Heat-conducting silicone rubber material and preparation method thereof
By using thermally conductive silicone rubber materials, an effective thermal conductivity network is formed through hydrogen bonding and electrostatic self-assembly technology, which solves the problem of low bonding strength between inorganic fillers and organic rubber, and significantly improves thermal conductivity and mechanical properties , suitable for the electronics industry.
Patent Information
- Application Number
- CN202411020322.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing thermally conductive silicone rubber materials have poor thermal conductivity due to the low interface bonding strength between inorganic fillers and organic rubber molecules, which limits their application in the electronics industry.
Using thermally conductive reinforced components, the nanocrystals and thermally conductive fillers are prepared by ring-opening reaction and chemical crosslinking. The nanocellulose structure and thermally conductive fillers promote dispersion through hydrogen bonding, and are also produced by nanoalumina and nitriding. The synergistic action of boron forms an effective thermal conductivity network to improve thermal conductivity.
It significantly improves the thermal conductivity and mechanical properties of rubber, enhances the dispersion and compatibility of thermal fillers, forms a continuous thermal conductivity path, and improves the comprehensive performance of the material.
Smart Images

Figure BDA0004967030110000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber preparation, in particular to a thermally conductive silicone rubber material and a preparation method thereof. Background Art
[0002] Silicone rubber-based thermally conductive composite materials can simultaneously meet the requirements of a wide operating temperature range, good elasticity, strong toughness, high thermal conductivity, etc., and also have comprehensive properties that other materials cannot match, and have good application prospects in the electronics industry.
[0003] Rubber materials are poor conductors of heat and electricity, so thermally conductive rubber is often prepared by filling it with thermally conductive fillers. However, since filler particles are often inorganic materials, when filled into an organic rubber matrix, there is no direct bonding between the inorganic filler particles and the rubber molecules, and the interface bonding strength is low, so the thermal conductivity of the rubber composite material is still poor.
[0004] Therefore, the preparation of thermally conductive silicone rubber with high thermal conductivity is of great significance to the development of the domestic electronics industry. Summary of the invention
[0005] The object of the present invention is to provide a thermally conductive silicone rubber material and a preparation method thereof, so as to solve the problems raised in the background technology.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A thermally conductive silicone rubber material, comprising the following raw materials in parts by weight: 100-110 parts of EPDM rubber, 35-45 parts of fluorosilicone rubber, 85-95 parts of carboxyl nitrile rubber, 40-50 parts of a thermally conductive enhancing component, 3-6 parts of a structural control agent, and 1-3 parts of a vulcanizing agent;
[0008] The preparation method of the thermal conductive silicone rubber material comprises the following steps:
[0009] According to weight, EPDM rubber, fluorosilicone rubber, carboxyl nitrile rubber, thermal conductivity enhancing component and structure control agent are added into a kneader, kneaded, and then a vulcanizing agent is added. The mixture is mixed at 162-164° C. for 2.6-3 hours and shaped to obtain a thermally conductive silicone rubber material.
[0010] Furthermore, the shaping process conditions are: firstly use a hot press to hot press for 12-14 minutes at 230-240°C and 15-20MPa, and then transfer to an oven and treat at 260-280°C for 8-10 hours.
[0011] Furthermore, the structure control agent is one or both of hexamethyldisilazane and hydroxy silicone oil mixed in any proportion.
[0012] Furthermore, the vulcanizing agent is any one of dicumyl peroxide and dibenzoyl peroxide.
[0013] Furthermore, the preparation method of the thermal conductivity enhancing component comprises the following steps:
[0014] Step A1, mixing microcrystalline cellulose and a 64% sulfuric acid solution evenly, stirring at 55° C. for 2 hours, adding distilled water to stop the reaction, standing for 4-6 hours, and after the reactant is precipitated, pouring out the supernatant, centrifuging and dialyzing the remaining suspension to neutrality, and freeze-drying at -45° C. to obtain cellulose nanocrystals, wherein the amount ratio of microcrystalline cellulose to sulfuric acid solution is 3g:50-60mL; using microcrystalline cellulose as a raw material, preparing cellulose nanocrystals by sulfuric acid hydrolysis;
[0015] Step A2, adding cellulose nanocrystals to DMF, heating to 45-55°C, stirring evenly, adding epichlorohydrin dropwise, controlling the dropping speed to 3-5 drops / second, heating to 60-70°C after the addition is completed, stirring and reacting for 5-6 hours, and removing excess epichlorohydrin in the reaction solution by vacuum distillation to obtain epoxidized cellulose nanocrystals, wherein the amount ratio of cellulose nanocrystals, DMF and epichlorohydrin is 1.2-1.4g:45-55mL:0.1-0.2mL. In the above reaction process, using DMF as solvent, the active hydroxyl groups on the cellulose nanocrystals react with the chlorine atoms on the epichlorohydrin to undergo nucleophilic substitution reaction to obtain epoxidized cellulose nanocrystals;
[0016] Step A3, ultrasonically dispersing the epoxidized cellulose nanocrystals and DMF, dripping tetrabutylammonium bromide, thermal conductive filler and DMF mixed solution a, heating to 110°C and stirring for 2-3h after the reaction is completed, adding triglycidyl p-aminophenol, continuing to stir for 1-2h, centrifuging, washing the precipitate with 40% ethanol solution for 3-5 times, and drying to obtain a thermal conductivity enhancing component, wherein the amount ratio of epoxidized cellulose nanocrystals, DMF, mixed solution a and triglycidyl p-aminophenol is 0. 6-0.8g:55-65mL:20-30mL:0.2-0.3mL, in the mixed solution a, the amount ratio of tetrabutylammonium bromide, thermal conductive filler and DMF is 0.1-0.2g:0.4-0.6g:20-30mL, in the above reaction process, DMF is used as solvent, under the catalytic action of tetrabutylammonium bromide, the epoxy group on the epoxidized cellulose nanocrystal and the thiol group on the thermal conductive filler undergo a ring-opening reaction, and then triglycidyl p-aminophenol is chemically cross-linked to obtain a thermal conductivity enhancing component.
[0017] Furthermore, the preparation method of the thermal conductive filler comprises the following steps:
[0018] Step B1, adding nano hexagonal boron nitride to a 40% sodium hydroxide solution by mass, heating the oil bath to 105-110°C, stirring at a speed of 400-600rpm for 36-48h, then centrifuging the reaction solution at 3500r / min, washing the precipitate with anhydrous methanol for 3-5 times, and drying at 65°C for 12-16h to obtain hydroxylated nano boron nitride, wherein the amount ratio of nano hexagonal boron nitride to sodium hydroxide solution is 2.4-2.8g:500mL;
[0019] Step B2, adding hydroxylated nano boron nitride and active monomers to deionized water, adjusting the pH to 4-5 with glacial acetic acid, ultrasonically dispersing for 0.5-1h, continuing stirring at a speed of 60-80rpm for 3.5-4.5h, vacuum drying at 45°C for 8-12h, obtaining 18-24h, and obtaining a thermal conductive filler, wherein the amount ratio of hydroxylated nano boron nitride, active monomer and deionized water is 2.5-3.5g:5-8g:60-80mL. In the above reaction process, under acidic conditions, the active monomer is positively charged due to hydrolysis of surface amino groups, and the hydroxylated boron nitride is negatively charged due to hydrolysis of surface hydroxyl groups. The negatively charged hydroxylated boron nitride and the positively charged active monomer self-assemble under electrostatic conditions to obtain a thermal conductive filler with a core-shell structure.
[0020] Furthermore, the preparation method of the active monomer comprises the following steps:
[0021] Step C1, mix anhydrous ethanol, deionized water and KH-560 evenly, adjust the pH to 5-6 with glacial acetic acid, add nano-alumina while stirring, heat to 55-65°C, stir for 2-3h, filter after the reaction, wash the filter cake with anhydrous ethanol for 3-5 times, and dry at 65°C for 8-12h to obtain amino-alumina, wherein the amount ratio of anhydrous ethanol, deionized water, KH-560 and nano-alumina is 55-65mL:25-35mL:0.8-1.4mL:5-10g. In the above reaction process, under acidic conditions, the active hydroxyl group on the nano-alumina chemically bonds with the amino group on the KH-560 to obtain amino-alumina;
[0022] Step C2, adding amination nano-alumina and N, N-dicyclohexylcarbodiimide to THF, heating to 35-45°C, adding a mixture of p-hydroxyphenylpropionic acid, 4-dimethylaminopyridine and anhydrous ethanol dropwise while stirring, and controlling the dripping to be completed within 30 minutes. After the dripping is completed, the temperature is raised to reflux and stirred for 8-12 hours. After the reaction is completed, centrifugation is performed, and the precipitate is washed 3-5 times with a mass fraction 40% ethanol solution, and vacuum dried at 65°C for 12-16 hours to obtain a hydroxyl monomer, wherein amination nano-alumina, N, N-dicyclohexylcarbodiimide The amount ratio of imine, THF and mixed solution b is 5-10g: 5-10mL: 60-80mL: 45-55mL. In the mixed solution b, the amount ratio of p-hydroxyphenylpropionic acid, 4-dimethylaminopyridine and anhydrous ethanol is 4-8g: 3.5-6.5g: 45-55mL. In the above reaction process, THF is used as a solvent, 4-dimethylaminopyridine is used as an acylating agent, and N,N-dicyclohexylcarbodiimide is used as a dehydrating agent. The amino group on the aminated nano-alumina reacts with the carboxyl group on the p-hydroxyphenylpropionic acid to obtain a hydroxyl monomer.
[0023] Step C3, adding hydroxyl monomer, D-cysteine and p-toluenesulfonic acid to DMF, heating to 65-75°C, stirring and reacting for 8-9h, after the reaction, removing DMF by rotary evaporation to obtain active monomer, wherein the amount ratio of hydroxyl monomer, D-cysteine, p-toluenesulfonic acid and DMF is 5-10g:
[0024] 1.8-3.6g: 0.06-0.12g: 55-65mL, In the above reaction process, DMF is used as solvent and p-toluenesulfonic acid is used as catalyst, and the active hydroxyl group on the hydroxyl monomer and the carboxyl group on D-cysteine undergo esterification reaction to obtain an active monomer.
[0025] Compared with the prior art, the present invention has the following beneficial effects: in order to improve the thermal conductivity and elasticity of rubber, the present invention adds a thermal conductivity enhancing component, which is prepared by ring-opening reaction of epoxidized cellulose nanocrystals and thermal conductive fillers, and then chemically cross-linked. The nanocellulose structure in the thermal conductive enhancing component not only has excellent mechanical properties, but also its surface oxygen-containing active functional groups can form hydrogen bonds with amino groups in the thermal conductive filler to promote its dispersion, thereby improving the thermal conductivity. In addition, the nanocellulose structure has lyotropic liquid crystal properties, which can assist the orientation and distribution of the thermal conductive filler during the solvent volatilization process, prompting it to build a continuous thermal conductive path, further improving the thermal conductivity of the rubber. The thermal conductive filler is composed of hydroxylated nano nitrogen in the core layer. The active monomers of boron nitride and shell are prepared by electrostatic self-assembly. On the one hand, the synergistic effect between nano-alumina and boron nitride in the active monomer will promote the formation of more effective interconnected structure and thermal conductive network, further improving the thermal conductivity. On the other hand, the amide group and carboxyl group in the active monomer can form hydrogen bonds with the thermal conductive filler, which improves the compatibility while further improving its thermal conductivity and mechanical properties. The triglycidyl p-aminophenol that plays a cross-linking role contains benzene rings and epoxy groups. The presence of the benzene ring causes it to produce a π-π effect with the benzene ring in the active monomer, further improving the compatibility and thermal conductivity. In addition, the epoxy group can promote the compatibility between the thermal conductivity enhancing component and the rubber base material, further improving the thermal conductivity and mechanical properties. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0027] Example 1
[0028] Preferably, this embodiment provides a method for preparing an active monomer, comprising the following steps:
[0029] Step C1, 60 mL of anhydrous ethanol, 30 mL of deionized water and 1.1 mL of KH-560 were mixed evenly, the pH was adjusted to 5.5 with glacial acetic acid, 7.5 g of nano-alumina was added while stirring, the temperature was raised to 60° C., and stirred for 2.5 h. After the reaction was completed, the mixture was filtered, and the filter cake was washed with anhydrous ethanol for 4 times, and dried at 65° C. for 10 h to obtain amino-modified nano-alumina;
[0030] Step C2, add 7.5g of amino-modified nano-alumina and 7.5mL of N,N-dicyclohexylcarbodiimide to 70mL of THF, heat to 40°C, and add a mixed solution b of 6g of p-hydroxyphenylpropionic acid, 5g of 4-dimethylaminopyridine and 50mL of anhydrous ethanol dropwise while stirring, and control the dripping to be completed within 30min. After the dripping is completed, heat to reflux and stir for 10h. After the reaction is completed, centrifuge, wash the precipitate with a 40% ethanol solution by mass for 4 times, and vacuum dry at 65°C for 14h to obtain a hydroxyl monomer;
[0031] Step C3, add 7.5 g of hydroxyl monomer, 2.7 g of D-cysteine and 0.09 g of p-toluenesulfonic acid into 60 mL of DMF, heat to 70° C., stir and react for 8.5 h. After the reaction is completed, remove DMF by rotary evaporation to obtain an active monomer.
[0032] Example 2
[0033] Preferably, this embodiment provides a method for preparing a thermally conductive filler, comprising the following steps:
[0034] Step B1, adding 2.6g of nano hexagonal boron nitride to a 40% sodium hydroxide solution, heating the oil bath to 108°C, stirring at 500rpm for 36-48h, then centrifuging the reaction solution at 3500r / min, washing the precipitate with anhydrous methanol 4 times, and drying at 65°C for 14h to obtain hydroxylated nano boron nitride;
[0035] Step B2, add 3.0g of hydroxylated nano-boron nitride and 6.5g of the active monomer prepared in Example 1 into deionized water, adjust the pH to 4.5 with glacial acetic acid, ultrasonically disperse for 0.75h, continue stirring at a speed of 70rpm for 4.0h, and vacuum dry at 45°C for 10h to obtain 21h to obtain a thermally conductive filler.
[0036] Example 3
[0037] Preferably, this embodiment provides a method for preparing a thermal conductivity enhancing component, comprising the following steps:
[0038] Step A1, 3 g of microcrystalline cellulose and 55 mL of 64% sulfuric acid solution were mixed evenly, stirred at 55° C. for 2 h, distilled water was added to stop the reaction, and the mixture was allowed to stand for 5 h. After the reactant was precipitated, the supernatant was discarded, and the remaining suspension was centrifuged and dialyzed to neutrality, and freeze-dried at -45° C. to obtain cellulose nanocrystals;
[0039] Step A2, add 1.3 g of cellulose nanocrystals to 50 mL of DMF, heat to 50° C., stir evenly, add 0.15 mL of epichlorohydrin dropwise, and control the dropping speed to 4 drops / second. After the addition is completed, heat to 65° C., stir and react for 5.5 hours, and remove excess epichlorohydrin in the reaction solution by reduced pressure distillation to obtain epoxidized cellulose nanocrystals;
[0040] Step A3, ultrasonically disperse 0.7 g of epoxidized cellulose nanocrystals and 60 mL of DMF, dropwise add 0.15 g of tetrabutylammonium bromide, 0.5 g of the thermally conductive filler prepared in Example 2 and 25 mL of DMF mixed solution a, after the addition is completed, heat to 110 ° C and stir for 2.5 h, after the reaction is completed, add 0.25 mL of triglycidyl p-aminophenol, continue stirring for 1.5 h, centrifuge, wash the precipitate with 40% by mass ethanol solution 4 times, and dry to obtain a thermal conductivity enhancing component.
[0041] Example 4
[0042] This embodiment provides a thermally conductive silicone rubber material, comprising the following raw materials in parts by weight: 100 parts of EPDM rubber, 35 parts of fluorosilicone rubber, 85 parts of carboxylated nitrile rubber, 40 parts of the thermally conductive enhancement component prepared in Example 3, 3 parts of hexamethyldisilazane, and 1 part of dicumyl peroxide;
[0043] The preparation method of the thermal conductive silicone rubber material comprises the following steps:
[0044] According to weight, EPDM rubber, fluorosilicone rubber, carboxyl nitrile rubber, the thermal conductivity enhancing component prepared in Example 3 and hexamethyldisilazane are added to a kneader, kneaded, and then diisopropylbenzene peroxide is added, and the mixture is mixed at 162°C for 2.6 hours and shaped to obtain a thermally conductive silicone rubber material, wherein the shaping process conditions are: first, hot pressing at 230°C and 15MPa for 12 minutes using a hot press, and then transferred to an oven and treated at 260°C for 8 hours.
[0045] Example 5
[0046] This embodiment provides a thermally conductive silicone rubber material, comprising the following raw materials in parts by weight: 105 parts of EPDM rubber, 40 parts of fluorosilicone rubber, 90 parts of carboxyl nitrile rubber, 45 parts of the thermally conductive enhancement component prepared in Example 3, 4.5 parts of hydroxy silicone oil, and 2 parts of a vulcanizing agent;
[0047] The preparation method of the thermal conductive silicone rubber material comprises the following steps:
[0048] According to weight portions, EPDM rubber, fluorosilicone rubber, carboxyl nitrile rubber, the thermal conductivity enhancing component prepared in Example 3 and hydroxy silicone oil were added to a kneader and kneaded. Then, dibenzoyl peroxide was added and mixed at 163° C. for 2.8 hours and shaped to obtain a thermally conductive silicone rubber material.
[0049] Furthermore, the shaping process conditions are: firstly hot pressing at 235°C and 18MPa for 13min using a hot press, and then transferring to an oven and treating at 270°C for 9h.
[0050] Example 6
[0051] This embodiment provides a thermally conductive silicone rubber material, comprising the following raw materials in parts by weight: 110 parts of EPDM rubber, 45 parts of fluorosilicone rubber, 95 parts of carboxylated nitrile rubber, 50 parts of the thermally conductive enhancement component prepared in Example 3, 6 parts of hexamethyldisilazane, and 3 parts of dicumyl peroxide;
[0052] The preparation method of the thermal conductive silicone rubber material comprises the following steps:
[0053] According to weight portions, EPDM rubber, fluorosilicone rubber, carboxyl nitrile rubber, the thermal conductivity enhancing component prepared in Example 3 and hexamethyldisilazane are added to a kneader, kneaded, and then dicumyl peroxide is added, mixed at 164°C for 3 hours, and shaped to obtain a thermally conductive silicone rubber material, wherein the shaping process conditions are: first hot press at 240°C and 20MPa for 14 minutes using a hot press, and then transferred to an oven and treated at 280°C for 10 hours.
[0054] Comparative Example 1
[0055] The p-hydroxyphenylpropionic acid in Example 1 is removed, and the other raw materials and the preparation process remain unchanged. The prepared substance is then replaced with the active monomer in Example 2, and the other raw materials and the preparation process remain unchanged. The prepared substance is then replaced with the thermal conductive filler in Example 3, and the other raw materials and the preparation process remain unchanged. The prepared substance is then replaced with the thermal conductivity enhancing component in Example 5, and the other raw materials and the preparation process remain unchanged.
[0056] Comparative Example 2
[0057] The 40% mass fraction of sodium hydroxide solution in Example 2 is removed, and the prepared substance is replaced by the thermal conductive filler in Example 3, and the other raw materials and preparation process remain unchanged. The prepared substance is then replaced by the thermal conductivity enhancing component in Example 5, and the other raw materials and preparation process remain unchanged.
[0058] Comparative Example 3
[0059] The cellulose nanocrystals in Example 3 are removed, and the other raw materials and preparation process remain unchanged. The prepared material is then replaced with the thermal conductivity enhancing component in Example 5, and the other raw materials and preparation process remain unchanged.
[0060] Comparative Example 4
[0061] The triglycidyl-p-aminophenol in Example 3 was removed, and the other raw materials and the preparation process remained unchanged. The prepared substance was then replaced with the thermal conductivity enhancing component in Example 5, and the other raw materials and the preparation process remained unchanged.
[0062] Comparative Example 5
[0063] The thermally conductive filler in Example 3 is removed, and the other raw materials and preparation process remain unchanged. The prepared material is then replaced with the thermally conductive enhancing component in Example 5, and the other raw materials and preparation process remain unchanged.
[0064] Comparative Example 6
[0065] The thermal conductivity enhancing component in Example 5 was removed, and the remaining raw materials and preparation process remained unchanged.
[0066] Performance Testing
[0067] The tensile strength, tensile strength and elongation at break of the thermally conductive silicone rubber materials prepared in Examples 4-6 and Comparative Examples 1-6 were measured according to GB / T 170-2001, and the thermal conductivity was tested according to the ASTM D5470 steady-state hot plate method. The test results are shown in Table 1:
[0068] Table 1
[0069]
[0070]
[0071] It can be seen from Table 1 that, compared with Comparative Examples 1-6, the rubber prepared in Examples 4-6 has higher tensile strength, tensile elongation and higher thermal conductivity. Therefore, the embodiments of the present invention not only have high thermal conductivity but also have more excellent mechanical properties.
[0072] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A thermally conductive silicone rubber material, comprising the following raw materials in parts by weight: 100-110 parts of EPDM rubber, 35-45 parts of fluorosilicone rubber, 85-95 parts of carboxyl nitrile rubber, 40-50 parts of thermally conductive enhancing component, 3-6 parts of structure control agent and 1-3 parts of vulcanizing agent; The thermal conductivity enhancing component is firstly prepared by acidifying microcrystalline cellulose with sulfuric acid to obtain cellulose nanocrystals, then reacting with epichlorohydrin crystals to obtain epoxidized cellulose nanocrystals, then reacting with thermal conductive fillers to undergo a ring-opening reaction, and finally chemically cross-linking with triglycidyl p-aminophenol to obtain the thermal conductivity enhancing component. The thermal conductive filler is firstly prepared by subjecting nano hexagonal boron nitride to high temperature heat treatment under alkaline conditions to obtain hydroxylated nano boron nitride, and then further prepared by electrostatic self-assembly with active monomers under acidic conditions; The active monomer is firstly prepared by chemically bonding nano-alumina and KH-560 under acidic conditions to obtain amino nano-alumina, which is then subjected to amidation reaction with p-hydroxyphenylpropionic acid to obtain hydroxyl monomer, and finally subjected to esterification reaction with D-cysteine to obtain the active monomer.
2. A thermally conductive silicone rubber material according to claim 1, characterized in that: The method for preparing the thermal conductivity enhancing component comprises the following steps: Step A1, mix microcrystalline cellulose and 64% sulfuric acid solution, stir at 55°C for 2h, add distilled water to stop the reaction, let stand for 4-6h, pour out the supernatant after the reactant precipitates, centrifuge and dialyze the remaining suspension to neutrality, and freeze-dry at -45°C to obtain cellulose nanocrystals; Step A2, adding cellulose nanocrystals to DMF, heating to 45-55°C, stirring evenly, adding epichlorohydrin dropwise, controlling the dropping speed to 3-5 drops / second, and after the addition is completed, heating to 60-70°C, stirring for reaction for 5-6h, and removing excess epichlorohydrin in the reaction solution by vacuum distillation to obtain epoxidized cellulose nanocrystals; Step A3, ultrasonically disperse the epoxidized cellulose nanocrystals and DMF, drop tetrabutylammonium bromide, thermal conductive filler and DMF mixed solution a, after the dropwise addition is completed, heat to 110°C and stir for 2-3h, after the reaction is completed, add triglycidyl p-aminophenol, continue stirring for 1-2h, centrifuge, wash the precipitate with 40% ethanol solution by mass for 3-5 times, and dry to obtain a thermal conductivity enhancing component.
3. The thermally conductive silicone rubber material according to claim 1, characterized in that: The preparation method of the thermal conductive filler comprises the following steps: Step B1, adding nano hexagonal boron nitride to a 40% by mass sodium hydroxide solution, heating the oil bath to 105-110° C., stirring at a speed of 400-600 rpm for 36-48 hours, then centrifuging the reaction solution at 3500 r / min, washing the precipitate with anhydrous methanol for 3-5 times, and drying at 65° C. for 12-16 hours to obtain hydroxylated nano boron nitride; Step B2, add hydroxylated nano-boron nitride and active monomers into deionized water, adjust the pH to 4-5 with glacial acetic acid, ultrasonically disperse for 0.5-1h, continue stirring at a speed of 60-80rpm for 3.5-4.5h, vacuum dry at 45°C for 8-12h, and obtain 18-24h to obtain a thermal conductive filler.
4. A thermally conductive silicone rubber material according to claim 2, characterized in that: The method for preparing the active monomer comprises the following steps: Step C1, mix anhydrous ethanol, deionized water and KH-560 evenly, adjust the pH to 5-6 with glacial acetic acid, add nano-alumina while stirring, heat to 55-65°C, stir for 2-3h, filter after the reaction, wash the filter cake with anhydrous ethanol for 3-5 times, and dry at 65°C for 8-12h to obtain amino-alumina; Step C2, adding amino nano-alumina and N,N-dicyclohexylcarbodiimide to THF, heating to 35-45°C, adding a mixed solution b of p-hydroxyphenylpropionic acid, 4-dimethylaminopyridine and anhydrous ethanol dropwise while stirring, and controlling the dripping to be completed within 30 minutes. After the dripping is completed, the temperature is raised to reflux and stirred for 8-12 hours. After the reaction is completed, centrifugation is performed, and the precipitate is washed 3-5 times with a mass fraction of 40% ethanol solution, and vacuum dried at 65°C for 12-16 hours to obtain a hydroxyl monomer; Step C3, add hydroxyl monomer, D-cysteine and p-toluenesulfonic acid into DMF, raise the temperature to 65-75° C., stir and react for 8-9 hours. After the reaction is completed, remove DMF by rotary evaporation to obtain an active monomer.
5. The thermally conductive silicone rubber material according to claim 2, characterized in that: In the step A1, the usage ratio of microcrystalline cellulose and sulfuric acid solution is 3 g:50-60 mL.
6. The thermally conductive silicone rubber material according to claim 2, characterized in that: In the step A2, the usage ratio of cellulose nanocrystals, DMF and epichlorohydrin is 1.2-1.4 g:45-55 mL:0.1-0.2 mL.
7. The thermally conductive silicone rubber material according to claim 3, characterized in that: In the step A3, the usage ratio of epoxidized cellulose nanocrystals, DMF, mixed solution a and triglycidyl p-aminophenol is 0.6-0.8 g: 55-65 mL: 20-30 mL: 0.2-0.3 mL, and the usage ratio of tetrabutylammonium bromide, thermal conductive filler and DMF in the mixed solution a is 0.1-0.2 g: 0.4-0.6 g: 20-30 mL.
8. The thermally conductive silicone rubber material according to claim 2, characterized in that: In the step B1, the usage ratio of nano hexagonal boron nitride and sodium hydroxide solution is 2.4-2.8 g: 500 mL, and in the step B2, the usage ratio of hydroxylated nano boron nitride, active monomer and deionized water is 2.5-3.5 g: 5-8 g: 60-80 mL.
9. The thermally conductive silicone rubber material according to claim 4, characterized in that: In the step C1, the usage ratio of anhydrous ethanol, deionized water, KH-560 and nano-alumina is 55-65 mL: 25-35 mL: 0.8-1.4 mL: 5-10 g; in the step C2, the usage ratio of amination nano-alumina, N,N-dicyclohexylcarbodiimide, THF and mixed solution b is 5-10 g: 5-10 mL: 60-80 mL: 45-55 mL; in the mixed solution b, the usage ratio of p-hydroxyphenylpropionic acid, 4-dimethylaminopyridine and anhydrous ethanol is 4-8 g: 3.5-6.5 g: 45-55 mL; in the step C3, the usage ratio of hydroxyl monomer, D-cysteine, p-toluenesulfonic acid and DMF is 5-10 g: 1.8-3.6 g: 0.06-0.12 g: 55-65 mL.
10. A method for preparing the thermally conductive silicone rubber material according to any one of claims 1 to 9, characterized in that: The following steps are involved: According to weight, EPDM rubber, fluorosilicone rubber, carboxyl nitrile rubber, thermal conductivity enhancing component and structure control agent are added into a kneader, kneaded, and then a vulcanizing agent is added. The mixture is mixed at 162-164° C. for 2.6-3 hours and shaped to obtain a thermally conductive silicone rubber material.
Citation Information
Cited By
High-thermal-conductivity aluminum-based copper-clad plate and preparation method thereof
CN119459051A
A high thermal conductivity aluminum-based copper clad laminate and its preparation method
CN119459051B
Insulation heat dissipation and electrified visualization three-dimensional hybrid material and preparation method thereof
CN121895860A
Insulating heat-dissipating and live visualizing three-dimensional hybrid material and preparation method thereof
CN121895860B