High-strength high-temperature-resistant PPO alloy and preparation method thereof
By reasonably combining PPO resin, silicone rubber, nanoceramics and compatibility agents in PPO alloys, high-strength and high-temperature resistance PPO alloys are prepared, which solves the problem that PPO alloys cannot take into account both high-strength and high-temperature resistance, and realizes the practical application performance improvement.
Patent Information
- Application Number
- CN202411083137.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
PPO alloys cannot take into account both high strength and high temperature resistance, and there is a problem of insufficient performance in practical applications.
Prepare by mixing PPO resin, silicone rubber, nanoceramics and compatibility agent in a specific proportion and undergoing melt extrusion treatment to form a high-strength, high-temperature resistant PPO alloy. Specific components include PPO resin, silicone rubber, nanoceramics and compatibility agents. Nanocerites include metal oxides, nanocarbon materials and nitride nanoparticles. The compatibility agent is styrene-methyl methacrylate copolymer, etc., which is reasonable. Compatible components for synergistic effects.
It realizes the performance of PPO alloys that take into account both high strength and high temperature resistance, improves mechanical strength and high temperature resistance, and is suitable for medical devices, mechanical and electrical industries and other fields.
Smart Images

Figure BDA0004985163360000101 
Figure BDA0004985163360000111 
Figure BDA0004985163360000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of PPO, and in particular to a high-strength and high-temperature-resistant PPO alloy and a preparation method thereof. Background Art
[0002] Polyphenylene oxide (PPO) is a thermoplastic engineering plastic widely used in medical devices, electromechanical industry, electronics, electrical and other fields. In practical applications, PPO is usually mixed with other resins and additives to form alloys, which have more excellent physical, chemical or mechanical properties. However, in the related art, PPO alloys cannot take into account both high strength and high temperature resistance. Therefore, it is urgent to provide a high-strength and high temperature resistant PPO alloy and a preparation method thereof. Summary of the invention
[0003] In view of the technical problem that the above-mentioned PPO alloy cannot achieve both high strength and high temperature resistance, the present invention provides a high-strength and high-temperature resistant PPO alloy and a preparation method thereof, wherein the PPO alloy can achieve both high strength and high temperature resistance.
[0004] In a first aspect, the present invention provides a high-strength and high-temperature-resistant PPO alloy, wherein the PPO alloy comprises the following components in parts by weight:
[0005] PPO resin, 100 parts by weight;
[0006] Silicone rubber, based on 100 parts by weight of the PPO resin, the content of the silicone rubber in the PPO alloy is 25 parts by weight to 50 parts by weight;
[0007] Nano-ceramics, based on 100 parts by weight of the PPO resin, the content of the nano-ceramics in the PPO alloy is 5 parts by weight to 15 parts by weight;
[0008] The compatibilizer is contained in the PPO alloy in an amount of 5 to 10 parts by weight based on 100 parts by weight of the PPO resin.
[0009] According to any of the aforementioned embodiments of the present invention, the PPO alloy further comprises the following components by weight:
[0010] Silicone rubber, 30 to 40 parts by weight;
[0011] Nano ceramics, 6 to 10 parts by weight;
[0012] Compatibilizer, 6 to 9 parts by weight.
[0013] According to any of the aforementioned embodiments of the present invention, the weight average molecular weight of the silicone rubber is 200,000 to 500,000.
[0014] According to any of the aforementioned embodiments of the present invention, the nano-ceramic includes at least one of metal oxide nano-particles, nano-carbon materials and nitride nano-particles.
[0015] According to any of the aforementioned embodiments of the present invention, the nano-ceramic comprises metal oxide nanoparticles, and the metal oxide nanoparticles comprise at least one of zinc oxide nanoparticles, titanium oxide nanoparticles and magnesium oxide nanoparticles.
[0016] According to any of the aforementioned embodiments of the present invention, the nanoceramic includes a nanocarbon material, and the nanocarbon material includes at least one of a nanotube and a nanofiber.
[0017] According to any of the foregoing embodiments of the present invention, the nano-ceramic comprises nitride nano-particles, and the nitride nano-particles comprise at least one of silicon nitride and boron nitride.
[0018] According to any of the aforementioned embodiments of the present invention, the nanoceramic includes metal oxide nanoparticles, nanocarbon materials and nitride nanoparticles, and the weight ratio of the metal oxide nanoparticles, the nanocarbon material and the nitride nanoparticles is 1:(1-2):1.
[0019] According to any of the aforementioned embodiments of the present invention, the PPO alloy further comprises the following components by weight:
[0020] The anti-aging agent is contained in the PPO alloy in an amount of 2 to 5 parts by weight based on 100 parts by weight of the PPO resin.
[0021] According to any of the aforementioned embodiments of the present invention, the anti-aging agent includes at least one of 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,4-bis[(octylthio)methyl]-6-methylphenol, p-methoxyphenol, N,N-di(octadecyl)hydroxylamine and tris(2,4-di-tert-butylphenyl) phosphite.
[0022] According to any of the aforementioned embodiments of the present invention, the compatibilizer includes at least one of styrene-methyl methacrylate copolymer, styrene-maleic anhydride copolymer and styrene-vinyl acetate copolymer.
[0023] In a second aspect, the present invention provides a method for preparing a PPO alloy as described in any embodiment of the first aspect of the present invention, comprising:
[0024] Mixing PPO resin, silicone rubber, nano-ceramics and a compatibilizer to obtain a mixture;
[0025] The mixed material is melt-extruded and cooled to obtain a PPO alloy.
[0026] The invention provides a high-strength and high-temperature-resistant PPO alloy and a preparation method thereof. The PPO alloy is based on reasonable matching components and matches appropriate weight portions of respective components to exert synergistic effects, so that the PPO alloy has both high-strength and high-temperature-resistant properties.
[0027] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. DETAILED DESCRIPTION
[0028] Unless otherwise specified, the terms used in the present invention have the commonly understood meanings that are generally understood by those skilled in the art.
[0029] Unless otherwise specified, the values of the parameters mentioned in the present invention can be measured by various test methods commonly used in the art, for example, they can be measured according to the test methods given in the embodiments of the present invention.
[0030] In a first aspect, the present invention provides a high-strength and high-temperature-resistant PPO alloy, wherein the PPO alloy comprises the following components by weight:
[0031] PPO resin, 100 parts by weight;
[0032] Silicone rubber, based on 100 parts by weight of PPO resin, the content of silicone rubber in the PPO alloy is 25 parts by weight to 50 parts by weight;
[0033] Nano-ceramics, based on 100 parts by weight of PPO resin, the content of nano-ceramics in the PPO alloy is 5 parts by weight to 15 parts by weight;
[0034] The compatibilizer has a content of 5 to 10 parts by weight based on 100 parts by weight of the PPO resin.
[0035] The high-strength and high-temperature-resistant PPO alloy provided by the present invention is based on reasonable matching of components, matches appropriate weight portions of the respective components, exerts synergistic effects, and enables the PPO alloy to have both high strength and high-temperature resistance properties.
[0036] In the embodiment of the present invention, the PPO resin has excellent high temperature resistance and mechanical strength properties. The high temperature resistance and mechanical strength of the PPO alloy can be further improved by selecting a suitable type of PPO resin and matching it with other components, and controlling its weight in the PPO alloy.
[0037] In some embodiments of the present invention, the weight average molecular weight of the PPO resin may be 25000 to 35000. When the weight average molecular weight of the PPO resin is controlled within the above range, the high temperature resistance and compressive strength of the PPO alloy can be further improved.
[0038] Specifically, in some embodiments, the weight average molecular weight of the PPO resin can be, but is not limited to, 25000, 25500, 26000, 26500, 27000, 27500, 28000, 28500, 29000, 29500, 30000, 30500, 31000, 31500, 32000, 32500, 33000, 33500, 34000, 34500, 35000, or a range consisting of any two values in the range of 25000 to 35000.
[0039] In the above embodiment, the PPO resin can be purchased from the market, such as LXR35 and LXR40 of Bluestar Chemical New Materials Co., Ltd.
[0040] In the PPO alloy provided by the embodiment of the present invention, the silicone rubber has good compatibility with other components such as PPO resin, which can make the alloy have excellent high temperature resistance, mechanical strength and processing performance. The high temperature resistance, mechanical strength and processing performance of the PPO alloy can also be further improved by selecting suitable types of silicone rubber and other components and controlling their weight in the PPO alloy.
[0041] In some embodiments of the present invention, the silicone rubber may include dimethyl silicone rubber and / or methyl vinyl silicone rubber.
[0042] In some embodiments of the present invention, the weight average molecular weight of the silicone rubber is 200,000 to 500,000. Controlling the weight average molecular weight of the silicone rubber within the above range can further help improve the high temperature resistance, mechanical strength and processing performance of the alloy.
[0043] Exemplarily, the weight average molecular weight of the silicone rubber can be, but is not limited to, 200,000, 210,000, 220,000, 230,000, 240,000, 250,000, 260,000, 270,000, 280,000, 290,000, 300,000, 310,000, 320,000, 330,000, 340,000, 350,000, 360,000, 370,000, 380,000, 390,000, 400,000, 410,000, 420,000, 430,000, 440,000, 450,000, 460,000, 470,000, 480,000, 490,000, 500,000, or a range consisting of any two values between 200,000 and 500,000.
[0044] In some specific embodiments, based on 100 parts by weight of PPO resin, the content of silicone rubber in the PPO alloy can be, but is not limited to, 25 parts by weight, 26 parts by weight, 27 parts by weight, 28 parts by weight, 29 parts by weight, 30 parts by weight, 31 parts by weight, 32 parts by weight, 33 parts by weight, 34 parts by weight, 35 parts by weight, 36 parts by weight, 37 parts by weight, 38 parts by weight, 39 parts by weight, 40 parts by weight, 41 parts by weight, 42 parts by weight, 43 parts by weight, 44 parts by weight, 45 parts by weight, 46 parts by weight, 47 parts by weight, 48 parts by weight, 49 parts by weight, 50 parts by weight, or a range consisting of any two values from 25 parts by weight to 50 parts by weight.
[0045] In the PPO alloy provided by the present invention, nano-ceramics can help improve the high temperature resistance and mechanical strength of the PPO alloy. The high temperature resistance and mechanical strengths such as tensile strength, yield strength, and compressive strength of the PPO alloy can also be further improved by selecting suitable types of nano-ceramics to be matched with other components and controlling their weight in the PPO alloy.
[0046] In some embodiments of the present invention, the nanoceramic includes at least one of metal oxide nanoparticles, nanocarbon materials and nitride nanoparticles. The above nanoparticles can make the PPO alloy have higher high temperature resistance and mechanical strength such as tensile strength, yield strength and compressive strength.
[0047] In some embodiments, the nanoceramic includes metal oxide nanoparticles, and the metal oxide nanoparticles include at least one of zinc oxide nanoparticles, titanium oxide nanoparticles, and magnesium oxide nanoparticles.
[0048] In other embodiments, the nanoceramic includes a nanocarbon material, and the nanocarbon material includes at least one of a nanotube and a nanofiber.
[0049] In some other embodiments, the nanoceramic includes nitride nanoparticles, and the nitride nanoparticles include at least one of silicon nitride and boron nitride.
[0050] In some specific embodiments, the nanoceramic includes metal oxide nanoparticles, nanocarbon materials, and nitride nanoparticles, and the weight ratio of the metal oxide nanoparticles, the nanocarbon materials, and the nitride nanoparticles is 1:(1-2):1.
[0051] In some embodiments of the present invention, based on 100 parts by weight of PPO resin, the content of nanoceramics in the PPO alloy can be but is not limited to 5 parts by weight, 5.5 parts by weight, 6 parts by weight, 6.5 parts by weight, 7 parts by weight, 7.5 parts by weight, 8 parts by weight, 8.5 parts by weight, 9 parts by weight, 9.5 parts by weight, 10 parts by weight or a range consisting of any two values from 5 parts by weight to 10 parts by weight.
[0052] In the PPO alloy provided by the present invention, the compatibilizer can help improve the compatibility between the PPO resin, silicone rubber, nano-ceramics and other components, so that they can be better matched to exert a synergistic effect.
[0053] In some embodiments of the present invention, the compatibilizer includes at least one of styrene-methyl methacrylate copolymer, styrene-maleic anhydride copolymer, and styrene-vinyl acetate copolymer.
[0054] In some embodiments of the present invention, based on 100 parts by weight of PPO resin, the content of the compatibilizer in the PPO alloy may be, but is not limited to, 5 parts by weight, 5.5 parts by weight, 6 parts by weight, 6.5 parts by weight, 7 parts by weight, 7.5 parts by weight, 8 parts by weight, 8.5 parts by weight, 9 parts by weight, 9.5 parts by weight, 10 parts by weight or a range consisting of any two values from 5 parts by weight to 10 parts by weight.
[0055] In some specific embodiments of the present invention, the PPO alloy further comprises the following components by weight:
[0056] Silicone rubber, 30 to 40 parts by weight;
[0057] Nano ceramics, 6 to 10 parts by weight;
[0058] Compatibilizer, 6 to 9 parts by weight.
[0059] Other suitable additives may be added to the PPO alloy provided by the present invention to increase its service life, such as anti-aging agents and antioxidants.
[0060] In some embodiments, the PPO alloy further comprises the following components by weight: an anti-aging agent, wherein the content of the anti-aging agent in the PPO alloy is 2 to 5 parts by weight based on 100 parts by weight of the PPO resin.
[0061] In some specific embodiments, based on 100 parts by weight of PPO resin, the content of the anti-aging agent in the PPO alloy can be but is not limited to 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight, 4.5 parts by weight, 5 parts by weight or a range consisting of any two values between 2 parts by weight and 5 parts by weight.
[0062] In some embodiments, the anti-aging agent includes at least one of 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,4-bis[(octylthio)methyl]-6-methylphenol, p-methoxyphenol, N,N-dioctadecylhydroxylamine and tris(2,4-di-tert-butylphenyl) phosphite.
[0063] In a second aspect, the present invention provides a method for preparing a PPO alloy as in any embodiment of the first aspect of the present invention, comprising:
[0064] Mixing PPO resin, silicone rubber, nano-ceramics and a compatibilizer to obtain a mixture;
[0065] The mixed material is melt-extruded and cooled to obtain a PPO alloy.
[0066] The following embodiments describe the contents disclosed in the present application in more detail, and these embodiments are only used for illustrative explanations, because it is obvious to those skilled in the art that various modifications and changes are made within the scope of the present application disclosure. Unless otherwise stated, all parts, percentages and ratios reported in the following embodiments are based on mass, and all reagents used in the embodiments are commercially available or synthesized according to conventional methods, and can be used directly without further processing, and the instruments used in the embodiments are commercially available.
[0067] Example 1
[0068] This embodiment provides a method for preparing a PPO alloy, comprising the following steps:
[0069] 100 parts by weight of PPO resin (LXR35 purchased from Bluestar Chemical New Materials Co., Ltd., with a weight average molecular weight of 28,000), 30 parts by weight of methyl vinyl silicone rubber (Foshan Simei Organic Silicone Material Co., Ltd., with a weight average molecular weight of 300,000), 6 parts by weight of zinc oxide nanoparticles (Ningbo Beijiaer New Materials Co., Ltd.) and 6 parts by weight of styrene-methyl methacrylate copolymer (MS750, Nippon Steel) were mixed to obtain a mixture;
[0070] The mixed material is added into a twin-screw extruder, and the PPO alloy is prepared through extrusion, cooling and granulation, wherein the extrusion temperature is 300°C.
[0071] Example 2
[0072] The preparation method of this embodiment is similar to that of embodiment 1, except that: 40 parts by weight of methyl vinyl silicone rubber.
[0073] Example 3
[0074] The preparation method of this embodiment is similar to that of embodiment 1, except that: 50 parts by weight of methyl vinyl silicone rubber.
[0075] Example 4
[0076] The preparation method of this embodiment is similar to that of embodiment 1, except that: 10 parts by weight of zinc oxide nanoparticles.
[0077] Example 5
[0078] The preparation method of this embodiment is similar to that of embodiment 1, except that: 13 parts by weight of zinc oxide nanoparticles.
[0079] Example 6
[0080] The preparation method of this embodiment is similar to that of embodiment 1, except that the weight average molecular weight of the PPO resin is 30,000, and the resin is purchased from Bluestar Chemical New Materials Co., Ltd. as LXR40.
[0081] Example 7
[0082] The preparation method of this embodiment is similar to that of embodiment 1, except that the weight average molecular weight of the PPO resin is 34,000, and the resin is purchased from Bluestar Chemical New Materials Co., Ltd. as LXR40.
[0083] Example 8
[0084] The preparation method of this embodiment is similar to that of embodiment 1, except that the weight average molecular weight of the methyl vinyl silicone rubber is 400,000.
[0085] Example 9
[0086] The preparation method of this embodiment is similar to that of embodiment 1, except that the weight average molecular weight of the methyl vinyl silicone rubber is 450,000.
[0087] Example 10
[0088] The preparation method of this embodiment is similar to that of embodiment 1, except that the nanoceramic is a nanofiber having a length of 5 mm and an outer diameter of 20 μ□m.
[0089] Embodiment 11
[0090] The preparation method of this embodiment is similar to that of embodiment 1, except that the nano-ceramic is boron nitride.
[0091] Example 12
[0092] The preparation method of this embodiment is similar to that of embodiment 1, except that the nanoceramic is a mixture of 2 parts by weight of titanium oxide nanoparticles, 2 parts by weight of nanofibers and 2 parts by weight of boron nitride, wherein the nanofibers have a length of 5 mm and an outer diameter of 20 μm.
[0093] Embodiment 13
[0094] The preparation method of this embodiment is similar to that of embodiment 1, except that 3 parts by weight of p-methoxyphenol is further included.
[0095] Comparative Example 1
[0096] The preparation method of this comparative example is similar to that of Example 1, except that there is no methyl vinyl silicone rubber component.
[0097] Comparative Example 2
[0098] The preparation method of this comparative example is similar to that of Example 1, except that polypropylene with the same weight average molecular weight is used to replace the methyl vinyl silicone rubber.
[0099] Comparative Example 3
[0100] The preparation method of this comparative example is similar to that of Example 1, except that there is no nano-ceramic component.
[0101] Comparative Example 4
[0102] The preparation method of this comparative example is similar to that of Example 1, except that: 10 parts by weight of methyl vinyl silicone rubber.
[0103] Comparative Example 5
[0104] The preparation method of this comparative example is similar to that of Example 1, except that: 55 parts by weight of methyl vinyl silicone rubber.
[0105] Comparative Example 6
[0106] The preparation method of this comparative example is similar to that of Example 1, except that: 3 parts by weight of zinc oxide nanoparticles.
[0107] Test Section
[0108] The PPO alloys of the embodiments and comparative examples were subjected to the following performance tests.
[0109] (1) Tensile strength and elongation at break test
[0110] The tensile strength and elongation at break were tested in accordance with GB / T 2951.11-2008. The test results are shown in Table 1.
[0111] (2) High temperature resistance test
[0112] The glass transition temperature (Tg) of the PPO alloy was measured on a DSC-25 differential scanning calorimeter, wherein the test conditions were: N2 atmosphere, a heating rate of 15°C / min, and a temperature range of 25°C to 400°C.
[0113] (3) Aging resistance test
[0114] After the test sample was placed at 180°C and aged for 240 hours, it was tested according to GB / T 2951.11-2008 to obtain the tensile strength and elongation at break after aging. The test results are shown in Table 1.
[0115] Table 1 Test results of embodiments and comparative examples
[0116]
[0117]
[0118]
[0119] According to Table 1, by comparing the test results of Examples 1-13 and Comparative Examples 1-6, it can be seen that the high-strength and high-temperature-resistant PPO alloy provided by the present invention matches the appropriate weight portions of each component on the basis of reasonable matching components to exert a synergistic effect, so that the PPO alloy has both high strength and high temperature resistance properties.
[0120] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them; although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention. In particular, as long as there is no structural conflict, the various technical features mentioned in each embodiment can be combined in any way. The present invention is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A high-strength and high-temperature resistant PPO alloy, characterized in that: The PPO alloy comprises the following components by weight: PPO resin, 100 parts by weight; Silicone rubber, based on 100 parts by weight of the PPO resin, the content of the silicone rubber in the PPO alloy is 25 parts by weight to 50 parts by weight; Nano-ceramics, based on 100 parts by weight of the PPO resin, the content of the nano-ceramics in the PPO alloy is 5 parts by weight to 15 parts by weight; The compatibilizer is contained in the PPO alloy in an amount of 5 to 10 parts by weight based on 100 parts by weight of the PPO resin.
2. The PPO alloy according to claim 1, characterized in that The PPO alloy further comprises the following components by weight: Silicone rubber, 30 to 40 parts by weight; Nano ceramics, 6 to 10 parts by weight; Compatibilizer, 6 to 9 parts by weight.
3. The PPO alloy according to claim 1 or 2, characterized in that: The weight average molecular weight of the silicone rubber is 200,000 to 500,000.
4. The PPO alloy according to claim 1 or 2, characterized in that: The nano-ceramic includes at least one of metal oxide nano-particles, nano-carbon materials and nitride nano-particles.
5. The PPO alloy according to claim 4, characterized in that The nano-ceramic comprises metal oxide nanoparticles, and the metal oxide nanoparticles comprise at least one of zinc oxide nanoparticles, titanium oxide nanoparticles and magnesium oxide nanoparticles; And / or, the nano-ceramic includes a nano-carbon material, and the nano-carbon material includes at least one of a nano-tube and a nano-fiber; And / or, the nano-ceramic includes nitride nano-particles, and the nitride nano-particles include at least one of silicon nitride and boron nitride.
6. The PPO alloy according to claim 4, characterized in that The nano-ceramic comprises metal oxide nano-particles, nano-carbon materials and nitride nano-particles, and the weight ratio of the metal oxide nano-particles, the nano-carbon materials and the nitride nano-particles is 1:(1-2):
1.
7. The PPO alloy according to claim 1, characterized in that The PPO alloy further comprises the following components by weight: The anti-aging agent is contained in the PPO alloy in an amount of 2 to 5 parts by weight based on 100 parts by weight of the PPO resin.
8. The PPO alloy according to claim 7, characterized in that: The anti-aging agent includes at least one of 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,4-bis[(octylthio)methyl]-6-methylphenol, p-methoxyphenol, N,N-dioctadecylhydroxylamine and tris(2,4-di-tert-butylphenyl)phosphite.
9. The PPO alloy according to claim 1, characterized in that: The compatibilizer includes at least one of styrene-methyl methacrylate copolymer, styrene-maleic anhydride copolymer and styrene-vinyl acetate copolymer.
10. A method for preparing a PPO alloy as claimed in any one of claims 1 to 9, characterized in that: include: Mixing PPO resin, silicone rubber, nano-ceramics and a compatibilizer to obtain a mixture; The mixed material is melt-extruded and cooled to obtain a PPO alloy.
Citation Information
Patent Citations
Polyphenylene oxide resin composition and method for inhibiting discoloration of polyphenylene oxide resin
CN101423658A
Polyphenyl ether composite material and preparation method of polyphenyl ether composite material
CN102876003A
High-impact-resistance high-temperature-resisting halogen-free flame-retardant PPO (Polyphenylene Oxide) alloy material and preparation method thereof
CN109265963A
Flame-retardant polyphenylene oxide (PPO) alloy special for fuel cell and preparation method of PPO alloy
CN109294202A
Surface-hydrophobic nano ceramic resin composite material, preparation method and application