Hot-processable polybutyrolactam and preparation method thereof
By introducing long-chain hyperbranched polymers into polybutylactam for ring-opening polymerization, the problems of non-melt processing and high brittleness are solved, high thermal stability and good mechanical properties are achieved, and its application prospects are broadened.
Patent Information
- Application Number
- CN202410970331.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-01
AI Technical Summary
Polybutylactam is limited in commercial applications due to its high density of amide groups on the molecular chain, resulting in non-melt processing and high brittleness.
Polybutyracam is modified in situ by long-chain hyperbranched polymer, and the thermal stability and processability are improved by performing ring-opening polymerization at room temperature.
The elongation and mechanical strength of polybutyracam were significantly improved, with melting point below 235℃, thermal decomposition temperature above 270℃, and tensile strength of 40~70MPa, and elongation of break of 15~40%, improving Its non-melt processing and brittleness problems are solved.
Smart Images

Figure CN118879063A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of high molecular polymers, and in particular relates to a heat-processable polybutyrolactam and a preparation method thereof. Background Art
[0002] Polyamide, commonly known as nylon (PA), is a general term for thermoplastic resins containing repeated amide groups on the main chain of the molecule. As the first of the five major engineering materials, polyamide is gradually replacing some metals and ceramic glass materials, and is widely used in many fields such as aerospace, machinery industry, biomedicine, clothing and accessories.
[0003] As more and more non-degradable plastic products are discarded, they have caused serious damage to the ecosystem. Therefore, the recycling and resource utilization of polymer materials is a crucial issue. Polybutyrolactam (PA4) can be prepared from bio-based raw materials and can be completely degraded in the natural environment within a few months. It has good hygroscopicity, wear resistance and heat resistance, which makes PA4 have broad application prospects in packaging engineering, textile industry, mechanical engineering, etc.
[0004] However, due to the extremely high density of amide groups on the PA4 molecular chain and the strong hydrogen bonding between the molecular chains, PA4 has the disadvantages of being non-melt processable and highly brittle, which greatly limits its commercial application. Therefore, widening the thermal processing window and improving toughness are the key points in the research of PA4 materials.
[0005] In recent years, hyperbranched polymers have been widely used to improve the processability and toughness of polymers due to their good solubility, low viscosity, and high thermal stability. Long-chain hyperbranched polymers combine the advantages of hyperbranched polymers and linear polymers, retaining the advantages of small hydrodynamic volume and low viscosity of hyperbranched polymers while increasing the chain entanglement between molecules. When they are used to modify linear polymers, they can effectively inhibit the long-range order of the polymer microphase separation structure and improve the processability and toughness of the polymer group. Summary of the invention
[0006] In view of this, the object of the present invention is to provide a heat-processable polybutyrolactam and a preparation method thereof, and to in-situ modify PA4 using a long-chain hyperbranched polymer that is flowable at room temperature and has high thermal stability, thereby improving the problems of PA4 being non-melt processable and having high brittleness.
[0007] In order to achieve the above-mentioned invention object, the present invention provides the following technical solutions:
[0008] A method for preparing heat-processable polybutyrolactam comprises the following steps:
[0009] Step (1), adding butyrolactam and an alkali catalyst into container A and mixing them evenly to obtain a mixed solution;
[0010] Step (2), adding butyrolactam and the first initiator into container B and mixing them evenly, and then adding the long-chain hyperbranched polymer into container B and mixing them evenly;
[0011] Step (3), pouring the mixed solution in container A into container B to carry out a ring-opening polymerization reaction to obtain heat-processable polybutyrolactam.
[0012] Preferably, in step (1), the amount of base catalyst added is 1-10% of the mass fraction of butyrolactam; the reaction conditions of butyrolactam and base catalyst are: reacting at 40-100° C. for 0.5-4 h under the protection of inert gas.
[0013] Preferably, in step (1), the base catalyst is selected from one or more of sodium tert-butoxide, potassium tert-butoxide, sodium hydroxide and potassium hydroxide.
[0014] Preferably, in step (2), the amount of the first initiator added is 0.1-3% of the mass fraction of butyrolactam; the reaction conditions of butyrolactam and the initiator are: under the protection of inert gas, react at 30-45° C. for 0.5-1 h.
[0015] Preferably, in step (2), the first initiator is selected from one or more of benzoyl chloride, oxalyl chloride, acetyl chloride, tetradecanoyl chloride and diisocyanate.
[0016] Preferably, in step (2), the amount of long-chain hyperbranched polymer added is 3-20% of the mass fraction of butyrolactam; after the long-chain hyperbranched polymer is added, the mixing conditions are: stirring at 30-45° C. for 0.5-1 h under the protection of inert gas.
[0017] Preferably: in step (2), the long-chain hyperbranched polymer is obtained by polymerizing a binary active olefin group, a multi-active thiol group, and a second initiator in a solvent through a "thiol-ene" click reaction, and then inactivated with a capping agent;
[0018] Wherein, the binary active olefin group is one or more of diacrylate polyethylene glycol (CH2=CHCOO-(C2H4O)n-COCH=CH2, wherein n=3-25), diene polyethylene glycol (CH2=CHCH3-(C2H4O)n-CH3CH=CH2, wherein n=3-25), diacrylamide polyethylene glycol (CH2=CHCONH-(C2H4O)n-CONHCH=CH2, wherein n=3-25), diacrylate polyethylene (CH2=CHCOO-(C2H4)n-COCH=CH2, wherein n=3-25), diene polyethylene (CH2=CHCH3-(C2H4)n-CH3CH=CH2, wherein n=3-25) and diacrylamide polyethylene (CH2=CHCONH-(C2H4)n-CONHCH=CH2, wherein n=3-25);
[0019] The polyvalent active mercapto group is one or more of trimercaptomethane, trimercaptopropane, trimercaptobenzene, trimercaptosilane, trimercaptophosphorus, thiocyanuric acid, trimethylolpropane tris(thioglycolic acid), tetramercaptobenzene and pentaerythritol tetrakis(3-mercaptopropionic acid);
[0020] The second initiator is selected from one or more of azobisisobutyronitrile, benzoyl peroxide, dimethylaminopyridine, dibutyl phosphate and hydroxycyclohexane phenone;
[0021] Wherein, the solvent is selected from one or more of dichloromethane, chloroform, tetrahydrofuran, benzophenone and toluene, and the solution concentration is 5 to 20 wt%;
[0022] Wherein, the end-capping agent is one or more of methyl crotonate, acrylate, 2-allylphenol, eugenol, methyl eugenol, 3-allyl-N,N-dimethylaniline and bisphenol S monopropylene ether.
[0023] Preferably: the conditions of the "thiol-ene" click reaction are:
[0024] The binary active alkenyl group, the multi-active thiol group and 0.5-3wt% of the second initiator are dissolved in a solvent, reacted at 50-90°C for 0.5-24h, and then a capping agent is added to react at 50-90°C for 0.5-24h, the solution after the reaction is precipitated in ether, and dried at 60-100°C for 12h; wherein the active group molar ratio of the multi-active thiol group: alkenyl / thiol=0.5-0.9; the active group molar ratio of the capping agent: alkenyl / thiol=0.2-0.6.
[0025] Preferably, in step (3), the ring-opening polymerization reaction conditions are: reaction at 40-70° C. for 4-24 hours.
[0026] The embodiment of the present invention further provides a heat-processable polybutyrolactam, which is prepared by the above-mentioned preparation method.
[0027] The invention improves the problem that polybutyrolactam cannot be melt processed by adding a long-chain hyperbranched polymer, significantly improves the elongation at break of polybutyrolactam while maintaining good mechanical strength. Specifically, the melting point of the polybutyrolactam of the invention is lower than 235°C, the thermal decomposition temperature is higher than 270°C, the yield can reach 75-90%, the tensile strength is 40-70MPa, and the elongation at break is 15-40%. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the infrared spectrum of the long-chain hyperbranched polymer LHBP.
[0029] Figure 2 This is the hydrogen nuclear magnetic resonance spectrum of the long-chain hyperbranched polymer LHBP.
[0030] Figure 3 Optical photograph of long-chain hyperbranched polymer LHBP.
[0031] Figure 4 TGA and DTG curves of long-chain hyperbranched polymer LHBP.
[0032] Figure 5 This is the SEM image of the tensile fracture of the long-chain hyperbranched polymer / nylon 4 composite material. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the invention claimed for protection, but merely represents the selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0034] The present invention is further described below in conjunction with specific implementation examples, but the protection scope of the present invention is not limited thereto:
[0035] Example 1
[0036] The preparation method of the long-chain hyperbranched polymer / nylon 4 composite material of this embodiment is as follows:
[0037] 1) Preparation of long-chain hyperbranched polymer LHBP1: A long-chain hyperbranched polymer was prepared by a "thiol-ene" click reaction. Polyethylene glycol 200 (4.2 mL), pentaerythritol tetrakis (3-mercaptopropionic acid) ester (5.8 mL), azobisisobutyronitrile (0.1 g), and toluene (100 mL) were added to a round-bottom flask and mixed evenly. The mixture was reacted for 2 h at 70° C. under a nitrogen atmosphere. Ether was added for precipitation. The supernatant was removed and the organic solvent was removed by rotary evaporation to obtain A2B4-1. Methyl crotonate (20 ml) and azobisisobutyronitrile (0.1 g) were then added. The mixture was reacted for 2 h at 70° C. under a nitrogen atmosphere. Ether was added for precipitation. The supernatant was removed and the organic solvent was removed by rotary evaporation to obtain a transparent and viscous LHBP1.
[0038] 2) Preparation of 10% LHBP1 / PA4 composite material: 25 g of butyrolactam and 1.5 g of base catalyst were added to container A, and the mixture was reacted at 90°C for 2 h under a nitrogen atmosphere. 25 g of butyrolactam and 0.5 g of initiator were added to container B, and the mixture was reacted at 40°C for 0.5 h under a nitrogen atmosphere. Then 5 g of LHBP1 was added to container B, and the mixture was mixed at 40°C for 1 h under a nitrogen atmosphere. When the temperature of the solution in container A dropped to 40°C, the mixed solution in container A was poured into container B, and the mixture was reacted at 40°C for 12 h under a nitrogen atmosphere to obtain heat-processable polybutyrolactam with a yield of 78%.
[0039] Example 2
[0040] The preparation method of the long-chain hyperbranched polymer / nylon 4 composite material of this embodiment is as follows:
[0041] 1) Preparation of long-chain hyperbranched polymer LHBP2: A long-chain hyperbranched polymer was prepared by a "thiol-ene" click reaction. Polyethylene glycol 400 (5.9 mL), pentaerythritol tetrakis (3-mercaptopropionic acid) ester (4.1 mL), azobisisobutyronitrile (0.1 g), and toluene (100 mL) were added to a round-bottom flask and mixed evenly. The mixture was reacted for 2 h at 70° C. under a nitrogen atmosphere. Ether was added to precipitate the mixture. The supernatant was removed and the organic solvent was removed by rotary evaporation to obtain A2B4-2. Methyl crotonate (20 ml) and azobisisobutyronitrile (0.1 g) were then added. The mixture was reacted for 2 h at 70° C. under a nitrogen atmosphere. Ether was added to precipitate the mixture. The supernatant was removed and the organic solvent was removed by rotary evaporation to obtain a transparent and viscous LHBP2.
[0042] 2) Preparation of 10% LHBP2 / PA4 composite material: 25 g of butyrolactam and 1.5 g of base catalyst were added to container A, and the mixture was reacted at 90°C for 2 h under a nitrogen atmosphere. 25 g of butyrolactam and 0.5 g of initiator were added to container B, and the mixture was reacted at 40°C for 0.5 h under a nitrogen atmosphere. Then 5 g of LHBP2 was added to container B, and the mixture was mixed at 40°C for 1 h under a nitrogen atmosphere. When the temperature of the solution in container A dropped to 40°C, the mixed solution in container A was poured into container B, and the mixture was reacted at 40°C for 12 h under a nitrogen atmosphere to obtain heat-processable polybutyrolactam with a yield of 79%.
[0043] Example 3
[0044] The preparation method of the long-chain hyperbranched polymer / nylon 4 composite material of this embodiment is as follows:
[0045] 1) Preparation of long-chain hyperbranched polymer LHBP3: A long-chain hyperbranched polymer was prepared by a "thiol-ene" click reaction. Polyethylene glycol diacrylate 1000 (7.8 mL), pentaerythritol tetrakis (3-mercaptopropionic acid) ester (2.2 mL), azobisisobutyronitrile (0.1 g), and toluene (100 mL) were added to a round-bottom flask and mixed evenly. The mixture was reacted for 2 h at 70° C. under a nitrogen atmosphere. Ether was added to precipitate the mixture. The supernatant was removed and the organic solvent was removed by rotary evaporation to obtain A2B4-3. Methyl crotonate (20 ml) and azobisisobutyronitrile (0.1 g) were then added. The mixture was reacted for 2 h at 70° C. under a nitrogen atmosphere. Ether was added to precipitate the mixture. The supernatant was removed and the organic solvent was removed by rotary evaporation to obtain a transparent and viscous LHBP3.
[0046] 2) Preparation of 10% LHBP3 / PA4 composite material: 25 g of butyrolactam and 1.5 g of base catalyst were added to container A, and the mixture was reacted at 90°C for 2 h under a nitrogen atmosphere. 25 g of butyrolactam and 0.5 g of initiator were added to container B, and the mixture was reacted at 40°C for 0.5 h under a nitrogen atmosphere. Then 5 g of LHBP3 was added to container B, and the mixture was mixed at 40°C for 1 h under a nitrogen atmosphere. When the temperature of the solution in container A dropped to 40°C, the mixed solution in container A was poured into container B, and the mixture was reacted at 40°C for 12 h under a nitrogen atmosphere to obtain heat-processable polybutyrolactam with a yield of 78%.
[0047] Test Example 1
[0048] The long-chain hyperbranched polymers prepared in Examples 1-3 were characterized and tested according to the following test methods:
[0049] The structure of the samples was tested by infrared spectroscopy (ATR-FTIR) using a Nicolet IS 50 Fourier transform infrared spectrometer from Thermo Fischer Scientific Company, USA, in the range of 4000 to 400 cm-1 and 32 scans.
[0050] The structure of the sample was characterized by 1H-NMR using an AVANCE III 500MHz nuclear magnetic resonance spectrometer from Bruker, Switzerland. 5 mg of the sample and 1 mL of deuterated chloroform (CDCl3) were poured into a tube and repeatedly ultrasonically dissolved, then transferred to a nuclear magnetic resonance tube and slightly shaken to fully mix and dissolve. The hydrogen proton signal of the sample was recorded at 500 MHz.
[0051] The apparent number average (Mn) and weight average molecular weight (Mw) of the samples were characterized using the PL-GPC50 gel permeation chromatograph of Agilent, USA, where the test temperature was 25°C, THF was used as the eluent, the flow rate was 1 mL / min, and linear polystyrene was used as the standard sample.
[0052] The thermal stability of the hot-pressed composite material was tested using a TGA-2 thermogravimetric analyzer from METTLER TOLEDO, Switzerland. Before the test, a small amount of hot-pressed composite material sample was vacuum dried in a forced air drying oven at 80°C for 1 hour, and then the sample was immediately taken out for thermogravimetric testing. 6 to 8 mg of the sample was weighed and placed in an alumina crucible. In a N2 atmosphere, the system was heated from 30°C to 600°C at a heating rate of 10°C / min, and the gas flow rate was 50 mL / min.
[0053] For the solubility test of LHBP (LHBP1, LHBP2, LHBP3), a certain amount of LHBP was weighed with an analytical balance and dissolved in dichloromethane (chloroform, tetrahydrofuran, toluene, dimethyl sulfoxide) (0.2 g LHBP and 2 mL solvent) at a concentration of 10 wt%. A stirring bar was added and sealed. After stirring at room temperature for 24 h on a magnetic stirrer, the stirring bar was removed and the dissolution was recorded by photographing. The test data are shown in Tables 1 and 2.
[0054] Table 1 GPC test data of long chain hyperbranched polymers prepared in Examples 1-3
[0055] sample M Mn PDI <![CDATA[LHBP1]]> 15305 3303 4.6 <![CDATA[LHBP2]]> 24660 4244 5.8 <![CDATA[LHBP3]]> 17502 5502 3.2
[0056] Table 2 TGA test data of long chain hyperbranched polymers prepared in Examples 1-3
[0057] sample Td5(℃) Tmax(℃) Residual weight (wt%) <![CDATA[LHBP1]]> 343 368 2.5 <![CDATA[LHBP2]]> 345 370 1.6 <![CDATA[LHBP3]]> 350 373 0.2
[0058] like Figure 1 As shown, Figure 1 (a) is the infrared spectrum of A2B4-X. Figure 1 (a) It can be seen that the characteristic peaks of carbon-carbon double bonds at 1655 and 809 cm-1 have disappeared significantly, and the peaks at 2565 cm-1 have -1 The characteristic peaks of thiol groups appeared at , which proved that thiol-ene click reaction occurred and A2B4-X with thiol groups at the end was obtained. Figure 1 In (b), it can be observed that 2565 cm -1 The characteristic peak of the thiol group at the position disappeared, proving that the double bond on methyl crotonate reacted with the terminal thiol group of A2B4-X, successfully capping the terminal active thiol group of A2B4-X and obtaining LHBP.
[0059] Figure 2 (a) is the H NMR spectrum of A2B4-X. Figure 2 (a) It can be seen that in the 1H-NMR of A2B4-X, the proton signal peak of the carbon-carbon double bond in A2-X disappeared at 5.8-6.2 ppm, indicating that A2-X and B4 underwent a thiol-ene click reaction, and a proton signal peak of the thiol group appeared at 1.65 ppm, which proved that the terminal group of A2B4-X was a thiol group. Figure 2 (b) is the H NMR spectrum of LHBP. Figure 2 The thiol proton signal peak at 1.65 ppm in (b) disappeared, and the methyl proton signal peak belonging to the capping agent methyl crotonate appeared, indicating that the terminal active thiol group of A2B4-X was successfully capped to obtain LHBP. As the molecular chain length of the reaction monomer A2 gradually increased, the ratio of the methylene proton signal peak area on the thioether group in LHBP to the methylene proton signal peak area of polyethylene glycol in A2 gradually decreased, further indicating that the branch length in LHBP gradually increased, and LHBP1, LHBP2 and LHBP3 with different branch lengths were successfully synthesized.
[0060] Table 1 shows the GPC test data of the long-chain hyperbranched polymers prepared in Examples 1-3. The relative molecular weight and molecular weight distribution of the prepared LHBP are fitted from the GPC elution curve. The polydispersity index PDI is greater than 3 and shows a trend of first increasing and then decreasing, indicating that the molecular weight distribution of LHBP is relatively wide, and the weight-average molecular weights of the three LHBPs with different branch lengths are all greater than 15,000.
[0061] Figure 3 This is an optical photograph of LHBP. Figure 3 It can be seen that in this example, a transparent and viscous LHBP was prepared by using the thiol-ene click reaction, and as the length of the side chain increases, the viscosity of the LHBP gradually increases under the same synthesis conditions.
[0062] Table 2 is the thermal properties data of long chain hyperbranched polymers. Figure 4 Table 2 shows the TGA and DTG curves of the long-chain hyperbranched polymers. It can be seen from Table 2 that the three long-chain hyperbranched polymers have excellent thermal stability, Td5 is above 343°C, and the temperature Tmax corresponding to the maximum thermal decomposition rate is greater than 368°C.
[0063] Test Example 2
[0064] The composite materials prepared in Examples 1-3 were tested for thermal and mechanical properties according to the following test methods:
[0065] The DSC test of the hot-pressed composite material was carried out using a DSC-200 differential scanning calorimeter from NETZSCH, Germany. 3-5 mg of samples of similar size and shape were cut and placed horizontally in an aluminum crucible and tested in an Ar atmosphere at a temperature range of 30-270°C and a heating rate of 10°C / min.
[0066] The thermal stability of the hot-pressed composite material was tested using a TGA-2 thermogravimetric analyzer from METTLER TOLEDO, Switzerland. Before the test, a small amount of hot-pressed composite material sample was vacuum dried in a forced air drying oven at 80°C for 1 hour, and then the sample was immediately taken out for thermogravimetric testing. 6 to 8 mg of the sample was weighed and placed in an alumina crucible. In a N2 atmosphere, the system was heated from 30°C to 600°C at a heating rate of 10°C / min, and the gas flow rate was 50 mL / min.
[0067] 3) The mechanical properties of pure-PA4 and composite materials after hot pressing were tested using a CMT4204 electronic universal testing machine. The hot pressed composite materials were cut into dumbbell-shaped strips with an overall length of 27 mm and a width of 10 mm and a tensile zone length of 10 mm and a width of 5 mm using a customized stainless steel mold. The test temperature was 25°C, the tensile rate was 50 μm / s, and 3 to 5 groups were tested for each sample. The thickness of the film strips was measured with a micrometer before the test and recorded.
[0068] Table 3 TGA test data of the composite materials prepared in Examples 1-3
[0069]
[0070] Table 4 Mechanical properties test data of composite materials prepared in Examples 1-3
[0071] Sample name Tensile strength(MPa) Elongation at break (%) pure-PA4 43.7 9.8 10%LHBP1 / PA4 42.3 19.5 10%LHBP2 / PA4 42.6 20.4 10%LHBP3 / PA4 43.1 21.6
[0072] Table 3 shows the TGA test data of the composite materials prepared in Examples 1-3. It can be seen from Table 3 that the thermal processing window of the composite materials with the addition of LHBP is broadened, with Tm being less than 235°C and Td5 being greater than 270°C.
[0073] Table 4 shows the mechanical property test data of the composite materials prepared in Examples 1-3. It can be seen from Table 4 that the elongation at break of the composite materials with the addition of LHBP is improved, the toughness of PA4 is significantly improved, and the mechanical strength does not decrease significantly.
[0074] Test Example 3
[0075] The composite materials prepared in Examples 1-3 were subjected to relative viscosity tests according to the following test method: the relative viscosity of the composite materials was measured using the VISCO rotational viscometer produced by ATAGO Corporation; 0.2 g of the composite material was dissolved in 20 mL of m-cresol solution to obtain a m-cresol solution of the composite material with a concentration of 1 g / dL; the solution was subjected to relative viscosity tests using a rotational viscometer.
[0076] Table 5 Relative viscosity of the composite solutions prepared in Examples 1-3
[0077] sample Solution η(mPa·s) pure-PA4 12.61 10%LHBP1 / PA4 11.30 10%LHBP2 / PA4 11.74 10%LHBP3 / PA4 12.20
[0078] Table 5 shows the composite materials prepared in Examples 1-3. It can be seen from Table 5 that the addition of LHBP reduces the viscosity of the PA4 solution, indicating that low-viscosity LHBP can improve the rheological properties of PA4.
[0079] Test Example 4
[0080] The tensile fracture of the composite material prepared in Example 2 was observed for microscopic morphology according to the following test method: A cold field emission scanning electron microscope SU8010 of Hitachi (HITACHI) was used to characterize the microscopic morphology of the tensile fracture of the composite material. The sample was placed on an electron microscope plate (flat plate) with conductive tape attached, and after being gold-sprayed by an ion sputtering instrument (Japan, Hitachi E-1010), it was loaded under a scanning electron microscope for observation, and the working voltage was 5 kV.
[0081] Figure 5 (a) and Figure 5 In (b), the mass fractions of LHBP are 0% and 10%, respectively. Figure 5 (a) It can be seen that the tensile section of pure-PA4 has no obvious deformation, and the fracture is flat and smooth, which is an obvious brittle fracture; Figure 5(b) is a PA4 composite material with 10% LHBP2 added. The tensile section shows obvious plastic deformation, the fracture is rough and the fiber area is visible, and obvious ductile fracture occurs. Therefore, the addition of LHBP changes the PA4 from brittle fracture to ductile fracture, indicating that LHBP has a significant effect on improving the toughness of PA4.
[0082] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing heat-processable polybutyrolactam, characterized in that: The following steps are involved: Step (1), adding butyrolactam and an alkali catalyst into container A and mixing them evenly to obtain a mixed solution; Step (2), adding butyrolactam and the first initiator into container B and mixing them evenly, and then adding the long-chain hyperbranched polymer into container B and mixing them evenly; Step (3), pouring the mixed solution in container A into container B to carry out a ring-opening polymerization reaction to obtain heat-processable polybutyrolactam.
2. The method for preparing heat-processable polybutyrolactam according to claim 1, characterized in that: In step (1), the amount of base catalyst added is 1-10% of the mass fraction of butyrolactam; the reaction conditions of butyrolactam and base catalyst are: reacting at 40-100° C. for 0.5-4 hours under the protection of inert gas.
3. The method for preparing heat-processable polybutyrolactam according to claim 1, characterized in that: In step (1), the base catalyst is selected from one or more of sodium tert-butoxide, potassium tert-butoxide, sodium hydroxide and potassium hydroxide.
4. The method for preparing a heat-processable polybutyrolactam according to claim 1, characterized in that: In step (2), the amount of the first initiator added is 0.1-3% of the mass fraction of butyrolactam; the reaction conditions of butyrolactam and the first initiator are: reacting at 30-45° C. for 0.5-1 h under the protection of inert gas.
5. The method for preparing a heat-processable polybutyrolactam according to claim 1, characterized in that: In step (2), the first initiator is selected from one or more of benzoyl chloride, oxalyl chloride, acetyl chloride, tetradecanoyl chloride and diisocyanate.
6. The method for preparing a heat-processable polybutyrolactam according to claim 1, characterized in that: In step (2), the amount of long-chain hyperbranched polymer added is 3-20% of the mass fraction of butyrolactam; after the long-chain hyperbranched polymer is added to container B, the mixing conditions are: stirring at 30-45° C. for 0.5-1 h under the protection of inert gas.
7. The method for preparing a heat-processable polybutyrolactam according to claim 1, characterized in that: In step (2), the long-chain hyperbranched polymer is obtained by polymerizing a binary active olefin group, a multi-active thiol group, and a second initiator in a solvent through a "thiol-ene" click reaction, and then inactivated with a capping agent; Wherein, the binary active olefin group is one or more of diacrylate polyethylene glycol (CH2=CHCOO-(C2H4O)n-COCH=CH2, wherein n=3-25), diene polyethylene glycol (CH2=CHCH3-(C2H4O)n-CH3CH=CH2, wherein n=3-25), diacrylamide polyethylene glycol (CH2=CHCONH-(C2H4O)n-CONHCH=CH2, wherein n=3-25), diacrylate polyethylene (CH2=CHCOO-(C2H4)n-COCH=CH2, wherein n=3-25), diene polyethylene (CH2=CHCH3-(C2H4)n-CH3CH=CH2, wherein n=3-25) and diacrylamide polyethylene (CH2=CHCONH-(C2H4)n-CONHCH=CH2, wherein n=3-25); The polyvalent active mercapto group is one or more of trimercaptomethane, trimercaptopropane, trimercaptobenzene, trimercaptosilane, trimercaptophosphorus, thiocyanuric acid, trimethylolpropane tris(thioglycolic acid), tetramercaptobenzene and pentaerythritol tetrakis(3-mercaptopropionic acid); The second initiator is selected from one or more of azobisisobutyronitrile, benzoyl peroxide, dimethylaminopyridine, dibutyl phosphate and hydroxycyclohexane phenone; Wherein, the solvent is selected from one or more of dichloromethane, chloroform, tetrahydrofuran, benzophenone and toluene, and the solution concentration is 5 to 20 wt%; Wherein, the end-capping agent is one or more of methyl crotonate, acrylate, 2-allylphenol, eugenol, methyl eugenol, 3-allyl-N,N-dimethylaniline and bisphenol S monopropylene ether.
8. The method for preparing a heat-processable polybutyrolactam according to claim 7, characterized in that: The conditions for the "thiol-ene" click reaction are: The binary active alkenyl, the multi-active thiol and 0.5-3wt% of the second initiator are dissolved in a solvent, reacted at 50-90°C for 0.5-24h, and then a capping agent is added to react at 50-90°C for 0.5-24h, the solution after the reaction is precipitated in ether, and dried at 60-100°C for 12h; wherein the active group molar ratio of the multi-active thiol is: alkenyl / thiol=0.5-0.9; the active group molar ratio of the capping agent is: alkenyl / thiol=0.2-0.
6.
9. The method for preparing a heat-processable polybutyrolactam according to claim 1, characterized in that: In step (3), the ring-opening polymerization reaction conditions are: reaction at 40-70° C. for 4-24 hours.
10. A heat-processable polybutyrolactam, characterized in that: The method is prepared according to any one of claims 1 to 9.
Citation Information
Cited By
PA4 or PA5 and preparation method thereof
CN121699139A
PA4 or PA5 and a process for their preparation
CN121699139B