Vehicle-mounted optical film and preparation method thereof
By using silicon dioxide-titanium dioxide composite particles and silicone diffusion particles in vehicle-mounted optical films, the surface hardness and ultraviolet resistance of the optical film are improved, and the problems of low optical brightness and insufficient durability in the prior art are solved, so as to achieve Higher brightness uniformity and longer service life.
Patent Information
- Application Number
- CN202411145309.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-01
AI Technical Summary
The existing vehicle-mounted optical films have problems such as low optical brightness, low surface hardness and poor durability, and are susceptible to ultraviolet wear and degradation, which affects the use effect.
Silica-titanium dioxide composite particles and silicone diffusion particles are used as the main components of the composite coating. The photocatalytic properties of titanium dioxide decompose organic pollutants to improve self-cleaning effect, and utilize the low refractive index of silica and silicone. The scattering effect improves the brightness and UV resistance of the optical film, while enhancing surface hardness and wear resistance.
It improves the surface hardness, wear resistance and UV resistance of the optical film, enhances brightness and brightness uniformity, extends service life, and reduces wear and scratches of the optical film.
Smart Images

Figure BDA0005002035410000071
Abstract
Description
Technical Field
[0001] The present application relates to the field of optical films, and in particular to a vehicle-mounted optical film and a preparation method thereof. Background Art
[0002] With the rapid development of the automobile industry, the in-vehicle display system has become an important part of improving the driving experience. However, these flat panel displays do not emit light themselves. The light source of the picture is provided by the backlight module, and the light source needs to meet the requirements of uniformity and high brightness. The existing optical film mainly adopts coated optical film, which has the advantages of high light transmittance, large haze adjustment range and good appearance quality.
[0003] However, existing optical films have problems such as low optical brightness, low surface hardness, and poor durability. Long-term exposure to ultraviolet rays can easily cause wear and degradation, which in turn causes deformation of the optical film and affects its use. Summary of the invention
[0004] In order to improve the brightness and durability of a vehicle-mounted optical film, the present application provides a vehicle-mounted optical film and a preparation method thereof.
[0005] In a first aspect, the present application provides a vehicle-mounted optical film, which adopts the following technical solution: A vehicle-mounted optical film comprises a substrate and a composite coating, wherein the composite coating comprises the following raw materials in parts by weight: 40-50 parts of acrylate resin, 5-8 parts of diffusion particles, 8-15 parts of composite nanoparticles, and 3-5 parts of photoinitiator; the composite nanoparticles are silicon dioxide-titanium dioxide composite particles.
[0006] By adopting the above technical scheme, silicon dioxide and titanium dioxide have high strength, chemical stability and wear resistance, which can improve the surface hardness, wear resistance and impact resistance of the optical film and reduce the performance attenuation caused by environmental factors. The good photocatalytic performance of titanium dioxide can decompose organic pollutants, promote the optical film to have a good self-cleaning effect, and improve the brightness and UV resistance of the optical film. At the same time, low-refractive-index silicon dioxide can neutralize a part of the high-refractive index of titanium dioxide, so that the composite coating has good light transmittance and brightness uniformity. Titanium dioxide can be loaded into the porous structure of silicon dioxide, and silicon dioxide can play a role of filling and supporting, thereby improving the dispersibility of titanium dioxide. The use of diffusion particles can scatter the incident light, promote multiple scattering of light in the optical film, promote a more uniform distribution of light, reduce hot spots and dark areas, and thus improve the overall brightness and brightness uniformity of the optical film.
[0007] Preferably, the substrate is one of polycarbonate, polyethylene terephthalate and polymethyl methacrylate.
[0008] By adopting the above technical solution, polycarbonate, polyethylene terephthalate, and polymethyl methacrylate as the optical film substrate can make the optical film maintain a high light transmittance, which is conducive to the full passage of light and improves the overall brightness of the optical film. At the same time, polycarbonate and polyethylene terephthalate can maintain high strength and impact resistance under long-term use, reduce damage to the optical film during processing and use, and maintain the brightness and strength of the optical film.
[0009] Preferably, the diffusion particles are organic silicon diffusion particles, and the particle size of the diffusion particles is 0.1-1 μm.
[0010] By adopting the above technical solution, the organic silicon diffusion particles can be evenly distributed in the composite layer of the optical film, reducing the aggregation phenomenon of traditional diffusion particles and reducing the unevenness of light scattering, thereby improving the brightness and brightness uniformity of the optical film. Organic silicon diffusion particles have a high refractive index and chemical stability, which enhances the scattering effect of light and reduces the impact of environmental changes on the optical film. At the same time, organic silicon diffusion particles have good compatibility with the optical film substrate and can be firmly combined with the substrate to improve the brightness uniformity and brightness of the optical film.
[0011] Preferably, the method for preparing the organosilicon diffusion particles comprises the following specific steps: pre-dispersing the inorganic particles in an aqueous solution of a dispersant, stirring evenly, adjusting to acidity, then adding a non-polar organosilane monomer to mix to form a hydrolyzate, then adjusting the hydrolyzate to alkalinity, heating to react, forming organosilicon resin microspheres, then mixing the organosilicon resin microspheres with a polar organosilane monomer, stirring evenly, and drying to obtain organosilicon diffusion particles.
[0012] By adopting the above technical solution, by coating the inorganic particles inside the organosilicon, it is possible to cause a certain degree of reflection on the surface of the inorganic particles when the light passes through the organosilicon, thereby enhancing the scattering effect of the light, thereby improving the brightness and brightness uniformity of the optical film. The organosilane is hydrolyzed and polycondensed on the surface of the inorganic particles to block water and oxygen, and the inorganic particles are wrapped inside, so that the prepared organosilicon diffusion particles can be evenly dispersed on the surface of the substrate, reducing the agglomeration of the organosilicon diffusion particles, thereby improving the brightness and brightness uniformity of the optical film.
[0013] Preferably, the mass ratio of the inorganic particles, the non-polar organosilicon monomer, and the polar organosilicon monomer is (5-8):100:(5-10).
[0014] By adopting the above technical solution and adjusting the mass ratio of inorganic particles, non-polar silicone monomers, and polar silicone monomers within an appropriate range, the inorganic particles can be made to maintain good strength and structural stability in the diffusion particle system. The non-polar silicone monomer forms a silicone protective layer on the surface of the inorganic particles. Using a larger mass of non-polar silicone monomers can make the protective layer have good durability, chemical stability and strength, thereby increasing the stability and strength of the diffusion particles. The polar silicone monomer can interact with the non-polar silicone monomer to adjust the dispersibility of the silicone diffusion particles in the composite coating system, and maintain the optical film with good luminance and brightness uniformity.
[0015] Preferably, the inorganic particles are at least one of barium sulfate, calcium carbonate and zinc oxide.
[0016] By adopting the above technical solution, barium sulfate, calcium carbonate and zinc oxide can improve the light transmittance of the optical film, make the light propagate more evenly in the film layer, effectively scatter the light, and thus improve the brightness and brightness uniformity of the optical film. At the same time, barium sulfate, calcium carbonate and zinc oxide have high hardness and strength, enhance the wear resistance and impact resistance of the optical film, and improve the durability of the optical film.
[0017] Preferably, the non-polar silicone monomer is one of methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, and propyltriethoxysilane; and the polar silicone monomer is one of methacryloxypropyltrimethoxysilane, methacryloxypropyltriethoxysilane, glycidyloxypropyltrimethoxysilane, glycidyloxypropyltriethoxysilane, acryloxypropyltrimethoxysilane, and acryloxypropyltriethoxysilane.
[0018] Preferably, the heating reaction temperature is 40-60°C.
[0019] In a second aspect, the present application provides a method for preparing a vehicle-mounted optical film, which adopts the following technical solution: A method for preparing a vehicle-mounted optical film comprises the following specific steps: The titanium dioxide sol is surface-modified using an epoxy silane coupling agent in advance, and after heating and aging, modified titanium dioxide is obtained. The silicon dioxide sol is hydrophobically modified using methyltrichlorosilane to obtain modified silicon dioxide. The modified silicon dioxide is mixed with 3-aminopropyltriethoxysilane, heated to 30-40° C. for reaction for 5-6 hours, and then the modified titanium dioxide is added, stirred for reaction, and silicon dioxide-titanium dioxide composite particles are obtained after aging; Acrylate resin, diffusion particles, composite nanoparticles, photoinitiator and solvent are mixed and stirred evenly to form a composite coating mixture, the composite coating mixture is coated on the surface of the substrate, and a composite coating is formed after drying, and molding and curing are performed in sequence on the surface of the composite coating to obtain a vehicle-mounted optical film.
[0020] By adopting the above technical solution, through the synergistic effect of various components, the optical film can have better brightness and strength, reduce the wear and scratches of the optical film, and improve the durability of the optical film.
[0021] Preferably, the mass ratio of modified titanium dioxide to modified silicon dioxide in the silicon dioxide-titania composite particles is (3-5):1.
[0022] In summary, this application has the following beneficial effects: 1. Since the present application uses silicon dioxide and titanium dioxide to compound, it can improve the surface hardness, impact strength and chemical stability of the optical film, while maintaining the optical film with good brightness and UV resistance uniformity. At the same time, the diffusion particles are used to reduce the hot spots and dark areas of the optical film, and improve the brightness and brilliance of the optical film.
[0023] 2. Inorganic particles are coated inside the organic silicon to form organic silicon diffusion particles. The strength of the inorganic particles can be used to improve the strength and structural stability of the diffusion particles, enhance the light scattering effect, and thus improve the brightness and brightness uniformity of the optical film. At the same time, the surface of the organic silicon diffusion particles is compounded with polar organic silicon monomers, which can improve the dispersibility of the diffusion particles in the composite coating system, thereby improving the brightness and brightness uniformity of the optical film. DETAILED DESCRIPTION
[0024] The present application is further described in detail below with reference to the embodiments.
[0025] All raw materials in the examples are commercially available.
[0026] Preparation Example of Silicone Diffusion Particles Preparation Example 1 The raw materials of the organosilicon diffusion particles include inorganic particles, non-polar organosilicon monomers, and polar organosilicon monomers, and the mass ratio of the inorganic particles, the non-polar organosilicon monomers, and the polar organosilicon monomers is 7:100:8. The inorganic particles are barium sulfate, the non-polar organosilicon monomers are methyltrimethoxysilane, the polar organosilicon monomers are methacryloxypropyltrimethoxysilane, and the average particle size of the inorganic particles is 0.05-0.08 μm.
[0027] The method for preparing organic silicon diffusion particles comprises the following specific steps: The inorganic particles are pre-dispersed in a sodium hexametaphosphate aqueous solution as a dispersant, stirred evenly, and the pH is adjusted to 4.5 with hydrochloric acid. Then, a non-polar organosilane monomer is added and mixed, stirred evenly to form a hydrolyzate. Then, the pH of the hydrolyzate is adjusted to 11 with ammonia water, heated to 50°C, and reacted for 4 hours to form silicone resin microspheres. Then, the silicone resin microspheres are mixed with the polar organosilane monomer, stirred evenly, and dried to obtain silicone diffusion particles.
[0028] Preparation Example 2 The difference between Preparation Example 2 and Preparation Example 1 is that the mass ratio of inorganic particles, non-polar organic silicon monomer, and polar organic silicon monomer in the organic silicon diffusion particle raw material is 5:100:10.
[0029] Preparation Example 3 The difference between Preparation Example 3 and Preparation Example 1 is that the mass ratio of inorganic particles, non-polar organic silicon monomer, and polar organic silicon monomer in the organic silicon diffusion particle raw material is 8:100:5.
[0030] Preparation Example 4 The difference between Preparation Example 4 and Preparation Example 1 is that the inorganic particles in the raw material of the organic silicon diffusion particles are zinc oxide.
[0031] Preparation Example 5 The difference between Preparation Example 5 and Preparation Example 1 is that the non-polar organosilicon monomer in the organosilicon diffusion particle raw material is propyltriethoxysilane.
[0032] Preparation Example 6 The difference between Preparation Example 6 and Preparation Example 1 is that the polar silicone monomer in the raw material of the silicone diffusion particles is acryloxypropyltrimethoxysilane.
[0033] Preparation Example 7 The difference between Preparation Example 7 and Preparation Example 1 is that no polar organosilicon monomer is used in the organosilicon diffusion particle raw material.
[0034] The method for preparing organic silicon diffusion particles comprises the following specific steps: Pre-disperse the inorganic particles in the dispersant aqueous solution, stir evenly, use hydrochloric acid to adjust the pH to 4.5, then add the non-polar organosilane monomer to mix, stir evenly to form a hydrolyzate, then use ammonia water to adjust the pH of the hydrolyzate to 11, heat to 50°C, react for 4 hours, and dry to form organosilicon diffusion particles. Example
[0035] Example 1 This embodiment provides a vehicle optical film, including a substrate and a composite coating, wherein the substrate is a polycarbonate film, the polycarbonate film is a Makrofol polycarbonate film, the average thickness of the substrate is 50 μm, and the composite coating includes the following raw materials in parts by weight: 45 kg of acrylate resin, 7 kg of diffusion particles, 12 kg of composite nanoparticles, and 4 kg of photoinitiator. The acrylate resin is purchased from Changxing Chemical Materials Co., Ltd. EM235, the photoinitiator is 2-hydroxy-2-methyl-1-phenylacetone, the composite nanoparticles are silicon dioxide-titanium dioxide composite particles, the diffusion particles are purchased from ethyltrimethoxysilane of Kebiri Chemical, and the average particle size of the diffusion particles is 0.1-1 μm.
[0036] The method for preparing a vehicle-mounted optical film comprises the following specific steps: S1: diluting the titanium dioxide sol with anhydrous ethanol to form a titanium dioxide solution with a mass fraction of 1% of titanium dioxide, then mixing the titanium dioxide solution with glycidyloxypropyl triethoxysilane, the mass ratio of the titanium dioxide solution to glycidyloxypropyl triethoxysilane is 1:1, stirring evenly, heating to 30°C for reaction for 2h, and then aging at a constant temperature of 25°C for 3d to obtain modified titanium dioxide; diluting silicon dioxide with anhydrous ethanol to form a silicon dioxide solution with a mass fraction of 1% of silicon dioxide, and then The silica solution was mixed with methyltrichlorosilane in a mass ratio of 1:1, and stirred evenly to obtain modified silica; the modified silica and 3-aminopropyltriethoxysilane were mixed, reacted at 30°C for 5 hours, and then modified titanium dioxide was added, the mass ratio of modified silica, 3-aminopropyltriethoxysilane and modified titanium dioxide was 1:0.5:4, and the reaction was continued with heat preservation and stirring for 2 hours, and aged at a constant temperature of 25°C for 3 days to obtain silica-titania composite particles.
[0037] S2: Mix acrylate resin, diffusion particles, composite nanoparticles, photoinitiator and solvent, stir evenly to form a composite coating mixture, apply the composite coating mixture on the surface of the substrate, and form a composite coating with an average thickness of 10 μm after drying, use a structure to emboss a microstructure on the surface of the composite coating, and cure the microstructure under UV light to obtain a vehicle-mounted optical film.
[0038] Example 2 The difference between Example 2 and Example 1 is that the amount of acrylic resin used in the raw material of the vehicle-mounted optical film composite coating is 40 kg, the amount of diffusion particles used is 8 kg, the amount of composite nanoparticles used is 15 kg, and the amount of photoinitiator used is 3 kg.
[0039] Example 3 The difference between Example 3 and Example 1 is that the amount of acrylic resin used in the raw material of the vehicle-mounted optical film composite coating is 50 kg, the amount of diffusion particles used is 5 kg, the amount of composite nanoparticles used is 8 kg, and the amount of photoinitiator used is 5 kg.
[0040] Example 4 The difference between Example 4 and Example 1 is that the substrate of the vehicle-mounted optical film is a polyethylene terephthalate film purchased from Zhonglian Electronic Materials Co., Ltd.
[0041] Example 5 The difference between Example 5 and Example 1 is that the diffusion particles in the raw material of the vehicle-mounted optical film composite coating are derived from Preparation Example 1.
[0042] Example 6 The difference between Example 6 and Example 1 is that the diffusion particles in the raw material of the vehicle-mounted optical film composite coating are derived from Preparation Example 2.
[0043] Example 7 The difference between Example 7 and Example 1 is that the diffusion particles in the raw material of the vehicle-mounted optical film composite coating are derived from Preparation Example 3.
[0044] Example 8 The difference between Example 8 and Example 1 is that the diffusion particles in the raw material of the vehicle-mounted optical film composite coating are derived from Preparation Example 4.
[0045] Example 9 The difference between Example 9 and Example 1 is that the diffusion particles in the raw material of the vehicle-mounted optical film composite coating are derived from Preparation Example 5.
[0046] Example 10 The difference between Example 10 and Example 1 is that the diffusion particles in the raw material of the vehicle-mounted optical film composite coating are derived from Preparation Example 6.
[0047] Embodiment 11 The difference between Example 11 and Example 1 is that the diffusion particles in the raw material of the vehicle-mounted optical film composite coating are derived from Preparation Example 7.
[0048] Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that an equal amount of titanium dioxide is used in the raw material of the composite coating of the vehicle optical film to replace the composite nanoparticles.
[0049] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that an equal amount of silicon dioxide is used in the raw material of the composite coating of the vehicle optical film to replace the composite nanoparticles. Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that no composite nanoparticles are used in the raw materials of the composite coating of the vehicle-mounted optical film.
[0050] Performance testing The following performance tests were performed on the vehicle-mounted optical films provided in Examples 1-11 and Comparative Examples 1-3 of the present application. The specific test results are shown in Table 1.
[0051] Detection Methods 1. Brightness and viewing angle test Take a 21cm*30cm automotive optical film, put the test structure into the backlight module, light it up at 24V, and test its brightness with a luminance meter, the model of which is BM-7 from Japan's TOPCON company. Use the EZContrast viewing angle meter, and the test conditions are in accordance with the YD / T 1067 standard to detect the viewing angle of the optical film.
[0052] 2. Light transmittance Take a 21cm*30cm automotive optical film sample and put it into a haze tester to measure the light transmittance of the sample. The model of the haze tester is: NDH-2000 of Nippon Denshoku Corporation.
[0053] 3. Impact strength The optical film prepared in this application is horizontally fixed on a supporting fixture as a sample, and a marble with a diameter of 11 mm and a weight of 5 g is dropped from various heights h to the center of the sample optical film. The potential energy (mJ) of the steel ball at the critical height h when the film is not broken and when the film is broken is taken as the impact strength.
[0054] Table 1: Performance test results data table It can be seen from the performance test results that the vehicle-mounted optical film prepared in the present application has a high brightness while maintaining good strength.
[0055] By comparing Example 1 with Examples 5-7, it can be seen that Examples 5-7 use different diffusion particles. From the performance test results, it can be seen that the vehicle-mounted optical film prepared by Examples 5-7 has better brightness and better brightness at different viewing angles, and also enables the vehicle-mounted optical film to maintain good strength. It is further explained that the organosilicon diffusion particles prepared by the present application through inorganic particles, non-polar organosilicon monomers, and polar organosilicon monomers can effectively enhance the light scattering effect, and have good dispersibility in the composite coating system, thereby enabling the optical film to have higher brightness and brightness uniformity.
[0056] By comparing Example 5 with Example 11, it can be seen that the polar organic silicone monomer is not used in the raw material of the organic silicone diffusion particles in Example 11. From the performance test results, it can be seen that the brightness and brightness uniformity of the optical film will decrease, and the dispersibility of the organic silicone diffusion particles in the composite coating system will decrease, thereby affecting the strength performance of the optical film. It further illustrates that the polar organic silicone monomer can enhance the compatibility of the organic silicone diffusion particles with the composite coating matrix resin by utilizing its own active groups on the surface of the organic silicone diffusion particles, forming a uniform and smooth composite coating on the surface of the substrate, thereby improving the brightness and brightness uniformity of the optical film.
[0057] By comparing Comparative Examples 1-3 with Example 1, it can be seen that no silicon dioxide is used in the composite nanoparticles of Comparative Example 1, no titanium dioxide is used in the composite nanoparticles of Comparative Example 2, and no composite nanoparticles are used in Comparative Example 3. From the performance test results, it can be seen that the strength and brightness of the optical film are significantly reduced. This may be because without the use of silicon dioxide, the strength and impact resistance of the optical film are limited, and the light transmittance of the optical film is also affected. Using silicon dioxide alone without titanium dioxide is likely to cause the refractive index of the optical film to be lower, thereby affecting the brightness of the optical film. It further illustrates that by compounding silicon dioxide and titanium dioxide, the optical film can maintain a good brightness and strength, and reduce damage to the optical film during processing and use.
[0058] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.
Claims
1. A vehicle-mounted optical film, characterized in that: The invention comprises a substrate and a composite coating, wherein the composite coating comprises the following raw materials in parts by weight: 40-50 parts of acrylate resin, 5-8 parts of diffusion particles, 8-15 parts of composite nanoparticles, and 3-5 parts of photoinitiator; the composite nanoparticles are silicon dioxide-titanium dioxide composite particles.
2. The vehicle-mounted optical film according to claim 1, characterized in that: The substrate is one of polycarbonate, polyethylene terephthalate and polymethyl methacrylate.
3. The vehicle-mounted optical film according to claim 1, characterized in that: The diffusion particles are organic silicon diffusion particles, and the particle size of the diffusion particles is 0.1-1 μm.
4. The vehicle-mounted optical film according to claim 3, characterized in that: The preparation method of the organosilicon diffusion particles comprises the following specific steps: pre-dispersing inorganic particles in a dispersant aqueous solution, stirring evenly, adjusting to acidity, then adding a non-polar organosilane monomer to mix to form a hydrolyzate, then adjusting the hydrolyzate to alkalinity, heating to react, forming organosilicon resin microspheres, then mixing the organosilicon resin microspheres with a polar organosilane monomer, stirring evenly, and drying to obtain organosilicon diffusion particles.
5. The vehicle-mounted optical film according to claim 3, characterized in that: The mass ratio of the inorganic particles, the non-polar organic silicon monomer, and the polar organic silicon monomer is (5-8):100:(5-10).
6. The vehicle-mounted optical film according to claim 5, characterized in that: The inorganic particles are at least one of barium sulfate, calcium carbonate and zinc oxide.
7. The vehicle-mounted optical film according to claim 5, characterized in that: The non-polar silicone monomer is one of methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, and propyltriethoxysilane; the polar silicone monomer is one of methacryloxypropyltrimethoxysilane, methacryloxypropyltriethoxysilane, glycidyloxypropyltrimethoxysilane, glycidyloxypropyltriethoxysilane, acryloxypropyltrimethoxysilane, and acryloxypropyltriethoxysilane.
8. The vehicle-mounted optical film according to claim 3, characterized in that: The heating reaction temperature is 40-60°C.
9. A method for preparing a vehicle-mounted optical film according to any one of claims 1 to 8, characterized in that: The specific steps include: The titanium dioxide sol is surface-modified using an epoxy silane coupling agent in advance, and after heating and aging, modified titanium dioxide is obtained. The silicon dioxide sol is hydrophobically modified using methyltrichlorosilane to obtain modified silicon dioxide. The modified silicon dioxide is mixed with 3-aminopropyltriethoxysilane, heated to 30-40° C. for reaction for 5-6 hours, and then the modified titanium dioxide is added, stirred for reaction, and silicon dioxide-titanium dioxide composite particles are obtained after aging; Acrylate resin, diffusion particles, composite nanoparticles, photoinitiator and solvent are mixed and stirred evenly to form a composite coating mixture, the composite coating mixture is coated on the surface of the substrate, and a composite coating is formed after drying, and molding and curing are performed in sequence on the surface of the composite coating to obtain a vehicle-mounted optical film.
10. The method for preparing a vehicle-mounted optical film according to claim 9, characterized in that: The mass ratio of modified titanium dioxide to modified silicon dioxide in the silicon dioxide-titania composite particles is (3-5):1.