Low-cost building thermal insulation material and preparation method thereof
By introducing specific components and improving preparation methods into phenolic resin insulation materials, the problems of high cost and complex process of phenolic resin materials are solved, and the development of low-cost building insulation materials is realized, with good insulation performance and efficient preparation characteristics.
Patent Information
- Application Number
- CN202411205109.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-01
AI Technical Summary
The existing phenolic resin insulation materials are costly and complex in preparation processes, which limits their large-scale application.
Using phenolic resin as the main component, combining a specific amount of trimethylolpropane and 2,2-dimethylolpropionic acid, adding methyl ethyl ketone and trimethylacetamide and other ingredients, through the improvement of the formula and preparation method, Reduce raw material costs and improve mechanical properties, use toughener, leveling agent, etc. to improve performance, and prepare low-cost building insulation materials.
It has achieved the reduction of raw material costs while ensuring insulation performance, simplified the preparation process, and produced low-cost building insulation materials with good insulation performance, with high promotion prospects.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal insulation materials, and in particular to a low-cost building thermal insulation material and a preparation method thereof. Background Art
[0002] Phenolic resin is a foamed product of phenol and formaldehyde condensation. After foaming and curing, phenolic resin basically has no harmful substances. Phenolic foam material is a high molecular organic hard aluminum foil foam product, which is foamed by thermosetting phenolic resin. It is light, fireproof, does not burn when exposed to open flames, smokeless, non-toxic, and drip-free. It has a wide operating temperature range (-196 ~ +200℃) and does not shrink or become brittle in low temperature environments. It is an ideal insulation material for HVAC engineering. Due to the high closed-cell rate of phenolic foam, the thermal conductivity is low, the thermal insulation performance is good, and it has water resistance and water vapor permeability, making it an ideal thermal insulation and energy-saving material.
[0003] Phenolic resin insulation materials can effectively solve the problem of fireproofing and heat preservation of buildings. They do not melt or soften at high temperatures, have low smoke emission, do not spread flames, are flame-resistant, have excellent fireproof performance, and have good heat preservation and energy-saving effects. They combine excellent fireproof performance with good energy-saving effects and are suitable for external wall insulation. They can also be composited with the finishing layer to make an integrated insulation and decoration board, and can also be used to construct the fireproof isolation belt of the traditional EPS / XPS / PU external wall insulation system, used as fireproof and heat-insulating materials in curtain walls, heat-insulating materials in fireproof doors, and fireproof and heat-insulating materials in low or high temperature occasions. In the prior art, the raw material cost of phenolic resin materials is high, and the preparation process is relatively complicated, resulting in a higher price for the finished product than other insulation materials, which to a certain extent restricts the large-scale application of phenolic resin materials. Summary of the invention
[0004] The present invention aims to provide a low-cost building thermal insulation material and a preparation method thereof in view of the technical defects of the prior art, so as to solve the technical problems of high cost and complicated process of conventional phenolic resin thermal insulation materials.
[0005] In order to achieve the above technical objectives, the present invention adopts the following technical solutions: A low-cost building thermal insulation material comprises the following components in parts by weight: 75-80 parts of phenolic resin, 35-45 parts of trimethylolpropane, 20-25 parts of 2,2-dimethylolpropionic acid, 12-18 parts of trimethylolethane trinitrate, 8-10 parts of 5-methoxyisophthalic acid, 4-6 parts of methyl ethyl ketone, 1-4 parts of trimethylacetamide, 0.5-2 parts of disodium ethylenediaminetetraacetate, 2-8 parts of toughening agent, 3-6 parts of defoaming agent, 4-8 parts of leveling agent and 2-4 parts of antioxidant.
[0006] Preferably, the toughening agent is polyvinyl acetate.
[0007] Preferably, the defoaming agent is tributyl phosphate.
[0008] Preferably, the leveling agent is an acrylate homopolymer.
[0009] Preferably, the antioxidant is butylated hydroxyanisole.
[0010] Preferably, the low-cost building insulation material also includes 3 to 3.5 parts by weight of geranyl acetone.
[0011] Preferably, the low-cost building thermal insulation material further comprises 1 to 2 parts by weight of dihydromyrcenol.
[0012] On the basis of the above technical solution, the present invention further improves the preparation method of the above low-cost building insulation material, comprising the following steps: 1) Formaldehyde and resorcinol are mixed in a supersaturated sodium hydroxide environment, and aniline is added, and the mixture is stirred for 1-2 hours, and then the system is evaporated to half its volume at 20-30°C under reduced pressure, and then glass beads and 2-acetylcyclohexanone are added thereto, and the mixture is reacted for 20-30 minutes under shaking conditions, and then the temperature of the system is lowered to 0-1°C, and the solid phase is collected, washed with water, and dried to obtain a phenolic resin; 2) taking the phenolic resin in the formula amount, mixing it with the formula amount of trimethylacetamide and disodium ethylenediaminetetraacetate, and continuously introducing oxygen thereinto, reacting for 20 minutes, then replacing the oxygen with nitrogen, and heating to 50-60° C., maintaining for 1 hour, and then adding the formula amount of trimethylolethane trinitrate, 5-methoxyisophthalic acid, and methyl ethyl ketone therein, mixing well, and then dropping fumaric acid thereinto until crystals are precipitated, diluting it with water to 2 times the volume, and then adding tetraphenylpyrazine therein to fully react; 3) The product obtained in step 3) is mixed with a formulated amount of trimethylolpropane and 2,2-dimethylolpropionic acid, the temperature is raised to 120-150° C., a formulated amount of a toughening agent and a defoaming agent are added thereto, and then the mixture is naturally cooled. During the cooling process, when the system temperature is at 80-90° C., a formulated amount of a leveling agent is added thereto, and when the system temperature is at 60-70° C., a formulated amount of an antioxidant is added thereto. After cooling to room temperature, the solid phase is removed by suction filtration, and the mixture is washed and dried to obtain the low-cost building thermal insulation material.
[0013] Preferably, the entire process of replacing oxygen with nitrogen in step 2) takes no longer than 20 minutes.
[0014] Preferably, in step 3), the molar ratio of the toughening agent to the defoaming agent is 1:1.5.
[0015] The present invention provides a low-cost building thermal insulation material and a preparation method thereof. The technical scheme first improves the formula of the phenolic resin thermal insulation material, and designs a new preparation method on this basis. Specifically, the present invention uses phenolic resin as the main component, introduces a specific amount of trimethylolpropane and 2,2-dimethylolpropionic acid, thereby appropriately reducing the cost of raw materials while fully ensuring the thermal insulation performance; at the same time, the present invention adds components such as methyl ethyl ketone and trimethylacetamide, which helps to improve the mechanical properties of the thermal insulation material. At the preparation method level, the present invention first uses formaldehyde and resorcinol for condensation, and then uses 2-acetylcyclohexanone for modification. For the prepared modified phenolic resin, a reaction system is first constructed with trimethylacetamide and ethylenediaminetetraacetic acid, and then a cross-linked structure is formed, and finally a toughening agent, a leveling agent and other components are used to improve its performance. The present invention has low cost, high preparation efficiency, and the product has good thermal insulation performance, and has great promotion prospects. DETAILED DESCRIPTION
[0016] The specific embodiments of the present invention will be described in detail below. In order to avoid too much unnecessary details, the well-known structures or functions will not be described in detail in the following examples. The approximate language used in the following examples can be used for quantitative expression, indicating that the quantity can be allowed to have a certain change without changing the basic function. Unless otherwise defined, the technical and scientific terms used in the following examples have the same meaning as those generally understood by those skilled in the art to which the present invention belongs.
[0017] Example 1 A low-cost building thermal insulation material comprises the following components in parts by weight: 75-80 parts of phenolic resin, 35-45 parts of trimethylolpropane, 20-25 parts of 2,2-dimethylolpropionic acid, 12-18 parts of trimethylolethane trinitrate, 8-10 parts of 5-methoxyisophthalic acid, 4-6 parts of methyl ethyl ketone, 1-4 parts of trimethylacetamide, 0.5-2 parts of disodium ethylenediaminetetraacetate, 2-8 parts of toughening agent, 3-6 parts of defoaming agent, 4-8 parts of leveling agent and 2-4 parts of antioxidant.
[0018] The method for preparing the above-mentioned low-cost building thermal insulation material comprises the following steps: 1) Formaldehyde and resorcinol are mixed in a supersaturated sodium hydroxide environment, and aniline is added, and the mixture is stirred for 1-2 hours, and then the system is evaporated to half its volume at 20-30°C under reduced pressure, and then glass beads and 2-acetylcyclohexanone are added thereto, and the mixture is reacted for 20-30 minutes under shaking conditions, and then the temperature of the system is lowered to 0-1°C, and the solid phase is collected, washed with water, and dried to obtain a phenolic resin; 2) taking the phenolic resin in the formula amount, mixing it with the formula amount of trimethylacetamide and disodium ethylenediaminetetraacetate, and continuously introducing oxygen thereinto, reacting for 20 minutes, then replacing the oxygen with nitrogen, and heating to 50-60° C., maintaining for 1 hour, and then adding the formula amount of trimethylolethane trinitrate, 5-methoxyisophthalic acid, and methyl ethyl ketone therein, mixing well, and then dropping fumaric acid thereinto until crystals are precipitated, diluting it with water to 2 times the volume, and then adding tetraphenylpyrazine therein to fully react; 3) The product obtained in step 3) is mixed with a formulated amount of trimethylolpropane and 2,2-dimethylolpropionic acid, the temperature is raised to 120-150° C., a formulated amount of a toughening agent and a defoaming agent are added thereto, and then the mixture is naturally cooled. During the cooling process, when the system temperature is at 80-90° C., a formulated amount of a leveling agent is added thereto, and when the system temperature is at 60-70° C., a formulated amount of an antioxidant is added thereto. After cooling to room temperature, the solid phase is removed by suction filtration, and the mixture is washed and dried to obtain the low-cost building thermal insulation material.
[0019] Example 2 A low-cost building insulation material comprises the following components in parts by weight: 75-80 parts of phenolic resin, 35-45 parts of trimethylolpropane, 20-25 parts of 2,2-dimethylolpropionic acid, 12-18 parts of trimethylolethane trinitrate, 8-10 parts of 5-methoxyisophthalic acid, 4-6 parts of methyl ethyl ketone, 1-4 parts of trimethylacetamide, 0.5-2 parts of disodium ethylenediaminetetraacetate, 2-8 parts of toughening agent, 3-6 parts of defoaming agent, 4-8 parts of leveling agent, and 2-4 parts of antioxidant. The toughening agent is polyvinyl acetate. The defoaming agent is tributyl phosphate. The leveling agent is an acrylate homopolymer. The antioxidant is butylated hydroxyanisole. The low-cost building insulation material also comprises 3-3.5 parts of geranyl acetone. The low-cost building insulation material also comprises 1-2 parts of dihydromyrcenol.
[0020] The method for preparing the above-mentioned low-cost building thermal insulation material comprises the following steps: 1) Formaldehyde and resorcinol are mixed in a supersaturated sodium hydroxide environment, and aniline is added, and the mixture is stirred for 1-2 hours, and then the system is evaporated to half its volume at 20-30°C under reduced pressure, and then glass beads and 2-acetylcyclohexanone are added thereto, and the mixture is reacted for 20-30 minutes under shaking conditions, and then the temperature of the system is lowered to 0-1°C, and the solid phase is collected, washed with water, and dried to obtain a phenolic resin; 2) taking the phenolic resin in the formula amount, mixing it with the formula amount of trimethylacetamide and disodium ethylenediaminetetraacetate, and continuously introducing oxygen thereinto, reacting for 20 minutes, then replacing the oxygen with nitrogen, and heating to 50-60° C., maintaining for 1 hour, and then adding the formula amount of trimethylolethane trinitrate, 5-methoxyisophthalic acid, and methyl ethyl ketone therein, mixing well, and then dropping fumaric acid thereinto until crystals are precipitated, diluting it with water to 2 times the volume, and then adding tetraphenylpyrazine therein to fully react; 3) The product obtained in step 3) is mixed with a formulated amount of trimethylolpropane and 2,2-dimethylolpropionic acid, the temperature is raised to 120-150° C., a formulated amount of a toughening agent and a defoaming agent are added thereto, and then the mixture is naturally cooled. During the cooling process, when the system temperature is at 80-90° C., a formulated amount of a leveling agent is added thereto, and when the system temperature is at 60-70° C., a formulated amount of an antioxidant is added thereto. After cooling to room temperature, the solid phase is removed by suction filtration, and the mixture is washed and dried to obtain the low-cost building thermal insulation material.
[0021] In step 2), the whole process of replacing oxygen with nitrogen takes no longer than 20 minutes. In step 3), the molar ratio of toughening agent to defoaming agent is 1:1.5.
[0022] The embodiments of the present invention are described in detail above, but the contents are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the scope of the present invention shall be included in the protection scope of the present invention.
Claims
1. A low-cost building insulation material, characterized in that The invention comprises the following ingredients in parts by weight: 75-80 parts of phenolic resin, 35-45 parts of trimethylolpropane, 20-25 parts of 2,2-dimethylolpropionic acid, 12-18 parts of trimethylolethane trinitrate, 8-10 parts of 5-methoxyisophthalic acid, 4-6 parts of methyl ethyl ketone, 1-4 parts of trimethylacetamide, 0.5-2 parts of disodium ethylenediaminetetraacetate, 2-8 parts of toughening agent, 3-6 parts of defoaming agent, 4-8 parts of leveling agent and 2-4 parts of antioxidant.
2. A low-cost building thermal insulation material according to claim 1, characterized in that: The toughening agent is polyvinyl acetate.
3. A low-cost building thermal insulation material according to claim 1, characterized in that: The defoaming agent is tributyl phosphate.
4. A low-cost building thermal insulation material according to claim 1, characterized in that: The leveling agent is an acrylate homopolymer.
5. A low-cost building thermal insulation material according to claim 1, characterized in that: The antioxidant is butylated hydroxyanisole.
6. A low-cost building thermal insulation material according to claim 1, characterized in that: The low-cost building thermal insulation material also includes 3 to 3.5 parts by weight of geranyl acetone.
7. A low-cost building thermal insulation material according to claim 1, characterized in that: The low-cost building thermal insulation material also includes 1 to 2 parts by weight of dihydromyrcenol.
8. The method for preparing the low-cost building thermal insulation material according to claim 1, characterized in that The following steps are involved: 1) Formaldehyde and resorcinol are mixed in a supersaturated sodium hydroxide environment, and aniline is added, and the mixture is stirred for 1-2 hours, and then the system is evaporated to half its volume at 20-30°C under reduced pressure, and then glass beads and 2-acetylcyclohexanone are added thereto, and the mixture is reacted for 20-30 minutes under shaking conditions, and then the temperature of the system is lowered to 0-1°C, and the solid phase is collected, washed with water, and dried to obtain a phenolic resin; 2) taking the phenolic resin in the formula amount, mixing it with the formula amount of trimethylacetamide and disodium ethylenediaminetetraacetate, and continuously introducing oxygen thereinto, reacting for 20 minutes, then replacing the oxygen with nitrogen, and heating to 50-60° C., maintaining for 1 hour, and then adding the formula amount of trimethylolethane trinitrate, 5-methoxyisophthalic acid, and methyl ethyl ketone therein, mixing well, and then dropping fumaric acid thereinto until crystals are precipitated, diluting it with water to 2 times the volume, and then adding tetraphenylpyrazine therein to fully react; 3) The product obtained in step 3) is mixed with a formulated amount of trimethylolpropane and 2,2-dimethylolpropionic acid, the temperature is raised to 120-150° C., a formulated amount of a toughening agent and a defoaming agent are added thereto, and then the mixture is naturally cooled. During the cooling process, when the system temperature is at 80-90° C., a formulated amount of a leveling agent is added thereto, and when the system temperature is at 60-70° C., a formulated amount of an antioxidant is added thereto. After cooling to room temperature, the solid phase is removed by suction filtration, and the mixture is washed and dried to obtain the low-cost building thermal insulation material.
9. The preparation method according to claim 8, characterized in that: In step 2), the entire process of replacing oxygen with nitrogen takes no longer than 20 minutes.
10. The preparation method according to claim 8, characterized in that: In step 3), the molar ratio of the toughening agent to the defoaming agent is 1:1.5.