Anti-flash-rust water-borne epoxy resin, preparation method thereof and anti-flash-rust water-borne epoxy resin coating

By introducing corrosion inhibitors with thiol or amino groups into epoxy resin, the flash rust problem in water-based coatings is solved, and excellent anti-flash rust and mechanical properties are achieved, avoiding adverse effects on coating performance .

CN118878786APending Publication Date: 2024-11-01广州境好新材料有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411105988.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Water-based coatings are prone to cause flash rust on the metal matrix during the coating process, especially in the welding area, which leads to a decrease in the anti-corrosion performance of the coating. Existing methods such as adding anti-flash rust agents have compatibility problems and adverse effects on the performance of the coating. .

Method used

By introducing thiol or amino groups that can form complexes with the metal matrix into the epoxy resin, and using a corrosion inhibitor grafting reaction, an anti-flash rust-proof epoxy resin is designed to avoid the impact on the performance of the coating.

Benefits of technology

It effectively reduces the reaction point between metal and water, inhibits flash rust phenomenon, and maintains the original mechanical properties of the epoxy resin coating, providing excellent flash rust resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses an anti-flash-rust water-borne epoxy resin, the resin is designed from a molecular chain segment structure and an aggregation state, and a corrosion inhibitor is introduced into the epoxy resin structure through grafting, so that the anti-flash-rust problem of a coating is solved. The anti-flash-rust water-borne epoxy resin is an emulsion obtained by carrying out a grafting reaction on epoxy resin and a corrosion inhibitor and introducing a group capable of forming a complex with a metal matrix on an epoxy resin main body structure; the group capable of forming the complex with the metal matrix is sulfydryl or / and amino. The invention further provides a preparation method of the anti-flash-rust water-borne epoxy resin and a water-borne epoxy resin coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of functional coatings, and in particular to an anti-flash rust waterborne epoxy resin and a preparation method and application thereof Background Art

[0002] In recent years, in the coatings industry, many companies have given full play to their professional and technical advantages, accelerated the transformation of coatings from solvent-based coatings to hydrophilic coatings, and actively promoted water-based coatings. Environmental protection has become an important direction for the high-quality development of the coatings industry.

[0003] Since water-based paint dries slowly during the painting process, and the drying process is greatly affected by the ambient temperature and humidity, the latent heat of evaporation of water in water-based paint is large, the evaporation rate is slow, and the water is in contact with the metal substrate for a long time during the construction process, it is easy to cause flash rust on the metal substrate during the actual painting process. In addition, in the observation of the actual construction process, it was found that flash rust was particularly serious in the welding area where water-based paint was used on the metal substrate. In the actual construction process, it is often necessary to use coatings in the welding area to form a protective layer in the welding area to enhance the anti-corrosion performance of the area. The appearance of flash rust will undoubtedly weaken the anti-corrosion performance and various performance of the coating in this area, and even cause the coating to fail. The occurrence of flash rust is a common problem in the painting process of water-based paint, and it is also one of the most urgent problems to be solved in the use of water-based paint.

[0004] Flash rust has a great influence on the performance of the coating. Usually, flash rust occurs some time before the coating film dries and solidifies. Metal substrate, water and oxygen are the three elements of flash rust, and flash rust is an electrochemical phenomenon. Its cause is related to the dissolution and precipitation of iron compounds, because water-based paint itself is a conductor. Charge transfer channels are formed in different areas with potential differences. Under the combined action of water and oxygen, corrosion occurs, and brown or black rust appears on the surface of the film. At the same time, some unfavorable factors will also accelerate flash rust, such as slow drying conditions: low temperature, high humidity (especially serious when the relative humidity is greater than 85%), and too long curing time; unclean and unstable iron substrates that are pre-treated. Usually, newly treated steel surfaces are most prone to flash rust; the lower the Ph value of the coating system, the more likely it is to flash rust.

[0005] At present, the best way for the coating industry to solve the flash rust problem during the coating process of water-based coatings is to add an appropriate amount of anti-flash rust agent to the coating. By adding anti-flash rust agents during the coating preparation process, the coating can have better anti-flash and anti-rust properties. At present, this method is widely used in water-based anti-corrosion primers, but this method also has disadvantages. If there are compatibility problems with the coating and the resin does not contain anti-flash rust additives, it is easy to have an adverse effect on the later coating. Therefore, there is an urgent need for a coating that can solve the anti-flash rust problem. Summary of the invention

[0006] In order to overcome the deficiencies of the prior art, the purpose of the present application is to provide an anti-flash rust water-based epoxy resin, design the resin from the perspective of molecular segment structure and aggregation state, and introduce a corrosion inhibitor into the epoxy resin structure by grafting to solve the anti-flash rust problem of the coating.

[0007] To solve the above problems, the technical solutions adopted in this application are as follows:

[0008] The embodiment of the present application provides an anti-flash rust water-based epoxy resin, which is an emulsion obtained by introducing a group capable of forming a complex with a metal matrix into the main structure of the epoxy resin through a grafting reaction between the epoxy resin and the corrosion inhibitor; the group capable of forming a complex with the metal matrix is ​​a thiol group and / or an amino group.

[0009] As a further preferred embodiment, the epoxy resin described in the embodiment of the present application is one or more of bisphenol A type epoxy resin, bisphenol A type E-51 epoxy resin, bisphenol A type E-44 epoxy resin, bisphenol F type E-51 epoxy resin, and bisphenol F type E-44 epoxy resin.

[0010] As a further preferred scheme, the corrosion inhibitor described in the embodiment of the present application is one or more of 3-amino-5-mercapto-1,2,4-triazole, 1H-1,2,4-triazole-3-thiol, and 5-(4-pyridyl)-1H-1,2,3-triazole-3-thiol.

[0011] As a further preferred solution, the mass percentages of the epoxy resin and the corrosion inhibitor described in the embodiments of the present application are 95%-99% and 1%-5%, respectively.

[0012] The present application also provides a method for preparing an anti-flash rust waterborne epoxy resin, comprising:

[0013] Dissolving the corrosion inhibitor: adding an organic solvent to the corrosion inhibitor, stirring and heating in a hot water bath until the corrosion inhibitor is completely dissolved to obtain a corrosion inhibitor mixed solution;

[0014] Graft copolymerization reaction: add the epoxy resin into the reactor, start heating and stirring at the first stirring speed, when the epoxy resin is heated to the reaction temperature and the temperature is kept constant, add the above corrosion inhibitor mixed solution dropwise into the epoxy resin, and start timing after the addition is completed until the reaction is complete to obtain a resin reaction solution;

[0015] Emulsification: add deionized water to the above reaction solution, adjust the heating temperature until the temperature in the reactor drops to the emulsification reaction temperature, add emulsifier until the emulsifier is completely melted, add deionized water, stir at the second stirring speed until the reaction is complete, and obtain a water-based epoxy emulsion.

[0016] As a further preferred scheme, in the process of dissolving the corrosion inhibitor described in the embodiment of the present application, the temperature of the hot water bath is 75°C-85°C; in the graft copolymerization reaction, the reaction temperature is 95°C-110°C; and the emulsification reaction temperature is 60°C-70°C.

[0017] As a further preferred solution, the first stirring speed described in the embodiment of the present application is 300-800 rpm, and the second stirring speed is 1100-1200 rpm.

[0018] The present application also provides an anti-flash rust water-based epoxy resin coating, comprising the following components in percentage by mass:

[0019] The anti-flash rust waterborne epoxy resin described in the embodiment of the present application: 55%-65%,

[0020] Wetting agent: 0.1%-1%,

[0021] Defoaming agent: 0.1%-1%,

[0022] Dispersed color paste: 25%-35%,

[0023] Dispersant: 0.1%-1%,

[0024] Solvent: Balance.

[0025] As a further preferred scheme, the wetting agent described in the embodiment of the present application is one or more of Deqian 469 and TEGO4100; the defoaming agent is one or more of BYK 1789, TEGO 901W, and TEGO902W; the curing agent is one or more of Huntman 38-1 and Westlake6520.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1. The flash rust-proof waterborne epoxy resin described in the present application introduces a group capable of forming a complex with a metal matrix into the resin structure through a grafted corrosion inhibitor, which can effectively reduce the reaction points of metal and water on the metal matrix, thereby achieving the inhibition of flash rust.

[0028] 2. The anti-flash rust water-based epoxy resin described in this application is used in coatings without the need to add additional small molecule anti-flash rust inhibitors. It has excellent anti-flash rust resistance without sacrificing the original mechanical properties of the epoxy resin coating.

[0029] The present invention is further described in detail below in conjunction with specific implementation modes and accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1This is a Fourier infrared spectrum of the anti-flash rust waterborne epoxy resin described in the embodiments of the present application.

[0031] Figure 2 This is a gel permeation chromatogram of the anti-flash rust waterborne epoxy resin described in the examples of this application.

[0032] Figure 3 This is a graph showing the change in epoxy value of the anti-flash rust waterborne epoxy resin described in the examples of this application.

[0033] Figure 4 The optimized molecular structure, charge density distribution, and energy density diagram of the anti-flash rust waterborne epoxy resin described in the embodiments of the present application; wherein a is the optimized molecular structure of the ASTA molecule after reacting with the epoxy resin, b is the charge density distribution diagram of the ASTA molecule after the reaction, c is the HOMO energy density distribution of the ASTA molecule after the reaction, and d is the LUMO energy density distribution of the molecule.

[0034] Figure 5 This is a graph showing the results of a flash rust test on a cold-rolled steel plate under normal temperature and humid conditions for the water-based epoxy resin coating described in an embodiment of the present application.

[0035] Figure 6 These are the results of high-temperature and high-humidity flash rust tests on cold-rolled steel plates of the waterborne epoxy resin coating described in the examples of this application.

[0036] Figure 7 It is the surface drying time of the coating of the water-based epoxy resin coating described in the embodiment of the present application on the cold-rolled steel plate; wherein, a is the surface drying time of the cold-rolled steel plate wet-coated at room temperature, b is the flash rust area of ​​the cold-rolled steel plate and the wet coating at room temperature, c is the surface drying time of the cold-rolled steel plate with a high-temperature wet coating, and d is the flash rust area of ​​the cold-rolled steel plate at high temperature and wet coating.

[0037] Figure 8 These are the anti-rust test results of the water-based epoxy resin coating described in the embodiments of the present application on welded steel plates at room temperature, room temperature, and room temperature wet conditions.

[0038] Fig. 9 It is the surface drying time of the coating of the water-based epoxy resin coating described in the embodiment of the present application on the welded steel plate; wherein, a is the surface drying time of the welded steel plate with room temperature and wet coating, b is the flash rust area of ​​the welded steel plate and wet coating at room temperature, c is the surface drying time of the welded steel plate with high temperature and wet coating, and d is the flash rust area of ​​the welded steel plate coated under high temperature and humidity conditions.

[0039] Fig.10 These are the results of a high-temperature and high-humidity anti-rust test on a welded steel plate of a coating of the waterborne epoxy resin coating described in the examples of this application.

[0040] Fig.11These are the experimental results of the neutral salt spray resistance test of the coating of the waterborne epoxy resin coating described in the embodiments of the present application.

[0041] Fig.12 This is the electrochemical impedance spectroscopy test result of the waterborne epoxy resin coating described in the embodiments of the present application.

[0042] Fig.13 This is the electrical equivalent circuit (EEC) model diagram.

[0043] Fig.14 This is a graph showing the thermal stability of the waterborne epoxy resin coating of the present application.

[0044] Fig.15 This is a scanning electron microscope image of the coating of the waterborne epoxy resin coating described in the embodiment of the present application. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in combination with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0046] The term "comprising" and other equivalent descriptions involved in the specification and claims of this application are intended to cover non-exclusive inclusions, including both the contents clearly described in the specification and claims, and the steps or units that are not described in the specification and claims but are inherent in the product, method or structure.

[0047] The embodiment of the present application provides an anti-flash rust waterborne epoxy resin, which is an emulsion obtained by introducing a group capable of forming a complex with a metal matrix into the main structure of the epoxy resin through a grafting reaction between the epoxy resin and the corrosion inhibitor; the group capable of forming a complex with the metal matrix is ​​a thiol group or / and an amino group. Preferably, in order to achieve the purpose of the present application, the epoxy resin is a bisphenol A epoxy resin, and the corrosion inhibitor is a triazole compound of a thiol group or / and an amino group. In the embodiment of the present application, a corrosion inhibitor molecule containing a thiol group or / and an amino group is introduced through a grafting reaction, and there are S and N atoms on the epoxy resin. In the process of preparing the waterborne coating, it is inevitable that -OH and water are combined in large quantities in the form of hydrogen bonds, but in the adsorption process, S and N atoms can preferentially form chemical bonds with Fe to form adsorption, and this process protects the Fe substrate to a certain extent, avoids contact between Fe and water, and thus reduces the occurrence of flash rust. In some specific embodiments, the epoxy resin is one or more of bisphenol A epoxy resin, bisphenol A E-51 epoxy resin, bisphenol A E-44 epoxy resin, bisphenol F E-51 epoxy resin, and bisphenol F E-44 epoxy resin.

[0048] As a further preferred scheme, the corrosion inhibitor described in the embodiment of the present application is one or more of 3-amino-5-mercapto-1,2,4-triazole, 1H-1,2,4-triazole-3-thiol, and 5-(4-pyridyl)-1H-1,2,3-triazole-3-thiol.

[0049] As a further preferred solution, the mass percentages of the epoxy resin and the corrosion inhibitor described in the embodiments of the present application are 95%-99% and 1%-5%, respectively.

[0050] The present application also provides a method for preparing a flash rust-proof waterborne epoxy resin. By this method, the epoxy resin is reacted with a corrosion inhibitor to introduce a group capable of forming a complex with a metal matrix into the structure of the epoxy resin. The preparation method includes:

[0051] Dissolving the corrosion inhibitor: adding an organic solvent to the corrosion inhibitor, stirring and heating in a hot water bath at a temperature of 75°C-85°C until the corrosion inhibitor is completely dissolved to obtain a corrosion inhibitor mixed solution;

[0052] Graft copolymerization reaction: add the epoxy resin into the reactor, start heating and stirring at a speed of 300-800rpm. When the epoxy resin is heated to 95℃-110℃ and the temperature is kept unchanged for 10min, add the above corrosion inhibitor mixture dropwise into the epoxy resin. After the addition is completed, start timing until the reaction is complete to obtain a resin reaction liquid.

[0053] Emulsification: Add deionized water to the above reaction solution, adjust the heating temperature until the temperature in the reactor drops to 60°C-70°C, add emulsifier until the emulsifier is completely melted, then add deionized water, stir at a stirring speed of 1100-1200 rpm until the reaction is complete to obtain a water-based epoxy emulsion.

[0054] The present application also provides an anti-flash rust water-based epoxy resin coating, comprising the following components in percentage by mass:

[0055] The anti-flash rust waterborne epoxy resin described in the embodiment of the present application: 55%-65%,

[0056] Wetting agent: 0.1%-1%,

[0057] Defoaming agent: 0.1%-1%,

[0058] Dispersed color paste: 25%-35%,

[0059] Dispersant: 0.1%-1%,

[0060] Solvent: Balance.

[0061] As a further preferred scheme, the wetting agent described in the embodiment of the present application is one or more of Deqian 469 and TEGO 4100; the defoaming agent is one or more of BYK 1789, TEGO 901W, and TEGO902W; the curing agent is one or more of Huntman 38-1 and Westlake6520.

[0062] Example 1-Example 3

[0063] Example 1-Example 3 provides an anti-flash rust water-based epoxy resin emulsion. The components and amounts used to prepare the anti-flash rust water-based epoxy resin emulsion are shown in Table 1 below.

[0064] The anti-flash rust waterborne epoxy resin emulsion is prepared by the following method:

[0065] Dissolving the corrosion inhibitor: adding an organic solvent to the corrosion inhibitor, stirring and heating in a hot water bath at a temperature of 80° C. until the corrosion inhibitor is completely dissolved to obtain a corrosion inhibitor mixed solution;

[0066] Graft copolymerization reaction: add the epoxy resin into the reactor, start heating and stirring at a speed of 500 rpm. When the epoxy resin is heated to 100°C and the temperature is kept constant for 10 minutes, add the above corrosion inhibitor mixture dropwise into the epoxy resin. After the addition is completed, start timing until the reaction is complete to obtain a resin reaction solution.

[0067] Emulsification: Deionized water was added dropwise to the above reaction solution, the heating temperature was adjusted until the temperature in the reactor dropped to 70°C, an emulsifier was added until the emulsifier was completely melted, deionized water was added dropwise, and the mixture was stirred at a stirring speed of 1100 rpm until the reaction was complete to obtain a water-based epoxy emulsion.

[0068] The flash rust-proof waterborne epoxy resin described in Examples 1-3 reacts as follows:

[0069]

[0070] Comparative Example 1

[0071] This comparative example 1 provides a water-based epoxy resin emulsion, which is prepared according to the steps of the above examples 1-3. The components and amounts of the emulsion are shown in Table 1.

[0072] Table 1: Components and dosages for preparing anti-flash rust waterborne epoxy resin

[0073]

[0074] The anti-flash rust waterborne epoxy resin of Example 1 is named E51-ASTA 1%, the anti-flash rust waterborne epoxy resin of Example 2 is named E51-ASTA 3%, the anti-flash rust waterborne epoxy resin of Example 3 is named E51-ASTA 5%, and the anti-flash rust waterborne epoxy resin of Comparative Example 1 is named E51-ASTA 0%.

[0075] Performance test of waterborne epoxy resin of Examples 1-3 and Comparative Example 1

[0076] 1) Fourier transform infrared spectroscopy characterization

[0077] The chemical structure and groups of the anti-flash rust waterborne epoxy resin emulsion described in Examples 1-3 were characterized using a BRUKER VERTEX70V Fourier transform infrared spectrometer, and the structure of the polymer was characterized by the absorption peak of the special group. The experimental detection range was 4000-450cm -1 The test method is to press a KBr tablet and apply the product on the tablet for testing. The test results are shown in Figure 1 .

[0078] The grafting reaction of epoxy resin is essentially a ring-opening reaction in which the epoxy group is attacked by a nucleophilic group. In this reaction, the primary amine group and the thiol group in 3-amino-5-mercapto-1,2,4-triazole act as nucleophilic groups to attack the epoxy group of the epoxy resin, thereby carrying out a ring-opening reaction. Since 3-amino-5-mercapto-1,2,4-triazole contains a primary amino group, this reaction is also an alkaline self-catalytic ring-opening reaction. Under base catalysis, the O atom of the cyclic ether will not be protonated, and the nucleophile is a negative ion with strong nucleophilic ability. In the transition state, the breaking of the CO bond and the formation of the NC bond occur almost simultaneously. The nucleophilic group selectively attacks the C ring atom with fewer substituents and lower steric hindrance. As can be seen from the infrared spectrum, the transmission peak appears at 3460cm -1 In the four spectra near the wavelength, the peak is formed by the -OH of the epoxy resin itself and the -OH generated during the reaction. In addition, by observing the four spectra, it can be found that the intensity of the peak increases with the increase of ASTA participating in the reaction. This proves to a certain extent that OH is generated in the reaction due to the reaction between the ring opening of the epoxide group and ASTA. Figure 1 As shown in the spectrum at 3400cm -1 -3500cm -1 No characteristic peak of -NH2 was found in the 2500cm-1 mol / L NH2 group. Therefore, it can be confirmed that -NH2 participates in the ring-opening addition reaction of the epoxide group and is -1 The presence of -SH peaks was not detected in the three epoxy resins synthesized by adding ASTA, so it was concluded that -SH participated in the ring-opening addition reaction of the epoxy group and was also completely consumed in the reaction.

[0079] In addition, 2500cm -1 The transmission peak at wavelength is the CH stretching vibration peak in the benzene ring, 915.33cm -1 The transmission peak of the wavelength is the infrared characteristic peak of the epoxy group. In summary, it is proved that -NH2 and -SH react with the epoxy group to generate -NH, -S- and -OH. Since the amount of 3-amino-5-mercapto-1,2,4-triazole added is relatively small and the amount of epoxy group consumed after the reaction is also relatively small, the infrared characteristic peak of the epoxy group appears in the four infrared spectra, but the intensity of the peak can be seen to be slightly reduced in the infrared spectrum. Based on the above characterization data, it can be shown that the primary amino group in 3-amino-5-mercapto-1,2,4-triazole successfully reacts with the epoxy group on the E51 bisphenol A epoxy resin.

[0080] 2) Gel permeation chromatography test

[0081] The molecular weight and molecular weight distribution of the flash rust-proof waterborne epoxy resin were tested by TOSOH brand HLC-8420 gel permeation chromatograph, with tetrahydrofuran as the mobile phase. According to the reaction principle, it can be inferred that after the reaction of E51 bisphenol A epoxy resin and 3-amino-5-mercapto-1,2,4-triazole, its molecular weight will be higher than that of E51 bisphenol A epoxy resin. As the amount of 3-amino-5-mercapto-1,2,4-triazole participating in the reaction increases, the molecular weight of the synthetic resin will also increase, and it will be separated earlier in the gel permeation chromatography test. This gel permeation chromatography test can also verify this conclusion.

[0082] The first separation time of E51-ASTA 0% resin is 12.697 min, the first separation time of E51-ASTA 1% resin is 12.053 min, the first separation time of E51-ASTA 3% resin is 10.925 min, and the first separation time of E51-ASTA 5% resin is 10.462 min.

[0083] From the separation time, it can be seen that the higher the ASTA content involved in the reaction, the earlier the first separation time of the synthetic resin, which means that the molecular weight of the synthetic resin is larger, proving that the amount of ASTA grafted onto the E51 bisphenol A epoxy resin is greater.

[0084] From the GPC data table, we can see that the polydispersity index Mw / Mn of the E51-ASTA X series is relatively large, and the more ASTA participates in the reaction, the larger the polydispersity index is, proving that after the reaction, the molecular weight of the epoxy resin is relatively uniform. Figure 2 and Table 2.

[0085] Table 2: Gel Permeation Chromatography Test

[0086]

[0087] 3) Hydrochloric acid-acetone method titration epoxy value test

[0088] Epoxy value is one of the characteristic data of epoxy resin. Therefore, determining the epoxy value of epoxy resin can effectively determine whether the reaction of the resin is successful. The experiment uses Hiranuma brand MC-3000 model potentiometric titrator and hydrochloric acid-acetone titration method to test the epoxy value of the polymer.

[0089] The epoxy value is the amount of epoxy groups contained in every 100g of epoxy resin, and is the most important indicator for identifying the properties of epoxy resin. Since the basic principle of the grafting reaction is the ring-opening of the epoxy group to undergo an addition reaction, the epoxy value will decrease as the degree of reaction increases. The change in the epoxy value can be used to determine the degree of the reaction and whether the grafting is successful.

[0090] For specific changes in epoxy value, see Figure 3 From the epoxy value test, after the E51 bisphenol A epoxy resin reacted with different amounts of 3-amino-5-mercapto-1,2,4-triazole, the epoxy value of the synthetic resin decreased to varying degrees compared with the epoxy value of the epoxy resin before the reaction. The initial epoxy value of E51-ASTA 0% resin, i.e., E51 bisphenol A epoxy resin, was 0.549. After 7 hours of reaction, the epoxy value of E51-ASTA 1% epoxy resin was 0.484, the epoxy value of E51-ASTA 3% resin was 0.415, and the epoxy value of E51-ASTA 5% resin was 0.398. From the final epoxy value, as the ASTA content involved in the reaction increased, the epoxy value became lower and lower, which proved that the epoxy ring-opening addition reaction did take place during the reaction, and the epoxy group was consumed. At 6-7 hours, the epoxy value test curve tended to be horizontal and basically no longer changed, indicating that the grafting reaction was completed after 7 hours.

[0091] 4) Calculation of corrosion inhibitor front track parameters and charge density distribution

[0092] The HOMO energy and LUMO energy of the slow-release agent 3-amino-5-mercapto-1,2,4-triazole (ASTA) and the energy difference between the two were calculated. The results are shown in Tables 3 and 4. The charge density distribution of the corrosion inhibitor was obtained by optimizing the structure of the corrosion inhibitor compound. Figure 4 .

[0093] Table 3: Front track parameters

[0094] Reaction status <![CDATA[E HOMO / eV]]> <![CDATA[E LUMO / eV]]> ΔE / eV Before reaction -0.16772 -0.02365 0.14357 After the reaction -0.18099 -0.02472 0.15627

[0095] Figure 4 a is the optimized molecular structure of ASTA molecules after reacting with epoxy resin. Figure 4 b is the charge density distribution diagram of the ASTA molecule after the reaction. From this figure, it can be seen that the charge is distributed evenly on the whole molecule, but there is a larger density distribution around the S atom and the N atom. Figure 4 c is the HOMO energy density distribution of ASTA molecules after the reaction, Figure 4d is the LUMO energy density distribution of the molecule. It can be seen from the figure that the HOMO energy of the molecule is mainly distributed on the S atom and the N atom and the 1, 2, 4 triazole ring. Therefore, the corrosion inhibitor molecule is more inclined to form adsorption with the iron matrix surface with these three functional groups. From the change of HOMO energy before and after the reaction of the ASTA molecule in Table 3, the HOMO energy of the molecule is significantly increased after the reaction, the electron donating ability of the molecule is enhanced, and the orbital energy difference is also significantly reduced, and the reactivity of the molecule is also enhanced. Therefore, it can be proved that the adsorption ability and reactivity of the ASTA molecule are still very strong after the reaction, and the molecule is easily adsorbed with the carbon steel surface. This is also the reason why the ASTA molecule has a good anti-flash rust effect. Table 4 lists the calculated nucleophilic Fukui index f- and electrophilic Fukui index f+ of each atom on the ASTA molecule after the reaction. For this molecule, the N atom of the amino group has the largest nucleophilic Fukui index, followed by the S atom of the thiol group. The nucleophilic Fukui index of these two atoms is much larger than that of other atoms in the molecule. It can be inferred that the N atom and the S atom are the active sites of the nucleophilic reaction in the molecule. When interacting with the carbon steel surface, the N atom and the S atom provide electrons to bond with the Fe atom and adsorb on the carbon steel surface. At the same time, the S atom has the largest electrophilic Fukui index of all the atoms in the molecule, indicating that the S atom has a very strong electrophilic ability and is more likely to accept the negative charge from the carbon steel surface, thereby bonding and adsorbing to inhibit corrosion.

[0096] Table 4: Fukui function calculation results of reaction state

[0097]

[0098]

[0099] Application Examples 1-3

[0100] The anti-flash rust waterborne epoxy resin described in the above Examples 1-3 is made into a varnish, and the composition of the varnish is shown in Table 2 below, wherein the anti-flash rust waterborne epoxy resin used in Application Examples 1-3 corresponds to the anti-flash rust waterborne epoxy resin obtained in Examples 1-3, respectively.

[0101] In Application Examples 1-3, 63 g of anti-flash rust water-based epoxy resin, 30 g of white water-based super-dispersible color paste (Kodi super-dispersible color paste S series), 6 g of solvent PM (propylene glycol methyl ether), 0.2 g of wetting agent (Tego 4100), 0.3 g of defoaming agent (Tego Foamex822), and 0.5 g of dispersant (Allnex vxw6208) were used.

[0102] The preparation method of the varnish is as follows:

[0103] The anti-flash rust water-based epoxy resin emulsion was stirred at a speed of 1000 rpm using a high-speed disperser, and then the solvent, defoamer and white water-based super-dispersible color paste were gradually added to the emulsion in proportion while dispersing and adding, and stirred at a speed of 1200 rpm for 15 minutes using a high-speed disperser. The obtained paint was filtered through a gauze to obtain the varnish corresponding to Application Examples 1-3.

[0104] Comparative Examples 2-5

[0105] In Comparative Examples 2-5, varnishes were prepared according to the steps of Application Examples 1-3, except that the water-based epoxy resin emulsion and the anti-flash rust agent (Raybol 60) described in Comparative Example 1 were mixed to replace the anti-flash rust water-based epoxy resin. The mass percentages of the water-based epoxy resin emulsion and the anti-flash rust agent (Raybol 60) in Comparative Examples 2-5 are shown in Table 5 below.

[0106] Table 5: Composition of Comparative Examples 2-4

[0107]

[0108] The varnish obtained in the above-mentioned application examples 1-3 and comparative examples 2-5 was added with a curing agent (Westlake 6520) and deionized water, and then stirred at a speed of 700 r / min for 5 minutes using a constant speed mixer to obtain a coating.

[0109] Coating performance test

[0110] 1. Anti-flash rust performance test of coatings on different substrates

[0111] 1) Anti-flash rust performance test of coating on cold-rolled steel plate

[0112] The anti-flash rust performance of the coatings formed by the varnishes of Application Examples 1-3 and Comparative Examples 1-4 was tested in two different environments, mainly to test the effects of different construction environments on the anti-flash rust performance of the coatings. The two environments were a normal temperature and humidity environment (23±2°C, 55%±2%RH) and a high temperature and humidity environment (47±2°C, 98%±2%RH). A total of 4 groups of anti-flash rust performance test experiments were conducted.

[0113] Since there is a lack of data to make a strong judgment on the flash rust condition of the coating by direct visual observation, the following method is used to evaluate the anti-flash rust performance of the coating. The standard is based on ASTM D 610-85.

[0114] The specific evaluation method is to capture the area of ​​the coating in the photo after taking a photo of the coating, scan the photo, select the area of ​​the coating occupied by the rust spots in the photo, calculate the ratio of the pixels occupied by the rust spot area to the total pixels of the coating photo, and obtain the percentage of the rust spot area in each coating to the coating surface area, and use this percentage to evaluate the anti-flash rust performance of the coating. This evaluation method refers to the method used by the American Society for Testing and Materials to evaluate the flash rust situation of the coating surface, and Table 6 is the evaluation standard of this evaluation method.

[0115] Table 5: ASTM D 610-85 method evaluation system

[0116] Corrosion degree (%) Evaluation Index Corrosion degree (%) Evaluation Index <0.01 100 — 45 — 95 10 40 0.03 90 — 35 — 85 16 30 0.1 80 — 25 — 75 33 20 0.3 70 — 15 — 65 50 10 1 60 — 5 — 55 100 0 3 50

[0117] In order to test the anti-flash rust performance of the synthetic coating under different substrates and different scenarios in actual applications, this experiment used two substrates, cold-rolled steel plates and Q235 welded steel plates, to test the anti-flash rust of the coating, and set up two different anti-flash rust test environments. They are normal temperature and humidity (23±2℃, 50%±5%RH) and high temperature and high humidity environment (45±2℃, 98%±2%RH). Among them, the anti-flash rust test of the welded steel plate simulates the substrate that the coating needs to protect in the actual construction environment. After spraying the coating on the steel plate, the steel plate was placed in a wet heat box, and the coating was allowed to stand and dry in this environment. After the spraying was completed, all 7 groups of coatings were immediately placed in the same wet heat chamber to reduce the impact of temperature and humidity changes on the anti-rust performance test.

[0118] It is generally believed that 23℃±2℃ and 98%RH are normal temperature and humidity conditions. In this environment, although the temperature and humidity are relatively low, considering the nature of water-based coatings with water as the main dispersion, flash rust is still prone to occur during the drying process of the coating on the metal substrate. Therefore, it is necessary to test the anti-flash rust performance of the coating under normal temperature and humidity conditions. After spraying, all coatings are dried in a wet heat box for 24 hours and then taken out for observation.

[0119] from Figure 5 It can be seen that the seven groups of coatings sprayed on the cold-rolled steel plate did not show flash rust after drying for 24 hours. The thickness of each group of coatings is as follows Figure 5 As shown, it is shown that the waterborne epoxy coating sprayed on the cold rolled steel plate is not prone to flash rust under normal temperature and humidity conditions. Table 7 shows the evaluation of the anti-flash rust performance of the coating under normal temperature and humidity conditions.

[0120] Table 7: Evaluation of coating anti-flash performance

[0121]

[0122] Figure 6It is a flash rust prevention performance test on cold-rolled steel plates under high temperature and high humidity conditions. The E51-ASTA 0% coating dried under high temperature and high humidity conditions showed severe flash rust, with a flash rust area of ​​4.97%. However, among the coatings tested, the flash rust area of ​​the E51-ASTA1% coating was the smallest, at 0.01%. From the comparison of the flash rust area of ​​various coatings, the E51-ASTA1% coating has the most significant flash rust prevention effect when applied to the substrate in a high temperature and high humidity environment, and its flash rust prevention performance is better than that of the coating with the addition of an anti-flash rust agent. Table 8 shows the evaluation of the anti-flash rust performance of 7 groups of coatings under normal temperature and humidity environments.

[0123] Table 8: Evaluation of coating anti-flash rust performance

[0124] Coating Type Flash rust degree (%) Evaluation Index Application Example 1 0.01 95 Application Example 2 0.73 75 Application Example 3 4.63 73 Comparative Example 2 4.97 45 Comparative Example 3 0.61 65 Comparative Example 4 1.4 55 Comparative Example 5 0.67 65

[0125] from Figure 7 a and Figure 7 From the data of c, it can be seen that compared with drying in a normal temperature and humid environment, the coating dries significantly faster in a high temperature and humid environment, but is more prone to flash rust. The drying time of each group of coatings in a high temperature and humid environment is shorter than that in a normal temperature and humid environment.

[0126] 2) Anti-flash rust performance test of coating on welded steel plate

[0127] Since there may be welding areas on the substrate in the actual engineering construction environment, and the welding areas are also the areas where flash rusting of the water-based coating is more serious, this test is mainly to test the actual application of the coating, mainly to test whether the coating has good anti-flash rusting performance in the weld area and the ordinary steel plate area. The specific test method is: spray the 7 kinds of varnishes of Application Examples 1-3 and Comparative Examples 2-5 on the welded steel plate, and then quickly put the welded steel plate into a wet heat box with set temperature and humidity for drying, and take it out after 24 hours to observe the flash rusting situation. The coating spray thickness is 20±5μm.

[0128] The final test results of the 7 varnishes in the room temperature and humidity anti-flash rust performance test are as follows Figure 8 As shown. Under normal temperature and humidity conditions, small rust spots will appear on some coatings, which are difficult to observe with the naked eye. Therefore, during the observation process, an ultra-depth-of-field microscope is used to magnify the coating surface to facilitate the observation of rust spots on the coating surface.

[0129] Figure 8It can be seen that after the 7 groups of coatings are dried, the percentage of rust spot area to the total coating area. Under a microscope, it was found that no flash rust was found in the coating of Application Example 1 (E51-ASTA 1%), the coating of Comparative Example 3 (E51-Raybol 0.1%), the coating of Comparative Example 4 (E51-Raybol 0.5%) and the coating of Comparative Example 5 (E51-Raybo 1.0%). The flash rust areas of the coatings of Comparative Example 2 (E51-ASTA 0%), Application Example 2 (E51-ASTA 3%) and Application Example 3 (E51-ASTA 5%) were 0.26%, 0.23% and 0.26%, respectively. Table 9 provides an evaluation of the anti-flash rust performance of various coatings at room temperature and humidity.

[0130] Table 9: Evaluation of coating anti-flash rust performance at room temperature and humidity

[0131]

[0132] Since the surface drying time of the coating after spraying indirectly affects the anti-flash rust performance of the coating, and also indirectly reflects the anti-flash rust performance of the coating, the coating surface drying time test is also an important part of the anti-flash rust test process. The coating surface drying time test results are shown in Fig. 9 . The surface drying time of the 7 groups of coatings is as follows Fig. 9 As shown in a. The surface drying time of the coating of Comparative Example 2 in a normal temperature and humid environment is 41 minutes, which is the coating that achieves the slowest surface drying in a normal temperature and humid environment. Ordinary water-based epoxy coatings dry slowly without adding anti-flash rust agents, which increases the contact time between the substrate and the water in the water-based coating, and flash rust is prone to occur. The coating of Application Example 3 reaches surface drying within 27 minutes, the coating of Application Example 2 reaches surface drying within 32 minutes, and the coating of Application Example 1 reaches surface drying within 39 minutes. It can be seen that the drying speed of the three groups of coatings prepared by modified epoxy resin is much faster than that of the coating of Comparative Example 2, and the more ASTA is added in the modification, the faster the surface drying speed. The coating of Comparative Example 5 reaches surface drying within 30 minutes. This is the coating with the addition of a rust inhibitor, and it reaches the fastest surface drying. The coating of Comparative Example 4 reaches surface drying within 35 minutes, and the coating of Comparative Example 5 reaches surface drying within 38 minutes. This is the coating with the addition of an anti-flash rust inhibitor that reaches the slowest surface drying. From the three groups of paints with anti-flash rust agent added, it can be seen that adding anti-flash rust agent can also increase the drying speed of the paint. The more anti-flash rust agent is added, the faster the coating dries and the faster its surface dries.

[0133] Under normal temperature and humidity conditions, flash rust of the coating is not serious, because the air humidity and temperature of the construction environment are relatively low. Under such temperature and humidity conditions, the coating is not prone to flash rust. However, when the coating is used in actual construction, the high temperature and high humidity environment of some construction sites will be worse than the normal temperature and humidity environment. Under high temperature and high humidity conditions, the coating is also more prone to flash rust, so the anti-flash rust performance of the coating in high temperature and high humidity environments is particularly important.

[0134] Fig.10 The final test results of 7 groups of coatings participating in the high temperature and high humidity anti-flash rust performance test are shown. Fig. 9 As can be seen in b, the percentage of rust spot area of ​​the seven groups of coatings to the total coating area after drying. Fig. 9 a and Fig. 9 b It can be seen that under high temperature and high humidity environment, as the time required to achieve surface drying increases, the proportion of rust spots on the coating to the total coating area also increases.

[0135] Among them, the number of rust spots on the surface of the coating of comparative example 2 is large, but the area of ​​rust spots is small, accounting for 3.84% of the total coating area; the number of rust spots on the surface of the coating of application example 1 is small, the area of ​​rust spots is small, accounting for 0.22% of the total coating area. The surface rust spots of the coating of application example 2 are significantly larger than those of the first two coatings, and the number is large. The surface rust spots of the coating of application example 3 and application example 2 are similar to the surface rust spots of the coating of application example 3. The surface area rust spots of the coating of application example 3 are dense and large, and the surface rust spots of the coating of application example 3 account for 6.47% of the total surface coating. In the high temperature and high humidity anti-flash rust experiment, the performance of the three groups of layers coated with anti-flash rust agents is also poor. The rust spots of the E51 Raybol 0.1% coating only appear in the edge area, but the rust spots are large in shape, and the area of ​​rust spots accounts for 2.82% of the total coating area. The E51 Raybol 0.5% coating has the worst anti-rust effect, with rust spots all over the coating surface, and the area of ​​rust spots is large, accounting for 15.24% of the total coating area. The rust spots on the E51Raybol 1.0% coating are irregular in size. The main area is the edge of the coating, and the rust spot area accounts for 4.51% of the total coating area. Table 10 shows the flash rust performance scores of each group of coatings under high temperature and high humidity conditions.

[0136] Table 10: Flash rust performance under high temperature and high humidity conditions

[0137]

[0138] from Fig. 9It can be seen from Figures 9a and 9c that the surface drying time of each group of coatings under high temperature and high humidity conditions is shorter than the time to reach surface drying under normal temperature and high humidity. On the one hand, the surface drying time of the modified coating will also decrease with the increase of the amount of ASTA involved in the modification process. On the other hand, as the amount of flash rust inhibitor added to the coating increases, the corresponding surface drying time of the coating will also decrease, showing the same pattern as the test under normal temperature and humidity.

[0139] From the normal temperature and high humidity anti-flash rust test and the high temperature and high humidity anti-flash rust test, it can be seen that the coating of Application Example 1 exhibits good anti-flash rust performance in both environments. It can play an anti-flash rust role on both Q235 steel plates and carbon steel weldments. Among them, it can achieve a rust-free surface of the steel plate at normal temperature and humidity, and can also achieve a better anti-flash rust effect than adding an anti-flash rust agent in a high temperature and high humidity environment.

[0140] 2. Neutral salt spray test of coating

[0141] The coatings formed by Application Examples 1-3 and Comparative Examples 2-5 were placed in a salt spray test box containing a 5% sodium chloride saline solution for several days to observe the corrosion damage of the coatings. The corrosion level of the coatings in the salt spray resistance test was evaluated according to the coating damage evaluation standard in GB / T 1766-2008. The coating thickness was 100±10 μm.

[0142] Fig.11 The experimental results of the neutral salt spray resistance test of various types of coatings are shown. By observing these figures, it can be observed that after being placed in the neutral salt spray resistance test box for 24 hours, a large number of bubbles have appeared on the surface of the coating of Comparative Example 2 (E51-ASTA 0%), while the three groups of coatings with application strengths 1-3 are still intact. At 48 hours of the experiment, bubbles began to appear on the coating of Application Example 2 (E51-ASTA 3%) and the coating of Application Example 3 (E51-ASTA 5%), while the coating with application strength 1 (E51-ASTA 1%) remained intact. After 72 hours of the experiment, blistering occurred in the coating of Application Example 1. The neutral salt spray resistance test of the coating mainly relies on the anti-corrosion properties of its resin body to test the corrosiveness of salt spray. However, it can still be seen from this test that the anti-flash rust water-based resin has better salt spray resistance than the E51 epoxy resin as a whole. The salt spray resistance of the coating was evaluated, and the evaluation results are shown in Table 11.

[0143] Table 11: Evaluation results of coating salt spray resistance

[0144]

[0145]

[0146] 3. Electrochemical impedance spectroscopy test

[0147] In order to further test and analyze the anti-flash rust and anti-corrosion properties of the coating, the coating was subjected to electrochemical impedance spectroscopy test in 3.5wt% NaCl solution. The electrochemical impedance spectroscopy test was performed using a Gamry Reference 3000 electrochemical workstation with a test frequency of 50-60Hz. The electrolytic cell adopted a three-electrode system, with a platinum electrode as the auxiliary electrode, a saturated calomel electrode as the reference electrode, and the coating sample to be tested as the working electrode. Fig.12 a, 12d, 12g, 12j are Nyquist plots of the coating; 12b, 12e, 12h, 12k, 12c, 12f, 12i, 12l are Bode plots of the coating; Fig.13 The equivalent circuit diagram is shown in Figure 2. The solution used is 3.5% sodium chloride solution.

[0148] It can be seen from the Nyquist diagrams of each coating that the impedance arc radius of the coating of Application Example 1 (E51-ASTA 1%) is significantly larger than that of the other coatings, among which Application Example 1 has the largest impedance arc, and the impedance arc does not change much with the increase of immersion time. The coating of Comparative Example 2 (E51-ASTA 0%) has a relatively large impedance arc before immersion, indicating that the coating has relatively good corrosion resistance when not immersed, but with the increase of immersion time, its impedance arc changes greatly, and generally shows a trend of decreasing, which indicates that the salt water resistance of the coating is poor, and immersion in salt water will cause its corrosion resistance to drop rapidly. Although the impedance arcs of the coating of Application Example 2 (E51-ASTA 3%) and the coating of Application Example (E51-ASTA 5%) do not change much before and after immersion, the impedance arc before immersion is very small, which indicates that the corrosion resistance of these two groups of coatings is poor.

[0149] The EIS test results of the above coatings were further analyzed, and the effect of ASTA on the film-forming properties was evaluated by fitting them to the electrical equivalent circuit (EEC) model. Fig.13 represents the EEC model, Rs represents the solution resistance, Rc represents the coating resistance, CPEc represents the non-ideal capacitance of the coating, Rct represents the charge transfer resistance, and CPEdl represents the non-ideal capacitance of the double electrical layer. Among them, Rc and Rct are two key parameters, which are used to evaluate the effectiveness of the coating in providing corrosion protection. The Rc value is related to the physical barrier performance of the coating, and the Rct value is related to the charge transfer process at the interface between the metal surface and the coating. In general, the higher the Rc and Rct values, the better the corrosion protection.

[0150] Table 12 is the electrochemical equivalent circuit fitting data of the coating. Table 12 shows that the coating of Application Example 1 exhibits the highest Rc value of all coatings before and after immersion, which means that the coating has the best corrosion resistance. Another parameter, the Rct value, also shows a similar trend to the Rc value. The higher Rct value is attributed to the chemical adsorption formed by ASTA on the metal surface. During the dry film formation process, the S and N atoms in ASTA contribute their unshared electron pairs to the empty orbits of the Fe substrate to form adsorption, which inhibits the ability of Fe electron transfer. The significant increase in Rc and Rct values ​​indicates that electron transfer is successfully suppressed and the adsorption of the molecular chain on the metal matrix is ​​enhanced.

[0151] Table 12: Electrochemical equivalent circuit fitting data

[0152]

[0153]

[0154] 4. Mechanical properties test

[0155] The mechanical property tests of the coatings of Application Examples 1-3 and Comparative Example 2 mainly include adhesion test, pencil hardness test, flexibility test, and impact resistance test, wherein the standard for adhesion test refers to "Paints and varnishes - Scratch test" ISO 2049-2007, the standard for pencil hardness test refers to "Paints and varnishes - Determination of paint film hardness by pencil method" ISO 15184-1998 (GB / T 6739-2006), the standard for flexibility test refers to "Determination of paint film flexibility" GB / T1731-1993, and the standard for impact resistance test refers to "Determination of paint film impact resistance" GB / T 1732-93.

[0156] Adhesion test: The adhesion of the coating is tested by a scratch test. The tool is used to cut the paint film horizontally and vertically at an angle of 90° on the prepared coating, and the cutting depth reaches the substrate, and a good grid is formed between the cutting marks. Then the cut area is taped, and the tape is removed to observe the coating shedding. According to ISO 2409-2007 standard, the coating adhesion grade can be divided into 0, 1, 2, 3, 4, and 5 grades from good to bad according to the shedding of the coating cut grid.

[0157] Pencil hardness test: Use pencil scratch method to test the hardness of coating. Use 750g coating hardness tester to judge the different hardness levels of coating according to whether the pencil forms scratches on the coating surface. According to ISO 15184-1998 (GB / T6739-2006) standard, the hardness level of coating is divided into 19 levels from 9H to 9B from hard to soft.

[0158] Coating flexibility test: The coating flexibility test refers to bending and folding the coating sample on shafts of different diameters. The minimum shaft diameter that does not damage the coating after bending and folding is used to express the flexibility of the coating. Under the condition of not damaging the coating, the smaller the shaft diameter used for bending and folding the coating, the better the flexibility of the coating.

[0159] Impact resistance test: The impact resistance of the coating refers to placing the coating on the horizontal stage of the impact resistance tester, then pulling the plumb bob of the impact resistance tester to a certain height, and then releasing the plumb bob to let it impact the coating sample. If the coating sample does not fall off under the impact of the plumb bob at this height, it is judged to have passed the impact resistance test at this height.

[0160] The mechanical properties test results are shown in Table 13.

[0161] Table 13: Mechanical properties test results

[0162]

[0163]

[0164] It can be seen from the mechanical properties test results that the adhesion of the coating of Application Example 1 (E51-ASTA 1%) is one level lower than that of the coating of the comparative example (E51-ASTA 0%), but the hardness of the coating of Application Example 1 is better than that of the coating of Comparative Example 2. In addition, in the 50 cm impact resistance test, neither the forward impact nor the reverse impact caused damage to the coating of Application Example 1. In the coating flexibility test, the flexibility of the coating of Application Example 1 also reached 1 mm bending without damaging the coating.

[0165] 5. Coating thermal stability test

[0166] The thermal stability of the samples was tested using a thermogravimetric analyzer from TA, USA. The experimental atmosphere was nitrogen, the heating rate was 20°C / min, and the temperature range was 30°C to 550°C.

[0167] The thermal stability of E51-ASTA 1% coating and E51-ASTA 10% coating was tested by thermogravimetric analysis. The difference in thermal stability between E51-ASTA 0% coating and E51-ASTA 1%, E51-ASTA 3%, and E51-ASTA 5% coating can be analyzed. Therefore, it can be determined whether the grafting reaction affects the thermal stability of the epoxy coating. The test results can be found in Fig.14 .

[0168] like Fig.14As shown in Figs. 14a and 14b, the coating of Comparative Example 2 (E51-ASTA 0%) has only one thermal decomposition stage, which occurs at 378.76°C, and the decomposition peak is the thermal decomposition peak of E51 bisphenol A epoxy resin, while the coating of Application Example 1 (E51-ASTA-1%) has two thermal decomposition steps, the first stage at 364.67°C, which belongs to the decomposition of ASTA. The second stage, 378.45°C, belongs to the decomposition of E51 epoxy resin. The higher thermal decomposition temperature indicates that the coatings of Application Examples 1-3 have good thermal stability, and also proves that the grafting experiment will not have a significant impact on the thermal stability of the epoxy resin.

[0169] 6. Scanning Electron Microscope Experiment

[0170] The surface morphology of the coating was observed using a scanning electron microscope produced by ThermoFisher, USA.

[0171] Fig.15 The surface microstructure of the coating captured by SEM, Fig.15 a is the microstructure of the coating of comparative example 2 (E51-ASTA 0%), in which the pore size is 7.760 μm, which is relatively large, so water and air can easily contact the substrate surface through the pores. Fig.15 b is the microstructure of the coating of application example 1 (E51-ASTA 1%), and it can be seen that the pore structure is significantly reduced and the pore size is smaller. The pore size in the picture is 692.2nm, so direct contact between water and air and the substrate is avoided, thereby avoiding the occurrence of flash rust. Fig.15 c is the microstructure of the coating of Example 2 (E51-ASTA 3%), with a pore size of 1.005 μm. It can be seen from the figure that its pore structure is larger and denser than the pore structure in the coating of Example 1. Fig.15 d shows the microscopic surface morphology of the coating of Application Example 3 (E51-ASTA 5%), which obviously has more porous structure, dense pores and large pore size. The pore size in the figure is 2.613μm, and its anti-flash rust performance is not good. The white spots in the photo are white pastes added during the paint preparation process to facilitate the observation of flash rust of the coating. Since the white paste is a mixture of white powder and water, it is granular under the observation of SEM photos.

[0172] From the surface microstructure of the coating, the pore structure diameter of the coating of Comparative Example 1 is the largest, so it increases the contact between the substrate and the air, which is more likely to cause flash rust on the substrate. Although other coatings also have pore structures, the pore diameters are smaller, so the larger the pore diameter on the coating surface, the more likely it is to cause flash rust.

[0173] The components listed in the present invention, as well as the upper and lower limits and interval values ​​of the components of the present invention can realize the present invention, and the embodiments are not listed one by one here. Some specific embodiments are listed above to illustrate the present invention. It is necessary to point out here that the above and below specific embodiments are only used to further illustrate the present invention and do not represent a limitation on the protection scope of the present invention.

Claims

1. A flash rust-proof waterborne epoxy resin, characterized in that: The emulsion is obtained by introducing groups capable of forming a complex with a metal matrix into the main structure of the epoxy resin through a grafting reaction between the epoxy resin and the corrosion inhibitor; the groups capable of forming a complex with the metal matrix are mercapto groups and / or amino groups.

2. The flash rust-proof waterborne epoxy resin according to claim 1, characterized in that: The epoxy resin is one or more of bisphenol A epoxy resin, bisphenol A E-51 epoxy resin, bisphenol A E-44 epoxy resin, bisphenol F E-51 epoxy resin and bisphenol F E-44 epoxy resin.

3. The anti-flash rust waterborne epoxy resin according to claim 1, characterized in that: The corrosion inhibitor is one or more of 3-amino-5-mercapto-1,2,4-triazole, 1H-1,2,4-triazole-3-thiol, and 5-(4-pyridyl)-1H-1,2,3-triazole-3-thiol.

4. The flash rust-proof waterborne epoxy resin according to claim 1, characterized in that: The mass percentages of the epoxy resin and the corrosion inhibitor are 95%-99% and 1%-5% respectively.

5. A method for preparing the flash rust-proof waterborne epoxy resin according to claim 1, characterized in that: include Dissolving the corrosion inhibitor: adding an organic solvent to the corrosion inhibitor, stirring and heating in a hot water bath until the corrosion inhibitor is completely dissolved to obtain a corrosion inhibitor mixed solution; Graft copolymerization reaction: add the epoxy resin into the reactor, start heating and stirring at the first stirring speed, when the epoxy resin is heated to the reaction temperature and the temperature is kept constant, add the above corrosion inhibitor mixed solution dropwise into the epoxy resin, and start timing after the addition is completed until the reaction is complete to obtain a resin reaction solution; Emulsification: add deionized water to the above reaction solution, adjust the heating temperature until the temperature in the reactor drops to the emulsification reaction temperature, add emulsifier until the emulsifier is completely melted, add deionized water, stir at the second stirring speed until the reaction is complete, and obtain a water-based epoxy emulsion.

6. The preparation method according to claim 5, characterized in that: During the dissolution of the corrosion inhibitor, the temperature of the hot water bath is 75°C-85°C; during the graft copolymerization reaction, the reaction temperature is 95°C-110°C; and the emulsification reaction temperature is 60°C-70°C.

7. The preparation method according to claim 1, characterized in that: The first stirring speed is 300-800 rpm, and the second stirring speed is 1100-1200 rpm.

8. An anti-flash rust water-based epoxy resin coating, characterized in that: Contains the following components in mass percentage: The anti-flash rust water-based epoxy resin described in any one of claims 1 to 4: 55%-65%, Dispersed color paste: 25%-35%, Wetting agent: 0.1%-1%, Defoaming agent: 0.1%-1%, Dispersant: 0.1%-1%, Solvent: Balance.

9. The anti-flash rust waterborne epoxy resin coating according to claim 8, characterized in that: The wetting agent is one or more of Deqian 469 and TEGO 4100; the defoaming agent is one or more of BYK 1789, TEGO 901W, and TEGO902W; and the curing agent is one or more of Huntman 38-1 and Westlake 6520.

Citation Information

Cited By

  • Method and device for analyzing antirust performance test data of metal product

    CN119092023A