer monomers in the solution to prepare polymer-modified nanomaterials that run through the cyclodextrin MOFs.

[0032] The present invention also provides the use of the cyclodextrin MOFs composite material in capillary electrophoresis separation, preferably in capillary electrophoresis chiral separation, for example, as a coating modified on the inner wall of the capillary for separation of chiral substances.

[0033] According to an embodiment of the present invention, the chiral substance is an amino acid chiral enantiomer or a drug molecule, for example, one or a mixture of two chiral enantiomers of methionine, serine, histidine, phenylalanine and their derivatives.

[0034] The present invention also provides a capillary electrophoresis chiral separation method of the cyclodextrin MOFs composite material, comprising using the cyclodextrin MOFs composite material as a coating to modify the inner wall of the capillary to separate chiral substances.

[0035] According to an embodiment of the present invention, the method of modifying the inner wall of a capillary with a cyclodextrin MOFs composite material as a coating is as follows: injecting a cyclodextrin MOFs composite material solution into the capillary. For example, the injection flow rate of the cyclodextrin MOFs composite material solution is 0.1 to 0.5 mL / h, exemplified by 0.1 mL / h, 0.3 mL / h, and 0.5 mL / h.

[0036] According to an embodiment of the present invention, the concentration of the cyclodextrin MOFs composite material solution is 0.5 mg / mL-2.0 mg / mL, for example, 0.5 mg / mL, 1.0 mg / mL, 1.5 mg / mL, 2.0 mg / mL.

[0037] Beneficial effects of the present invention:

[0038] Cyclodextrin MOFs is a new type of organic composite material with excellent adsorption properties and large specific surface area. Therefore, in recent years, cyclodextrin MOFs have been successfully applied to redox reactions, methanol dehydrogenation reactions and adsorption of pollutants. However, in the field of chiral separation, research on cyclodextrin MOFs is still relatively small. The main reasons are as follows: (1) The synthesis and preparation process of cyclodextrin MOFs is lengthy, generally requiring 7-8 days of synthesis time; (2) Cyclodextrin MOFs materials have poor stability, will decompose in water and cannot tolerate acid and alkali; (3) Although cyclodextrin MOFs materials have good chiral separation capabilities, they do not have binding groups that can be covalently bonded to chromatographic separation media. Among polymer materials, polystyrene has good film-forming properties and controllable polymerization properties. In view of this:

[0039] (1) The present invention combines a polymer (such as polystyrene) with cyclodextrin MOFs to prepare a polymer@cyclodextrin MOFs hybrid material, which can not only give full play to the excellent chiral separation ability of cyclodextrin MOFs, but also utilize the film-forming property of polystyrene to prepare a chiral separation medium that can be modified on the inner wall of the capillary, thereby achieving capillary electrophoresis separation of chiral molecules. The present invention improves its film-forming ability and bonding performance with the chromatographic separation medium by modifying cyclodextrin MOFs with polystyrene, explores a new strategy for material synthesis and preparation, and studies its application in chiral drug separation.

[0040] (2) Styrene monomer enters the pores of cyclodextrin MOFs after ultrasound treatment, and after adding an initiator, light is irradiated to initiate polymerization, thereby obtaining a polymer-modified cyclodextrin MOFs material. Taking advantage of the good film-forming property of polystyrene, it can be evenly coated on the inner wall of the capillary. Styrene-modified cyclodextrin MOFs also have good chiral separation ability. After being coated on the inner wall of the capillary, it can be used as a coating column for capillary electrophoresis separation to achieve chiral separation of amino acid enantiomers. The method of the present invention overcomes the problem that when unmodified cyclodextrin MOFs are used as coatings, on the one hand, cyclodextrin MOFs have no film-forming property and cannot be evenly coated on the inner wall of the capillary; on the other hand, cyclodextrin MOFs decompose in a buffer solution and cannot maintain the ability of chiral separation. The polystyrene-modified cyclodextrin MOFs obtained by the present invention can not only protect the chiral separation of the material from being decomposed during capillary electrophoresis separation, but also provide a polymer that is evenly coated on the inner wall of the capillary.

[0041] (3) The present invention prepares different polystyrene-modified cyclodextrin MOFs samples by different modification methods. The chiral separation performance of these materials is studied experimentally, and the mechanism of chiral separation is analyzed. At the same time, the present invention applies these materials to actual chiral separation and evaluates their performance, in order to contribute to the development of new chiral separation materials and methods.

[0042] (4) The preparation method of the polymer@cyclodextrin MOFs composite material provided by the present invention uses ultraviolet light to initiate polymerization to prepare polystyrene-modified cyclodextrin MOFs, which can prevent styrene from being violently initiated to polymerize and cause uneven particle size distribution. The preparation cost is low and the operation is simple, which embodies the significance of green chemistry.

[0043] (5) Compared with liquid chromatography filler coating to achieve chiral separation of substances, the capillary electrophoresis-based coated tube separation technology constructed by the present invention requires less composite material, and only microliters of coating solution are needed to achieve capillary inner wall coating, thereby greatly reducing the cost of the chiral separation composite material used. At the same time, the capillary electrophoresis-based chiral separation technology requires less sample volume (the injection volume is in the nanoliter level of sample solution), and also provides an irreplaceable separation tool for the separation of trace or trace chiral substances.

[0044] (6) The preparation method of the polymer@cyclodextrin MOFs composite material constructed by the present invention is universal and can be applied to the preparation of various chiral MOFs bonded polymers and applied to capillary electrophoresis coating chiral separation. Polystyrene can also be replaced by other types of polymers, which can take into account the film-forming properties on the one hand, and can be mixed with multifunctional polymer blocks on the other hand to enhance the performance advantages of the polymer@MOFs composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1Schematic diagram of chiral stationary phase prepared for polystyrene modified cyclodextrin MOFs for chiral separation;

[0046] Figure 2 The particle size distribution diagram of the polystyrene modified cyclodextrin MOFs (polystyrene@MOFs) prepared in Example 1;

[0047] Figure 3 The XRD patterns of the polystyrene-modified cyclodextrin MOFs prepared in Example 1 before and after modification;

[0048] Figure 4 FT-IR spectrum of polystyrene modified cyclodextrin MOFs prepared in Example 1;

[0049] Figure 5 This is the SEM image of the polystyrene modified cyclodextrin MOFs prepared in Example 1;

[0050] Figure 6 This is the capillary electrophoresis amino acid chiral separation diagram of the polystyrene modified cyclodextrin MOFs prepared in Example 1.

[0051] Figure 7 This is the capillary electrophoresis amino acid chiral separation diagram of the polystyrene-modified cyclodextrin MOFs prepared in Example 2-5.

[0052] Figure 8 This is a graph showing the repeatability results of capillary electrophoresis amino acid chiral separation of polystyrene-modified cyclodextrin MOFs prepared in Example 6. DETAILED DESCRIPTION

[0053] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention, and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0054] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0055] Example 1

[0056] The preparation method of polystyrene modified cyclodextrin MOFs comprises the following steps:

[0057] (1) Disperse 50 mg of cyclodextrin MOFs (purchased from Xi'an Ruixi Biotechnology Co., Ltd.) in 10 mL of 1,4-dioxane;

[0058] (2) Add styrene monomer (1.0 g) and initiator azobisisobutyronitrile (10 mg) and disperse by ultrasonic for 30 minutes;

[0059] (3) removing oxygen from the reaction solution by using a freezing cycle method (first freezing the reaction solution into a solid using liquid nitrogen, then evacuating the solution with a vacuum pump for 3 minutes, then closing the vacuum system and introducing nitrogen to allow the solution to slowly heat up and melt. Repeat this operation three times);

[0060] (4) After 30 minutes of ultrasound, the polymer reaction was initiated by ultraviolet light and irradiated continuously for 12 hours;

[0061] (5) After the reaction, the mixture was centrifuged (rotation speed: 10,000 r / min), washed with 1,4-dioxane, and dried at 50° C. for 10 h to obtain polystyrene modified cyclodextrin MOFs (polystyrene@MOFs, PS-CDMOF).

[0062] Figure 2 This is the particle size distribution diagram of the styrene@MOFs prepared in this example. From the results, it can be seen that the polystyrene@MOFs prepared in this example did not decompose after ultrasonic dispersion in water (concentration of 1.0 mg / mL), the particle size was about 200 nm, and the particle size was evenly dispersed, which proves that polystyrene was successfully modified on cyclodextrin MOFs, thereby inhibiting the decomposition of cyclodextrin MOFs in water.

[0063] Figure 3 The XRD spectra of the polystyrene-modified cyclodextrin MOFs prepared in this example before (the product CDMOF of step (1)) and after modification (PS-CDMOF). From the results in the figure, it can be seen that the crystalline structure of the cyclodextrin MOFs is not destroyed before and after modification with polystyrene, and polystyrene is successfully modified on the cyclodextrin MOFs.

[0064] Figure 4 FT-IR spectrum of polystyrene modified cyclodextrin MOFs prepared in Example 1. As can be seen from the figure, at 1596 cm -1 The peak at 2919 cm -1 The characteristic peak at corresponds to the CH stretching vibration of the methylene group on PS, which indicates the successful preparation of polystyrene modified cyclodextrin MOFs composites.

[0065] Figure 5 This is the SEM spectrum of the polystyrene-modified cyclodextrin MOFs prepared in Example 1; it can be seen from the figure that after the polystyrene is modified, the MOFs still maintain their solid structure and are not damaged by the modification process.

[0066] Example 2

[0067] The preparation method of polystyrene modified cyclodextrin MOFs comprises the following steps:

[0068] (1) Disperse cyclodextrin MOFs (60 mg) in 10 mL 1,4-dioxane;

[0069] (2) Add styrene monomer (1.0 g) and initiator azobisisobutyronitrile (15 mg) and disperse by ultrasonic for 30 minutes;

[0070] (3) removing oxygen from the reaction solution by using a freezing cycle method (first freezing the reaction solution into a solid using liquid nitrogen, then evacuating the solution with a vacuum pump for 3 minutes, then closing the vacuum system and introducing nitrogen to allow the solution to slowly heat up and melt. Repeat this operation three times);

[0071] (4) After 30 minutes of ultrasound, the polymer reaction was initiated by ultraviolet light and irradiated continuously for 24 hours;

[0072] (5) After the reaction, the polystyrene-modified cyclodextrin MOFs were obtained by centrifugation (rotation speed: 10,000 r / min), washing with 1,4-dioxane, and drying at 50°C for 10 h.

[0073] Example 3

[0074] The preparation method of polystyrene modified cyclodextrin MOFs comprises the following steps:

[0075] (1) Disperse cyclodextrin MOFs (70 mg) in 10 mL 1,4-dioxane;

[0076] (2) Add styrene monomer (1.0 g) and initiator azobisisobutyronitrile (20 mg) and disperse by ultrasonic for 30 minutes;

[0077] (3) removing oxygen from the reaction solution by using a freezing cycle method (first freezing the reaction solution into a solid using liquid nitrogen, then evacuating the solution with a vacuum pump for 3 minutes, then closing the vacuum system and introducing nitrogen to allow the solution to slowly heat up and melt. Repeat this operation three times);

[0078] (4) After 30 minutes of ultrasound, the polymer reaction was initiated by ultraviolet light and irradiated continuously for 36 hours;

[0079] (5) After the reaction, the polystyrene-modified cyclodextrin MOFs were obtained by centrifugation (rotation speed: 10,000 r / min), washing with 1,4-dioxane, and drying at 50°C for 10 h.

[0080] Example 4

[0081] The preparation method of polystyrene modified cyclodextrin MOFs comprises the following steps:

[0082] (1) Disperse cyclodextrin MOFs (80 mg) in 10 mL 1,4-dioxane;

[0083] (2) Add styrene monomer (1.0 g) and initiator azobisisobutyronitrile (25 mg) and disperse by ultrasonic for 30 minutes;

[0084] (3) removing oxygen from the reaction solution by using a freezing cycle method (first freezing the reaction solution into a solid using liquid nitrogen, then evacuating the solution with a vacuum pump for 3 minutes, then closing the vacuum system and introducing nitrogen to allow the solution to slowly heat up and melt. Repeat this operation three times);

[0085] (4) After 30 minutes of ultrasound, the polymer reaction was initiated by ultraviolet light and irradiated continuously for 6 hours;

[0086] (5) After the reaction, the polystyrene-modified cyclodextrin MOFs were obtained by centrifugation, washing, and drying at 50°C for 10 h.

[0087] Example 5

[0088] The preparation method of polystyrene modified cyclodextrin MOFs comprises the following steps:

[0089] (1) Disperse cyclodextrin MOFs (100 mg) in 10 mL 1,4-dioxane;

[0090] (2) Add styrene monomer (1.0 g) and initiator azobisisobutyronitrile (15 mg) and disperse by ultrasonic for 30 minutes;

[0091] (3) removing oxygen from the reaction solution by using a freezing cycle method (first freezing the reaction solution into a solid using liquid nitrogen, then evacuating the solution with a vacuum pump for 3 minutes, then closing the vacuum system and introducing nitrogen to allow the solution to slowly heat up and melt. Repeat this operation three times);

[0092] (4) After 30 minutes of ultrasound, the polymer reaction was initiated by ultraviolet light and irradiated continuously for 12 hours;

[0093] (5) After the reaction, the polystyrene-modified cyclodextrin MOFs were obtained by centrifugation (rotation speed: 10,000 r / min), washing with 1,4-dioxane, and drying at 50°C for 10 h.

[0094] Example 6

[0095] The polystyrene-modified cyclodextrin MOFs prepared in Example 1 were used as coating materials to construct capillary chiral coatings and amino acid chiral separation methods:

[0096] Before coating the capillary, the capillary needs to be activated first, rinsed with methanol for 10-15 minutes, then rinsed with deionized water for 2-5 minutes, then rinsed with 0.1M NaOH for 15-30 minutes, and finally rinsed with deionized water for 2-5 minutes, and then rinsed with chloroform for 2-5 minutes.

[0097] Using chloroform as solvent, prepare a 1.0 mg / mL polystyrene-modified cyclodextrin MOFs solution, and slowly inject it into a capillary with a length of 20 cm and an inner diameter of 75 μm at a flow rate of 0.3 mL / h by a syringe until droplets continuously drip out from the other end. After the polystyrene-modified cyclodextrin MOFs are injected into the capillary, they are blown dry with nitrogen. A thin film will form on the capillary wall after drying (it should be noted during the coating process that too fast an injection speed may lead to uneven coating, while too slow an injection speed will affect the coating effect.). Finally, a capillary chiral column coated with polystyrene-modified cyclodextrin MOFs is obtained.

[0098] In order to determine the chiral separation performance of polystyrene-modified cyclodextrin MOFs, 25mM sodium tetraborate and 5mg / L SDS were used as buffer, Dns-DL-Met (a derivative of methionine derivatized with dansyl chloride) was used as the separation object, and the height difference (15cm) injection method was used with an injection volume of 10s to test the chiral separation ability of polystyrene-modified cyclodextrin MOFs. The chiral separation ability of the coated capillary with an effective length of 20cm and an inner diameter of 75μm was tested under the condition of a separation voltage of 10kV. The chiral separation results are shown in Figure 6 The results show that polystyrene-modified cyclodextrin MOFs can be successfully coated on the inner wall of the capillary and achieve the separation of chiral amino acids with good chiral separation ability.

[0099] Example 7

[0100] Capillary electrophoresis separation condition screening and sample preparation: The chiral amino acid Dns-DL-Met was used as a sample to investigate the chiral separation ability of the capillary chiral column coated with the polystyrene-modified cyclodextrin MOFs prepared in Example 2-5 as a coating material. The experimental method is as follows:

[0101] The polystyrene-modified cyclodextrin MOFs samples prepared in Examples 2-5 were dissolved in chloroform solvent to prepare a 1.0 mg / mL suspension, and were slowly injected into a capillary with a length of 20 cm and an inner diameter of 75 μm at a flow rate of 0.3 mL / h by a syringe. After the polystyrene-modified cyclodextrin MOFs were injected into the capillary, they were blown dry with nitrogen. A thin film was formed on the capillary wall after the blow-drying, and finally a capillary chiral column coated with polystyrene-modified cyclodextrin MOFs was obtained.

[0102] Using 25mM sodium tetraborate and 5mg / L SDS as buffer, Dns-DL-Met (derivative of methionine derivatized with dansyl chloride) as separation object, using height difference (15cm) injection method, injection volume of 10s, respectively tested the chiral separation ability of polystyrene modified cyclodextrin MOFs prepared in Examples 2-5 (CDMOFs were 60.0mg, 70.0mg, 80.0mg, 100.0mg). The chiral separation ability of the coated capillary with an effective length of 20cm and an inner diameter of 75μm was tested under the condition of separation voltage of 10kV. The chiral separation results are shown in Figure 7 The results show that polystyrene-modified cyclodextrin MOFs can be successfully coated on the inner wall of the capillary and achieve the separation of chiral amino acids. Changing the mass ratio of polymer monomer to cyclodextrin MOFs will affect the chiral separation ability of the prepared polystyrene-modified cyclodextrin MOFs.

[0103] Example 8

[0104] Stability test experiment of polystyrene-modified cyclodextrin MOFs coated capillary electrophoresis: The polystyrene-modified cyclodextrin MOFs prepared in Example 1 were modified on the inner wall of the capillary using the physical coating method constructed in Example 6, and the chiral separation of the chiral amino acid Dns-DL-Met was performed using the separation method in Example 7 (separation voltage of 10 kV and capillary column length of 20 cm and inner diameter of 75 μm). The test was repeated ten times, and the results were as follows: Figure 8 As shown in the figure, it can be seen that the chiral separation ability of the polystyrene-modified cyclodextrin MOFs-coated capillary column has not been significantly reduced after ten consecutive tests. This shows that the chiral stationary phase of the polystyrene-modified cyclodextrin MOFs-coated capillary column prepared by the present invention has good reusability and stability.

[0105] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A cyclodextrin MOFs composite material, characterized in that: The composite material comprises cyclodextrin MOFs and a polymer modified on the cyclodextrin MOFs. Preferably, in the composite material, the polymer runs through the cyclodextrin MOFs.

2. The cyclodextrin MOFs composite material according to claim 1, characterized in that: The particle size of the composite material is 200-400nm. Preferably, the cyclodextrin MOFs are MOFs prepared from γ-cyclodextrin; preferably, the cyclodextrin MOFs are MOFs prepared from γ-cyclodextrin and potassium ions or other metal ions. Preferably, the polymer is selected from one or a mixture of two or more of polystyrene, polymaleic anhydride, and poly(N-isopropylacrylamide).

3. The cyclodextrin MOFs composite material according to claim 1 or 2, characterized in that: The composite material is prepared by a polymerization reaction between polymer monomers and cyclodextrin MOFs under the action of an initiator and initiated by light to obtain a polymer-modified cyclodextrin MOFs material. Preferably, the polymer monomer may be one or a mixture of two or more of styrene, maleic anhydride, and N-isopropylacrylamide. Preferably, the mass ratio of the polymer monomer to the cyclodextrin MOFs is 1:0.05-1:0.

1. Preferably, the initiator is, for example, azobisisobutyronitrile. Preferably, the amount of the initiator used is 1%-3% of the amount of the polymer monomer used.

4. The method for preparing the cyclodextrin MOFs composite material according to any one of claims 1 to 3, characterized in that: The preparation method comprises the steps of initiating a polymerization reaction between polymer monomers and cyclodextrin MOFs under the action of an initiator and irradiating light to obtain a polymer-modified cyclodextrin MOFs material.

5. The preparation method according to claim 4, characterized in that: The cyclodextrin MOFs are added to the reaction system in the form of a solution. For example, the cyclodextrin MOFs are first dispersed in an organic solvent to obtain a cyclodextrin MOFs solution, and then mixed with a polymer monomer and an initiator to obtain a reaction solution. For example, the organic solvent is 1,4-dioxane, tetrahydrofuran, etc. Preferably, the concentration of the cyclodextrin MOFs solution is 1 to 10 mg / mL. Preferably, the polymer monomer is added to the cyclodextrin MOFs solution in a dropwise manner. Preferably, the preparation method further comprises deoxygenating the reaction liquid, for example, by removing oxygen from the reaction liquid using a refrigeration cycle. Preferably, the preparation method further comprises subjecting the deoxygenated reaction solution to ultrasonic treatment. Preferably, the ultrasonic treatment time is 20 to 40 minutes. Preferably, the illumination is ultraviolet light. Preferably, the light irradiation reaction time is 6-24 hours.

6. The preparation method according to claim 4 or 5, characterized in that: The method for preparing the composite material comprises the following steps: (1) dispersing cyclodextrin MOFs material in an organic solvent to obtain a cyclodextrin MOFs solution; (2) adding a polymer monomer solution and an initiator to the cyclodextrin MOFs solution of step (1); (3) removing oxygen from the reaction solution by a refrigeration cycle method; (4) Ultrasound and ultraviolet light to induce polymer reaction; (5) After the reaction is completed, centrifuge, wash and dry to obtain the target product.

7. Use of the cyclodextrin MOFs composite material according to any one of claims 1 to 3 and / or the cyclodextrin MOFs composite material prepared by the preparation method according to any one of claims 4 to 6 in capillary electrophoresis separation. Preferably, the cyclodextrin MOFs composite material is used in capillary electrophoresis chiral separation. For example, the cyclodextrin MOFs composite material is used as a coating modified on the inner wall of a capillary for separation of chiral substances.

8. The use according to claim 7, characterized in that The chiral substance is an amino acid chiral enantiomer or a drug molecule, for example, one or a mixture of two chiral enantiomers such as methionine, serine, histidine, phenylalanine and their derivatives.

9. A capillary electrophoresis chiral separation method for the cyclodextrin MOFs composite material according to any one of claims 1 to 3 and / or the cyclodextrin MOFs composite material prepared by the preparation method according to any one of claims 4 to 6, characterized in that: The method includes using a cyclodextrin MOFs composite material as a coating to modify the inner wall of a capillary to separate chiral substances.

10. The method according to claim 9, characterized in that The method for modifying the inner wall of a capillary with the cyclodextrin MOFs composite material as a coating is as follows: injecting a cyclodextrin MOFs composite material solution into the capillary. Preferably, the concentration of the cyclodextrin MOFs composite material solution is 0.5 mg / mL-2.0 mg / mL.

Citation Information

Patent Citations

  • Compounded metal-organic framework photocatalyst for controllable free-radical polymerization

    CN107973914A

  • Preparation method and application of glycosyl metal porous coordination polymer

    CN109851803A

  • Cyclodextrin based metallic organic frame material and preparation method thereof

    CN110054782A