A flame retardant plastic part and its preparation method and application
By enriching ionic liquid on the surface of plastic parts under the action of electric field, the problem of large amount of flame retardant in the prior art affecting performance is solved, and low-cost, high-fire retardant grade flame retardant plastic parts are achieved, which is suitable for the preparation of flame retardant plastic parts. Mass production.
Patent Information
- Application Number
- CN202411364512.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-29
AI Technical Summary
The large amount of flame retardant added to existing flame retardant plastic parts will affect other comprehensive properties of the plastic, and the halogen flame retardant is not friendly in the environment, and there is a lack of effective low-cost and high flame retardant preparation method.
Ionic liquid is used as flame retardant, and the surface of the plastic parts is enriched under the action of electric field, and the double-screw extrusion granulation and electric field treatment technology are used to prepare low-dose and efficient flame retardant plastic parts.
It is achieved with very little flame retardant addition, which reduces costs and has little impact on the mechanical properties of plastics. The preparation method is simple and easy to perform, and is suitable for large-scale production.
Smart Images

Figure CN118879044B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of composite materials, and in particular relates to a flame retardant plastic part and a preparation method and application thereof. Background Art
[0002] Flame-retardant plastic parts are an important type of plastic products, especially in the field of engineering plastics, where flame-retardant products account for about half of the market applications. With the gradual improvement of safety regulations in various countries, the requirements for flame retardancy levels in various application fields are getting higher and higher. Conventional flame retardant technology mainly involves adding halogen flame retardants or phosphorus flame retardants. A major disadvantage is that the amount added is large, which will significantly affect other comprehensive properties of plastic products. At the same time, halogen flame retardancy is restricted in more and more fields due to environmental unfriendliness. In order to reduce the amount of flame retardants used, one method is to use surface coating or spraying methods to enrich the flame retardant on the surface of plastic products. However, this requires secondary processing, which greatly increases costs, and it is also difficult to ensure the stability of surface flame retardants. There is no mature technology yet.
[0003] Ionic liquid flame retardants are a new type of flame retardant that has emerged in recent years. Ionic liquids themselves are organic compounds with good compatibility with plastics. By designing ionic liquids with different chemical structures and making them contain flame retardant elements such as phosphorus, fluorine, and nitrogen, ionic liquids can have flame retardant effects. However, the current disadvantages of ionic liquid flame retardants are mainly insufficient flame retardant efficiency and high prices. If the amount added is large, it will play a role similar to that of a plasticizer, reducing the mechanical properties of the plastic and significantly increasing the cost. Therefore, it is necessary to find a method for preparing flame-retardant plastic parts with a small amount of ionic liquid flame retardant added and excellent flame retardant effect. Summary of the invention
[0004] In order to overcome the shortcomings and deficiencies of the above-mentioned prior art, the primary purpose of the present invention is to provide a method for preparing an ionic liquid flame-retardant plastic product. The plastic product prepared by the method uses an ionic liquid as a flame retardant, and utilizes the migration characteristics of the ionic liquid in an electric field to enrich the ionic liquid on the surface of the plastic product. The amount of flame retardant is small, the cost is low, and the flame retardant grade is high, and the impact on other properties is small. Using this method, halogen-free flame retardancy can also be easily achieved.
[0005] Another object of the present invention is to provide an ionic liquid flame-retardant plastic product prepared by the above method.
[0006] Another object of the present invention is to provide applications of the above-mentioned ionic liquid flame-retardant plastic parts.
[0007] The purpose of the present invention is achieved through the following solutions:
[0008] A method for preparing an ionic liquid flame-retardant plastic part comprises the following steps:
[0009] 1) Prepare plastic particles comprising the following components in percentage by weight by twin-screw extrusion granulation:
[0010] Resin 57%-99.5%;
[0011] Ionic liquid flame retardant 0.5%-5%;
[0012] Glass fiber 0%-30%;
[0013] Antioxidant 0%-1%;
[0014] Release agent 0%-1%;
[0015] Toughening agent 0-6%;
[0016] 2) Processing plastic particles into required parts;
[0017] 3) When the plastic part is treated at a temperature higher than the Tg of the resin and a DC voltage, the ionic liquid will migrate to the surface of the plastic part and accumulate under the action of the electric field;
[0018] 4) After cooling to room temperature, the electric field is removed to obtain the plastic product.
[0019] The resin described in step (1) includes at least one of polycarbonate, polyamide, polybutylene terephthalate (PBT), polyphenylene oxide, poly(acrylonitrile-butadiene-styrene) (ABS), polyethylene terephthalate (PET), and polymethyl methacrylate (PMMA).
[0020] The ionic liquid flame retardant described in step (1) includes at least one of imidazole ionic liquids, pyrrolidine ionic liquids, quaternary ammonium salt ionic liquids, piperidine ionic liquids, and pyridine ionic liquids, preferably at least one of 1,3-dimethylimidazolium methanesulfonate ([C1MIm]MS), 1-ethylpyridinium hexafluorophosphate ([C2Py]PF6), and 1-ethyl-1-methylpiperidinium p-toluenesulfonate ([C2MPd]TS).
[0021] The antioxidant in step (1) is at least one of a hindered phenol antioxidant, a hindered amine antioxidant, and a phosphite antioxidant;
[0022] The release agent in step (1) is at least one of a fatty acid salt and a fatty acid ester, preferably pentaerythritol stearate PETS;
[0023] The toughening agent described in step (1) is at least one of polyolefin, polyacrylate copolymer and polybutadiene copolymer, preferably the toughening agent MBS.
[0024] The processing and molding described in step (2) is preferably performed by injection molding or extrusion molding, and the ionic liquid flame retardant will be evenly dispersed in the plastic part.
[0025] The plastic part described in step (2) is a flat plate part with a thickness of less than 1 mm.
[0026] The DC voltage in step (3) is 10-200V; the treatment time is 1min-60min; the positive and negative electrodes of the DC are both electrode plates, which are in direct contact with the two sides of the plastic part respectively, and the contact surface covers the entire surface of the part, thereby ensuring that all ionic liquids in the plastic part can move under the action of the electric field.
[0027] When the resin in step (1) is a crystalline polymer, the temperature in step (3) is preferably higher than the Tg of the resin and lower than the Tm of the resin; when the resin in step (1) is an amorphous polymer, the temperature in step (3) is preferably higher than the Tg of the resin and lower than the Tf of the resin.
[0028] In step (4), as the temperature drops below the Tg of the plastic, the ionic liquid will be fixed near the surface of the plastic part, achieving a higher flame retardant efficiency than uniform distribution.
[0029] An ionic liquid flame-retardant plastic product prepared by the method.
[0030] The above-mentioned ionic liquid flame-retardant plastic parts are used in automobiles, electronic appliances, and consumer electronic products.
[0031] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0032] The flame retardant plastic product of the present invention can achieve a higher flame retardant grade with very little addition of flame retardant, has little effect on the mechanical properties of the plastic, and can significantly reduce costs. At the same time, the preparation method of the present invention is simple and easy to implement, suitable for large-scale production, and can reduce costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 Schematic diagram of electrical treatment of plastic parts. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below in conjunction with the examples and drawings, but the embodiments of the present invention are not limited thereto. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0035] The technical solution of the present application is described in detail using an embodiment. The raw materials in the embodiment can be obtained from the market, as follows: polyamide 66 is BASF Ultramid A3L, PBT is Changchun Chemical 1100-211S, polycarbonate is SABIC Lexan 141R, MBS is Dow EXL2620, glass fiber is CPIC ECS307, ionic liquid 1,3-dimethylimidazolium methanesulfonate ([C1MIm]MS), 1-ethylpyridinium hexafluorophosphate ([C2Py]PF6), 1-ethyl-1-methylpiperidinium p-toluenesulfonate ([C2MPd]TS) are all purchased from Merck. The flame retardant test refers to UL94 standard. The tensile strength test refers to ISO527.
[0036] Example 1
[0037] The flame retardant plastic parts are prepared by the following steps:
[0038] 1) Through twin-screw extrusion processing, the processing temperature is 230-260°C, and plastic particles including the following components in weight percentage are prepared:
[0039] PBT 94.7%;
[0040] [C1MIm]MS 5%;
[0041] Antioxidant 1010 0.1%;
[0042] Release agent PETS 0.2%;
[0043] 2) The obtained plastic particles were molded into UL94 flame retardant strips with a thickness of 0.8 mm by injection molding, with an injection temperature of 260°C and a mold temperature of 50°C.
[0044] 3) Treat the workpiece at 120℃ and 30V DC voltage for 5 minutes.
[0045] 4) Remove the electric field after cooling naturally to room temperature. Test the flame retardant grade and tensile strength of the sample.
[0046] The sample of Comparative Example 1 has the same composition and operation as the sample of Example 1, except that the sample of Comparative Example 1 is not subjected to the electric field treatment of step (3).
[0047] Table 1 Flame retardancy and tensile strength test results of Comparative Example 1 and Example 1
[0048]
[0049] Example 2
[0050] The flame retardant plastic parts are prepared by the following steps:
[0051] 1) Through twin-screw extrusion processing, the processing temperature is 250-280°C, and plastic particles including the following components in weight percentage are prepared:
[0052] PC 98.7%;
[0053] [C2MPd]TS 1%;
[0054] Antioxidant 1076 0.1%;
[0055] Release agent PETS 0.2%;
[0056] 2) The obtained plastic particles were molded into UL94 flame retardant strips with a thickness of 0.4 mm by injection molding, with an injection temperature of 300°C and a mold temperature of 80°C.
[0057] 3) Treat the workpiece at 170°C and 100V DC voltage for 2 minutes.
[0058] 4) Remove the electric field after cooling naturally to room temperature. Test the flame retardant grade and tensile strength of the sample.
[0059] The sample of Comparative Example 2 has the same composition and operation as the sample of Example 2, except that the sample of Comparative Example is not subjected to the electric field treatment of step (3).
[0060] Table 2 Flame retardancy and tensile strength test results of Comparative Example 2 and Example 2
[0061]
[0062] Example 3
[0063] The flame retardant plastic parts are prepared by the following steps:
[0064] 1) Through twin-screw extrusion processing, the processing temperature is 260-280°C, and plastic particles including the following components in weight percentage are prepared:
[0065] PC 78.7%;
[0066] [C2MPd]TS 1%;
[0067] Glass fiber 20%;
[0068] Antioxidant 1076 0.1%;
[0069] Release agent PETS 0.2%;
[0070] 2) The obtained plastic particles were molded into UL94 flame retardant strips with a thickness of 0.6 mm by injection molding, with an injection temperature of 300°C and a mold temperature of 80°C.
[0071] 3) Treat the workpiece at 170°C and 100V DC voltage for 3 minutes.
[0072] 4) Remove the electric field after cooling naturally to room temperature. Test the flame retardant grade and tensile strength of the sample.
[0073] The sample of comparative example 3 has the same composition and operation as the sample of embodiment 3, except that the sample of comparative example 3 is not subjected to the electric field treatment of step (3).
[0074] Table 3 Flame retardancy and tensile strength test results of Comparative Example 3 and Example 3
[0075]
[0076] Example 4
[0077] The flame retardant plastic parts are prepared by the following steps:
[0078] 1) Through twin-screw extrusion processing, the processing temperature is 250-280°C, and plastic particles including the following components in weight percentage are prepared:
[0079] PC 93.2%;
[0080] [C2MPd]TS 1.5%;
[0081] MBS 5%;
[0082] Antioxidant 1076 0.1%;
[0083] Release agent PETS 0.2%;
[0084] 2) The obtained plastic particles were molded into UL94 flame retardant strips with a thickness of 0.6 mm by injection molding, with an injection temperature of 300°C and a mold temperature of 80°C.
[0085] 3) Treat the workpiece at 160℃ and 120V DC voltage for 2min.
[0086] 4) Remove the electric field after cooling naturally to room temperature. Test the flame retardant grade and tensile strength of the sample.
[0087] The sample of Comparative Example 4 has the same composition and operation as the sample of Example 4, except that the sample of Comparative Example 4 is not subjected to the electric field treatment of step (3).
[0088] Table 4 Flame retardancy and tensile strength test results of Comparative Example 4 and Example 4
[0089]
[0090] Example 5
[0091] The flame retardant plastic parts are prepared by the following steps:
[0092] 1) Through twin-screw extrusion processing, the processing temperature is 250-280°C, and plastic particles including the following components in weight percentage are prepared:
[0093] PA66 95.7%;
[0094] [C2Py]PF6 4%;
[0095] Antioxidant 1076 0.1%;
[0096] Release agent PETS 0.2%;
[0097] 2) The obtained plastic particles were molded into UL94 flame retardant strips with a thickness of 0.8 mm by injection molding, with an injection temperature of 280°C and a mold temperature of 60°C.
[0098] 3) Treat the workpiece at 140℃ and 50V DC voltage for 5 minutes.
[0099] 4) Remove the electric field after cooling naturally to room temperature. Test the flame retardant grade and tensile strength of the sample.
[0100] The sample of comparative example 5 has the same composition and operation as the sample of embodiment 5, except that the sample of comparative example 5 is not subjected to the electric field treatment of step (3).
[0101] Table 5 Flame retardancy and tensile strength test results of Comparative Example 5 and Example 5
[0102]
[0103] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing an ionic liquid flame-retardant plastic part, characterized in that The following steps are involved: 1) Prepare plastic particles comprising the following components in percentage by weight by twin-screw extrusion granulation: Resin 57%-99.5%; Ionic liquid flame retardant 0.5%-5%; Glass fiber 0%-30%; Antioxidant 0%-1%; Release agent 0%-1%; Toughening agent 0-6%; 2) Processing plastic particles into required parts; 3) Treating the plastic part at a temperature higher than the Tg of the resin and a DC voltage, so that the ionic liquid migrates to the surface of the plastic part and accumulates under the action of the electric field; 4) After cooling to room temperature, the electric field is removed to obtain the plastic product.
2. The method for preparing an ionic liquid flame-retardant plastic product according to claim 1, characterized in that: The resin described in step (1) includes at least one of polycarbonate, polyamide, polybutylene terephthalate, polyphenylene ether, poly(acrylonitrile-butadiene-styrene), polyethylene terephthalate, and polymethyl methacrylate.
3. The method for preparing the ionic liquid flame-retardant plastic product according to claim 1, characterized in that: The ionic liquid flame retardant described in step (1) includes at least one of imidazole ionic liquids, pyrrolidine ionic liquids, quaternary ammonium salt ionic liquids, piperidine ionic liquids, and pyridine ionic liquids.
4. The method for preparing an ionic liquid flame-retardant plastic product according to claim 1, characterized in that: The ionic liquid flame retardant described in step (1) includes at least one of 1,3-dimethylimidazolium methanesulfonate, 1-ethylpyridinium hexafluorophosphate, and 1-ethyl-1-methylpiperidinium p-toluenesulfonate.
5. The method for preparing the ionic liquid flame-retardant plastic product according to claim 1, characterized in that: The antioxidant in step (1) is at least one of a hindered phenol antioxidant, a hindered amine antioxidant, and a phosphite antioxidant; The release agent in step (1) is at least one of a fatty acid salt and a fatty acid ester; The toughening agent in step (1) is at least one of polyolefin, polyacrylate copolymer and polybutadiene copolymer.
6. The method for preparing an ionic liquid flame-retardant plastic product according to claim 1, characterized in that: The processing and molding described in step (2) is through injection molding or extrusion processing and molding, and the ionic liquid flame retardant will be evenly dispersed in the plastic part; The plastic part described in step (2) is a flat plate part with a thickness of less than 1 mm.
7. The method for preparing an ionic liquid flame-retardant plastic product according to claim 1, characterized in that: The DC voltage in step (3) is 10-200V; the treatment time is 1min-60min; the positive and negative electrodes of the DC are both electrode plates, which are in direct contact with the two sides of the plastic part respectively, and the contact surface covers the entire surface of the part, thereby ensuring that all ionic liquids in the plastic part can move under the action of the electric field.
8. The method for preparing an ionic liquid flame-retardant plastic product according to claim 1, characterized in that: When the resin in step (1) is a crystalline polymer, the temperature in step (3) is higher than the Tg of the resin and lower than the Tm of the resin; when the resin in step (1) is an amorphous polymer, the temperature in step (3) is higher than the Tg of the resin and lower than the Tf of the resin.
9. An ionic liquid flame-retardant plastic product prepared by the method according to any one of claims 1 to 8.
10. Use of the ionic liquid flame-retardant plastic parts according to claim 9 in automobiles, electronic appliances or consumer electronic products.
Citation Information
Patent Citations
Flame-retardant plastic using ionic liquid as fire retardant and preparation method of flame-retardant plastic
CN106751585A
Flame-retardant dyeing method of bamboo sheets
CN108972772A
Cited By
Ionic liquid flame-retardant plastic part as well as preparation and application thereof
CN119371785A
An ionic liquid flame-retardant plastic part and preparation and application thereof
CN119371785B