The invention relates to a preparation method of a polymer based on DOPO and 2, 2apos; novel phosphine-nitrogen flame retardant of-(1, 3-phenylene)-dioxazoline as well as preparation method and application of novel phosphine-nitrogen flame retardant
By combining DOPO and PBO, the new phosphine nitrogen flame retardant prepared solves the environmental and health hazards of traditional flame retardants, significantly improves the flame retardant performance and stability, is suitable for a variety of polymer matrix, and meets resistance Dual requirements for combustion effect and environmental protection requirements.
Patent Information
- Application Number
- CN202411385940.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional halogen-containing flame retardants release toxic gases and corrosive smoke during combustion, which poses harm to the environment and human health. A single flame retardant is difficult to meet the dual needs of flame retardant effect and environmental protection requirements.
By placing 9,10-dihydro-9-oxa-10-phosphophenophen-10-oxide (DOPO) with 2,2'-(1,3-phenylene)-dioxazoline (PBO) In combination, a new phosphine nitrogen flame retardant was prepared, which significantly improved the flame retardant performance using the phosphorus-nitrogen synergistic effect, and avoided the degradation reaction caused by the 'P-H' bond in the structure through specific process steps and catalysts.
This new flame retardant does not release toxic gases during combustion, maintains the mechanical properties of polyester materials, is widely used in various polymer matrixes, meets environmental protection and health safety requirements, and broadens the application range of DOPO and oxazoline. The development of halogen-free flame retardants provides new avenues.
Smart Images

Figure CN119039352A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of flame retardant material preparation, and in particular relates to a novel phosphine nitrogen flame retardant based on DOPO and 2,2'-(1,3-phenylene)-dioxazoline, and a preparation method and application thereof. Background Art
[0002] With the gradual tightening of regulations and growing environmental awareness, the demand for environmentally friendly flame retardants is increasing. Traditional halogen-containing flame retardants release toxic gases and corrosive fumes during combustion, posing a threat to the environment and human health. Therefore, the development of environmentally friendly and highly effective halogen-free flame retardants has become a key research direction.
[0003] 9,10-Dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) is a phosphaphenanthrene flame retardant monomer. Due to its phosphorus-containing structure, it possesses excellent flame retardancy and low toxicity, making it an important halogen-free flame retardant. Its structure contains a "PH" bond, which makes it acidic in the molten state. This can cause polyester resin degradation during the mixing process, limiting its application range. Furthermore, the "PH" bond can react with functional groups such as olefins, acetylenes, epoxy groups, and aldehydes to form a variety of compounds, making DOPO a promising candidate for research. However, in some applications, a single flame retardant may not meet the dual requirements of flame retardancy and environmental protection. Therefore, the development of composite flame retardants, combining different flame retardant mechanisms and material properties, has become an important research direction.
[0004] 2,2'-(1,3-phenylene)-bisoxazoline (PBO) is an important organic compound consisting of two oxazoline rings and a 1,3-phenylene bridging group. Its unique chemical structure and reactivity have made it a key player in polymer chemistry, materials science, and catalysis. Research and development of novel PBO-based materials and technologies will further advance its application in various fields. Summary of the Invention
[0005] In view of the above-mentioned deficiencies in the prior art, the present invention solves the problem of providing a novel phosphine nitrogen flame retardant based on DOPO and 2,2'-(1,3-phenylene)-bisoxazoline with good flame retardancy, stable performance and environmental protection, as well as a preparation method and application thereof.
[0006] In order to solve the above problems, the technical solutions adopted by the present invention are as follows:
[0007] A new phosphine-nitrogen flame retardant based on DOPO and 2,2'-(1,3-phenylene)-bisoxazoline, with the following structural formula:
[0008] A method for preparing a novel phosphine-nitrogen flame retardant based on DOPO and 2,2'-(1,3-phenylene)-dioxazoline, comprising the following steps:
[0009] S1. Add DOPO, PBO, anhydrous zinc acetate catalyst, xylene or chlorobenzene to a glass reaction vessel or glass-lined reactor, fill with nitrogen, start stirring, heat, stir, and reflux;
[0010] S2. Turn off the heating of the reaction phase in step S1, continue stirring, and cool to room temperature to precipitate a light yellow powder solid in the solution;
[0011] S3, separating the liquid-solid mixture in S2 to obtain a light yellow powder;
[0012] S4. Add the light yellow powder and anhydrous ethanol from S3 to a glass reaction vessel or a glass-lined reactor, fill with nitrogen, start stirring, heat, and continue stirring until the yellow powder dissolves;
[0013] S5. Turn off the heating of the liquid in S4, continue stirring, and cool to room temperature to precipitate a light yellow crystalline powder from the solution;
[0014] S6, separating the solid and liquid of the material in S5 to obtain a light yellow crystalline powder; washing with anhydrous ethanol;
[0015] S7. Drying the washed light yellow powder to obtain the flame retardant of the present invention.
[0016] Furthermore, in step S1, the weight proportions of the components are: 10-11 parts of DOPO, 5 parts of PBO, 0.1-0.2 parts of anhydrous zinc acetate as a catalyst, and 50-60 parts of xylene or chlorobenzene.
[0017] Furthermore, in step S1, the mixture is heated to 120-130° C. and refluxed for 10-12 hours.
[0018] Furthermore, in step S4, the weight portion of anhydrous ethanol is 90 to 100 parts; the heating temperature is 65 to 70° C.; and the stirring time is 10 to 20 minutes.
[0019] Furthermore, in step S6, washing is performed twice with anhydrous ethanol.
[0020] Furthermore, in step S7, the product is dried at 80° C. for 8 to 10 hours.
[0021] A novel phosphine-nitrogen flame retardant based on DOPO and 2,2'-(1,3-phenylene)-bisoxazoline is used in PET resin.
[0022] The structural formula of PBO is as follows:
[0023]
[0024] The chemical structure of DOPO is as follows:
[0025]
[0026] The synthetic route of the flame retardant is as follows:
[0027]
[0028] The beneficial effects of the present invention are as follows:
[0029] This patented invention is based on the unique properties of DOPO and oxazoline. By combining the two to prepare a new flame retardant, it will have significant advantages. First, the combination of DOPO and oxazoline can introduce a phosphorus-nitrogen synergistic effect, thereby significantly improving flame retardant properties. Second, this new flame retardant does not release toxic gases during combustion and is environmentally friendly. In addition, the "PH" bond in the structure is eliminated. When mixed with resin, it will not cause accelerated degradation of polyester materials, nor will it react with polyester polymer materials. Therefore, it will not cause the viscosity of PET resin to decrease during processing, thereby maintaining its mechanical properties. This flame retardant not only has excellent performance and is widely applicable in the field of material flame retardancy, but also meets environmental protection and health and safety requirements. This flame retardant has little effect on the mechanical properties of the material and can be widely used in various polymer matrices. The present invention not only broadens the application range of DOPO and oxazoline, but also provides a new path for the development of halogen-free flame retardants. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a high performance liquid chromatography test chart of the flame retardant in Example 1 of the present invention.
[0031] Figure 2 This is a thermogravimetric test chart of the flame retardant in Example 1 of the present invention.
[0032] Figure 3 This is a Fourier infrared spectrum of the flame retardant in Example 1 of the present invention.
[0033] Figure 4 This is a torque rheometer test data diagram of the flame retardant in Example 1 of the present invention. DETAILED DESCRIPTION
[0034] The present invention will be described in further detail below with reference to the accompanying drawings.
[0035] Example 1
[0036] A method for preparing a novel phosphine-nitrogen flame retardant based on DOPO and 2,2'-(1,3-phenylene)-dioxazoline, comprising the following steps:
[0037] S1. In a 5 L four-necked glass flask, add 400 g of DOPO, 200 g of PBO, 2000 g of xylene, and 5 g of anhydrous zinc acetate. Fill with nitrogen at a flow rate of 0.1 L / min, start stirring (stirring speed is 350 rpm), heat to 120°C, start stirring, and reflux for 10 hours.
[0038] S2. Turn off the heating, continue stirring, and cool to room temperature. A light yellow powder solid will precipitate from the solution.
[0039] S3. The feed liquid in S2 was filtered under reduced pressure at -0.1 MPa for solid-liquid separation (using a φ150 mm Buchner funnel, a 5000 mL suction flask, and medium-speed qualitative filter paper) to obtain a light yellow powder.
[0040] S4. In a 5L four-necked glass flask, add the light yellow powder in S3 and 4000g of anhydrous ethanol, fill with nitrogen at a flow rate of 0.1L / min, start stirring (stirring speed is 350r / min), heat to 66°C, and continue stirring for 15 minutes after the yellow powder is dissolved.
[0041] S5. Turn off the heating of the liquid in S4, continue stirring, and cool to room temperature. A light yellow crystalline powder will precipitate from the solution.
[0042] S6. The material in S5 was filtered under reduced pressure at -0.1 MPa for solid-liquid separation (using a φ150 mm Buchner funnel, a 5000 mL suction flask, and medium-speed qualitative filter paper) to obtain a light yellow crystalline powder. The powder was washed once with 650 g of anhydrous ethanol.
[0043] S7. The washed light yellow powder was dried at 80° C. for 8 hours to obtain 491.4 g of phosphine-nitrogen-containing flame retardant “1,3-PBO-DOPO” with a yield of 81.90%.
[0044] Example 2
[0045] A method for preparing a novel phosphine-nitrogen flame retardant based on DOPO and 2,2'-(1,3-phenylene)-dioxazoline, comprising the following steps:
[0046] S1. In a 50 L glass reactor (double-layer glass reactor, Lansgate Equipment Engineering Co., Ltd., model SF-50L), add 4100 g of DOPO, 2000 g of PBO, 45 g of anhydrous zinc acetate, and 22,000 g of xylene. Fill with nitrogen at a flow rate of 0.1 L / min, start stirring (stirring speed is 200 rpm), heat to 125°C, start stirring, and reflux for 11 hours.
[0047] S2. Turn off the heating of the reaction phase in the above step "1", continue stirring, and cool to room temperature. A light yellow powder solid will precipitate from the solution.
[0048] S3. The feed liquid in S2 was filtered under reduced pressure at -0.1 MPa for solid-liquid separation (using a φ350 mm Buchner funnel, a 25000 mL suction flask, and medium-speed qualitative filter paper) to obtain a light yellow powder.
[0049] S4. In a 50 L glass reactor (double-layer glass reactor, Lansget Equipment Engineering Co., Ltd., model SF-50L), add the light yellow powder in S3 and 38,000 g of anhydrous ethanol, fill with nitrogen at a flow rate of 0.1 L / min, start stirring (stirring speed is 200 r / min), heat to 70°C, and continue stirring for 15 minutes after the yellow powder is dissolved.
[0050] S5. Turn off the heating of the liquid in S4, continue stirring, and cool to room temperature. A light yellow crystalline powder will precipitate from the solution.
[0051] S6. The material in S5 was filtered under reduced pressure at -0.1 MPa for solid-liquid separation (using a φ350 mm Buchner funnel, a 25000 mL suction flask, and medium-speed qualitative filter paper) to obtain a light yellow crystalline powder. The powder was washed twice with 7000 g of anhydrous ethanol each time.
[0052] S7. The washed light yellow powder was dried at 80° C. for 9 hours to obtain 5071.3 g of phosphine-nitrogen-containing flame retardant “1,3-PBO-DOPO” with a yield of 84.52%.
[0053] Example 3
[0054] A method for preparing a novel phosphine-nitrogen flame retardant based on DOPO and 2,2'-(1,3-phenylene)-dioxazoline, comprising the following steps:
[0055] S1. In a 50 L glass reactor (double-layer glass reactor, Lansgate Equipment Engineering Co., Ltd., model SF-50L), add 4300 g of DOPO, 2000 g of PBO, 70 g of anhydrous zinc acetate, and 23,000 g of xylene. Fill with nitrogen at a flow rate of 0.1 L / min, start stirring (stirring speed is 200 rpm), heat to 130°C, start stirring, and reflux for 12 hours.
[0056] S2. Turn off the heating of the reaction phase in the above step "1", continue stirring, and cool to room temperature. A light yellow powder solid will precipitate from the solution.
[0057] S3. The feed liquid in S2 was filtered under reduced pressure at -0.1 MPa for solid-liquid separation (using a φ350 mm Buchner funnel, a 25000 mL suction flask, and medium-speed qualitative filter paper) to obtain a light yellow powder.
[0058] S4. In a 50 L glass reactor (double-layer glass reactor, Lansget Equipment Engineering Co., Ltd., model SF-50L), add the light yellow powder in S3 and 39,000 g of anhydrous ethanol, fill with nitrogen at a flow rate of 0.1 L / min, start stirring (stirring speed is 200 r / min), heat to 70°C, and continue stirring for 20 minutes after the yellow powder is dissolved.
[0059] S5. Turn off the heating of the liquid in S4, continue stirring, and cool to room temperature. A light yellow crystalline powder will precipitate from the solution.
[0060] S6. The material in S5 was filtered under reduced pressure at -0.1 MPa for solid-liquid separation (using a φ350 mm Buchner funnel, a 25000 mL suction flask, and medium-speed qualitative filter paper) to obtain a light yellow crystalline powder. The powder was washed twice with 7000 g of anhydrous ethanol each time.
[0061] S7. The washed light yellow powder was dried at 80° C. for 10 hours to obtain 5091.6 g of phosphine-nitrogen-containing flame retardant “1,3-PBO-DOPO” with a yield of 84.86%.
[0062] Figure 1 The high performance liquid chromatography (HPLC) test chart shows that the peak area percentage is 98.208% at a retention time of 4.858 min, indicating that the content of the flame retardant monomer prepared according to the process of the present invention can be greater than 98%.
[0063] Figure 2 The TG test graph shows that when the temperature reaches 299.6°C, the thermal weight loss reaches 1%; when the temperature reaches 326.3°C, the thermal weight loss reaches 5%, indicating that the flame retardant prepared by the present invention has a thermal stability greater than 290°C.
[0064] Figure 3 Fourier transform infrared (FTIR) analysis revealed characteristic absorption peaks for P=O at 1199.291 cm⁻¹, PO-Ph at 909.313 cm⁻¹, P-Ph at 1475.410 cm⁻¹, C=O at 1651.277 cm⁻¹, and PN at 1043.940 cm⁻¹. Furthermore, the absence of a characteristic pH peak at 2384.284 cm⁻¹ in the DOPO spectrum indicated that the pale yellow powder product was 1,3-PBO-DOPO.
[0065] Figure 4 Torque rheometer test data of medium flame retardant 1,3-PBO-DOPO.
[0066] Prepared by mass percentage
[0067] Sample 1#: 100% PET
[0068] Sample #2: 97% PET and 3% 1,3-PBO-DOPO
[0069] Sample #3: 97% PET and 3% DOPO
[0070] Three samples.
[0071] The torque change was measured using a torque rheometer at 260°C. The test data is shown in the figure below. The test data shows that the torque changes of samples 1# and 2# are almost identical, indicating no significant change in the viscosity of the fluids. However, the torque of sample 3#, after mixing PET with DOPO, decreases significantly, reflecting a significant decrease in the viscosity of the fluid. This demonstrates that the novel flame retardant prepared in this invention does not cause rapid degradation of the polyester material during the PET mixing process, nor does it undergo transesterification reactions that would affect the fluid viscosity.
[0072] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A novel phosphine-nitrogen flame retardant based on DOPO and 2,2'-(1,3-phenylene)-bisoxazoline, characterized in that: The structural formula is as follows:
2. A method for preparing a novel phosphine-nitrogen flame retardant based on DOPO and 2,2'-(1,3-phenylene)-bisoxazoline according to claim 1, characterized in that: Here are the steps: S1. Add DOPO, PBO, anhydrous zinc acetate catalyst, xylene or chlorobenzene to a glass reaction vessel or glass-lined reactor, fill with nitrogen, start stirring, heat, stir, and reflux; S2. Turn off the heating of the reaction phase in step S1, continue stirring, and cool to room temperature to precipitate a light yellow powder solid in the solution; S3, separating the liquid-solid mixture in S2 to obtain a light yellow powder; S4. Add the light yellow powder and anhydrous ethanol from S3 to a glass reaction vessel or a glass-lined reactor, fill with nitrogen, start stirring, heat, and continue stirring until the yellow powder dissolves; S5. Turn off the heating of the liquid in S4, continue stirring, and cool to room temperature to precipitate a light yellow crystalline powder from the solution; S6, separating the solid and liquid of the material in S5 to obtain a light yellow crystalline powder; washing with anhydrous ethanol; S7. Drying the washed light yellow powder to obtain the flame retardant of the present invention.
3. The method for preparing a novel phosphine-nitrogen flame retardant based on DOPO and 2,2'-(1,3-phenylene)-bisoxazoline according to claim 2, characterized in that: In step S1, the weight parts of each component are: 10-11 parts of DOPO, 5 parts of PBO, 0.1-0.2 parts of anhydrous zinc acetate as catalyst, and 50-60 parts of xylene or chlorobenzene.
4. The method for preparing a novel phosphine-nitrogen flame retardant based on DOPO and 2,2'-(1,3-phenylene)-bisoxazoline according to claim 2, characterized in that: In the step S1, heating to 120-130° C. Reflux for 10 to 12 hours.
5. The method for preparing a novel phosphine-nitrogen flame retardant based on DOPO and 2,2'-(1,3-phenylene)-bisoxazoline according to claim 2, characterized in that: In step S4, the weight portion of anhydrous ethanol is 90 to 100 parts; the heating temperature is 65 to 70° C.; and the stirring time is 10 to 20 minutes.
6. The method for preparing a novel phosphine-nitrogen flame retardant based on DOPO and 2,2'-(1,3-phenylene)-bisoxazoline according to claim 2, characterized in that: In step S6, washing is performed twice with anhydrous ethanol.
7. The method for preparing a novel phosphine-nitrogen flame retardant based on DOPO and 2,2'-(1,3-phenylene)-bisoxazoline according to claim 2, characterized in that: In step S7, the product is dried at 80° C. for 8 to 10 hours.
8. Use of the novel phosphine-nitrogen flame retardant based on DOPO and 2,2'-(1,3-phenylene)-bisoxazoline according to claim 1 in PET resin.
Citation Information
Patent Citations
Phosphorus-containing flame retardant, flame-retarding polyester thin film and preparation methods thereof
CN102634064A
9,10-dihydro-9-oxa-10-phosphenanthrene-10-oxide (DOPO) group phosphorus-nitrogen flame retardant and preparation method and application thereof
CN103059339A
Novel phosphorus-nitrogen flame retardant and preparation method thereof
CN110643066A
Flame retardant resin composition
US20070173572A1