Preparation method of PPS composite material with high magnetic permeability
By making a homemade comb-type high-temperature lubricant, the distribution of magnetic powder in the PPS matrix is solved, and the problem of low permeability of PPS-based magnetic materials is improved, and the magnetic permeability and mechanical properties are improved, forming a high-compatibility lubricating layer, which is enhanced. Combination of magnetic powder and substrate.
Patent Information
- Application Number
- CN202411126246.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-01
AI Technical Summary
The magnetic permeability of PPS-based plastic magnetic materials is difficult to improve, mainly due to the poor dispersion and uneven distribution of magnetic powder in the matrix, making it difficult for magnetic powder to form an effective magnetic circuit.
Using homemade comb high temperature lubricant, doping silicon chains with sulfhydryl chloride and diallylamine amidation, mercaptoethanol click addition and dialkyl dichlorosilane to form comb high temperature with sulfhydryl ether and amide structure. Lubricant enhances the compatibility and dispersion of magnetic powder and matrix, reduces dispersion resistance, and promotes uniform distribution of magnetic powder.
It significantly improves the magnetic permeability and mechanical properties, forms a high-compatibility lubricating layer, enhances the bonding toughness between the magnetic powder and the matrix, and improves the magnetic and impact resistance of the composite material.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of plastic magnetic materials, and in particular relates to a method for preparing a high magnetic permeability PPS composite material. Background Art
[0002] Traditional magnets are mostly hard and brittle materials, which are difficult to process and shape, greatly limiting the application of magnets. Reprocessable plastic magnetic materials can be made into workpieces with complex shapes and precise dimensions, and can be integrated with hardware, and are widely used in the automotive industry, home appliances, electronic information, and automation tools.
[0003] PPS (polyphenylene sulfide) is a common thermoplastic special engineering plastic with high physical strength, good temperature resistance, chemical corrosion resistance, non-flammability, thermal stability, and excellent electrical properties. As a binder, the prepared plastic magnetic material is more suitable for use in a demanding environment. However, PPS has a high viscosity after melting, a high heating temperature, and low fluidity, resulting in poor dispersion of magnetic powder in the PPS matrix, limiting the amount of magnetic powder added. At the same time, unevenly distributed magnetic powder is difficult to form an effective magnetic circuit, making it difficult to improve the magnetic permeability of PPS-based plastic magnetic materials. Summary of the invention
[0004] In order to solve the technical problems mentioned in the background technology, the purpose of the present invention is to provide a method for preparing a high magnetic permeability PPS composite material.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A preparation method of a high magnetic permeability PPS composite material comprises the following steps: mixing and melting a PPS resin, a comb-type high-temperature lubricant and an antioxidant, adding preheated magnetic powder, kneading at 300±5°C until the torque is stable, discharging and pelletizing to prepare the high magnetic permeability PPS composite material.
[0007] Preferably, the proportions of the components in the high magnetic permeability PPS composite material are: 9.5-14wt% PPS resin, 0.8-1.2wt% comb-type high-temperature lubricant, 0.11-0.15wt% antioxidant, and the remainder is magnetic powder.
[0008] Preferably, the antioxidant is a compound of antioxidant 1098 and antioxidant 168.
[0009] The comb-type high-temperature lubricant is prepared by the following method:
[0010] Step A1: diallylamine, potassium carbonate and anhydrous tetrahydrofuran are mixed, dry nitrogen is introduced for protection, the temperature is controlled at 5-15°C in an ice-water bath, stirring is applied at 60-120 rpm, alkyl acid chloride is added for reaction for 1-1.5 hours, then the temperature is raised to reflux for 3-4 hours, tetrahydrofuran is removed by rotary evaporation after the reaction is completed, the rotary evaporation substrate is washed with water and dried to obtain intermediate 1;
[0011] Furthermore, the dosage ratio of diallylamine, alkyl acyl chloride, potassium carbonate and anhydrous tetrahydrofuran is 0.1 mol: 0.102-0.105 mol: 2-3.5 g: 40-55 mL, and the alkyl acyl chloride and diallylamine undergo an amidation reaction under the promotion of potassium carbonate.
[0012] Preferably, the alkyl chain length of the alkyl acid chloride is C12-C18.
[0013] Step A2: Mix the intermediate 1, mercaptoethanol, benzoyl peroxide and toluene, raise the temperature to 70-90°C, apply stirring at 120-180 rpm and 200-300 W / m 2 UV irradiation, reaction for 5-7h, after the reaction is completed, toluene is removed by vacuum rotary evaporation to obtain intermediate 2;
[0014] Furthermore, the usage ratio of intermediate 1, mercaptoethanol, benzoyl peroxide and toluene is 0.1 mol: 0.2 mol: 15-30 mg: 110-160 mL, and mercaptoethanol click-adds to the double bond in the intermediate 1 molecule under the promotion of benzoyl peroxide and the initiation of ultraviolet radiation.
[0015] Step A3: Mix the intermediate 2, triethylamine and dimethylacetamide, introduce dry nitrogen protection, heat to 40-55°C, stir at 180-240 rpm, slowly add dialkyldichlorosilane and react for 1.2-1.8 hours, then continue to heat to 110-130°C and continue to react for 2.5-3.5 hours. After the reaction is completed, wash with water and dry to obtain a comb-shaped high-temperature lubricant;
[0016] Further, the usage ratio of intermediate 2, dialkyldichlorosilane, triethylamine and dimethylacetamide is 0.1 mol: 85-90 mmol: 15-25 mL: 80-120 mL, and under the promotion of triethylamine, dialkyldichlorosilane replaces the terminal hydroxyl group introduced in intermediate 2 to form a doped silicon chain;
[0017] Preferably, the alkyl chain length of the dialkyldichlorosilane is C4-C8.
[0018] Beneficial effects of the present invention:
[0019] The invention discloses a PPS-based magnetic composite material, wherein a self-made comb-type high-temperature lubricant is added to improve the lubricity of magnetic powder and a matrix during blending, and to enhance the uniformity of the distribution of the magnetic powder in the composite material, thereby enhancing the magnetic permeability of the composite material; the comb-type high-temperature lubricant is prepared by amidation reaction of alkyl acyl chloride and diallylamine to prepare an intermediate 1 having a terminal alkyl long chain and a double-branched double bond, and then mercaptoethanol is subjected to click addition to the double bond in the intermediate 1 molecule to introduce a thioether structure and a terminal hydroxyl group to modify, thereby obtaining an intermediate 2, and then dialkyldichlorosilane is substituted with the terminal hydroxyl group introduced in the intermediate 2 to form a chain compound; the thioether structure and the amide structure in the comb-type high-temperature lubricant molecule form a chelating effect, and during the blending process, the chelating force is used to enrich the surface of the magnetic powder, and the molecule A large number of alkyl chains on the side chains have good compatibility with the PPS matrix, forming a highly compatible lubricating layer on the magnetic powder. In addition, the main chain of the comb-type high-temperature lubricant contains a large number of silicone segments, which can maintain the stability of the lubricating layer during high-temperature blending, effectively reduce the dispersion resistance between the magnetic powder and the matrix and between the magnetic powders, so that the magnetic powder is fully dispersed, which is beneficial to the formation of the magnetic circuit and improves the magnetic properties. The side chains of the comb-type high-temperature lubricant molecules are formed by alternating double-branched alkyl chains and single long alkyl chains. After the composite material is formed, the branched alkyl chains are interspersed between the macromolecular chains of the PPS matrix to toughen the matrix. At the same time, a soft connection is formed between the hard magnetic powder and the matrix, which improves the bonding toughness between the magnetic powder and the matrix, thereby improving the mechanical properties of the composite material. DETAILED DESCRIPTION
[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0021] Example 1: Preparation of a high magnetic permeability PPS composite material, the specific implementation process is as follows:
[0022] (1) Preparation of comb-type high-temperature lubricant
[0023] Step A1: Mix diallylamine, potassium carbonate and anhydrous tetrahydrofuran, introduce dry nitrogen for protection, control the temperature at 5°C in an ice-water bath, stir at 60rpm, add alkyl acyl chloride to react for 1.5h, then heat and reflux for 4h, wherein the amount ratio of diallylamine, alkyl acyl chloride, potassium carbonate and anhydrous tetrahydrofuran is 0.1mol:0.102mol:2g:40mL, and the alkyl acyl chloride is selected from dodecanoyl chloride. After the reaction, remove tetrahydrofuran by rotary evaporation, wash the rotary evaporation substrate with water and dry it to obtain intermediate 1.
[0024] Step A2: Mix intermediate 1, mercaptoethanol, benzoyl peroxide and toluene, raise the temperature to 70°C, apply stirring at 120 rpm and 200 W / m 2 The reaction was carried out under ultraviolet irradiation for 7 hours, wherein the usage ratio of intermediate 1, mercaptoethanol, benzoyl peroxide and toluene was 0.1 mol: 0.2 mol: 15 mg: 110 mL. After the reaction was completed, toluene was removed by rotary evaporation under reduced pressure to obtain intermediate 2.
[0025] Step A3: Take intermediate 2, triethylamine and dimethylacetamide, mix them, pass dry nitrogen protection, heat to 40°C, stir at 180rpm, slowly add dialkyldichlorosilane to react for 1.8h, then continue to heat to 110°C and continue to react for 3.5h, wherein the amount ratio of intermediate 2, dialkyldichlorosilane, triethylamine and dimethylacetamide is 0.1mol:85mmol:15mL:80mL, and dialkyldichlorosilane is selected from dibutyldichlorosilane. After the reaction, wash with water and dry to obtain a comb-type high-temperature lubricant.
[0026] (2) Preparation of high magnetic permeability PPS composite materials
[0027] Ingredients: raw materials are taken according to weight percentage, 89.59wt% of magnetic powder, 2000 mesh NdFeB magnetic powder is used in the implementation process; 9.5wt% of PPS resin, Toray A900 pure resin raw material is used in the implementation process; 0.8wt% of comb-type high-temperature lubricant is made by this embodiment; 0.11wt% of antioxidant, antioxidant 1098 and antioxidant 168 are premixed in equal weight in the implementation process;
[0028] Compounding: PPS resin, comb-type high-temperature lubricant and antioxidant are mixed and melted, and then the magnetic powder is preheated to 300°C and added. The target temperature is controlled to 300°C, and the allowable error is 5°C. Mix until the torque tends to be stable, and cut into pellets to obtain a high magnetic permeability PPS composite material.
[0029] Example 2, preparation of high magnetic permeability PPS composite material, the specific implementation process is as follows:
[0030] (1) Preparation of comb-type high-temperature lubricant
[0031] Step A1: Mix diallylamine, potassium carbonate and anhydrous tetrahydrofuran, introduce dry nitrogen for protection, control the temperature at 15°C in an ice-water bath, apply stirring at 120rpm, add alkyl acid chloride to react for 1h, then heat and reflux for 3h, wherein the amount ratio of diallylamine, alkyl acid chloride, potassium carbonate and anhydrous tetrahydrofuran is 0.1mol:0.105mol:3.5g:55mL, and the alkyl acid chloride is selected from octadecanoyl chloride. After the reaction, remove tetrahydrofuran by rotary evaporation, wash the rotary evaporation substrate with water and dry it to obtain intermediate 1.
[0032] Step A2: Mix the intermediate 1, mercaptoethanol, benzoyl peroxide and toluene, raise the temperature to 90°C, stir at 180 rpm and 300 W / m 2 The reaction was carried out under ultraviolet irradiation for 5 hours, wherein the usage ratio of intermediate 1, mercaptoethanol, benzoyl peroxide and toluene was 0.1 mol: 0.2 mol: 30 mg: 160 mL. After the reaction was completed, toluene was removed by vacuum rotary evaporation to obtain intermediate 2.
[0033] Step A3: Take intermediate 2, triethylamine and dimethylacetamide, mix them, pass dry nitrogen protection, heat to 55°C, stir at 240rpm, slowly add dialkyldichlorosilane to react for 1.2h, then continue to heat to 130°C and continue to react for 2.5h, wherein the amount ratio of intermediate 2, dialkyldichlorosilane, triethylamine and dimethylacetamide is 0.1mol:90mmol:25mL:120mL, and dialkyldichlorosilane is selected from dioctyldichlorosilane. After the reaction, wash with water and dry to obtain a comb-type high-temperature lubricant.
[0034] (2) Preparation of high magnetic permeability PPS composite materials
[0035] Ingredients: raw materials are taken according to weight percentage, 84.65wt% of magnetic powder, 2000 mesh NdFeB magnetic powder is used in the implementation process; 14wt% of PPS resin, Toray A900 pure resin raw material is used in the implementation process; 1.2wt% of comb-type high-temperature lubricant is self-made in this embodiment; 0.15wt% of antioxidant, antioxidant 1098 and antioxidant 168 are premixed in equal mass in the implementation process;
[0036] Compounding: PPS resin, comb-type high-temperature lubricant and antioxidant are mixed and melted, and then the magnetic powder is preheated to 300°C and added. The target temperature is controlled to 300°C, and the allowable error is 5°C. Mix until the torque tends to be stable, and cut into pellets to obtain a high magnetic permeability PPS composite material.
[0037] Example 3, preparation of high magnetic permeability PPS composite material, the specific implementation process is as follows:
[0038] (1) Preparation of comb-type high-temperature lubricant
[0039] Step A1: Mix diallylamine, potassium carbonate and anhydrous tetrahydrofuran, introduce dry nitrogen for protection, control the temperature at 10°C in an ice-water bath, stir at 90rpm, add alkyl acyl chloride to react for 1.2h, then heat and reflux for 3.5h, wherein the amount ratio of diallylamine, alkyl acyl chloride, potassium carbonate and anhydrous tetrahydrofuran is 0.1mol:0.103mol:2.5g:45mL, and the alkyl acyl chloride is selected from tetradecanoyl chloride. After the reaction, remove tetrahydrofuran by rotary evaporation, wash the rotary evaporation substrate with water and dry it to obtain intermediate 1.
[0040] Step A2: Mix the intermediate 1, mercaptoethanol, benzoyl peroxide and toluene, raise the temperature to 80°C, apply stirring at 150 rpm and 260 W / m 2 The reaction was carried out under ultraviolet irradiation for 6 hours, wherein the usage ratio of intermediate 1, mercaptoethanol, benzoyl peroxide and toluene was 0.1 mol: 0.2 mol: 20 mg: 140 mL. After the reaction was completed, toluene was removed by vacuum rotary evaporation to obtain intermediate 2.
[0041] Step A3: Take intermediate 2, triethylamine and dimethylacetamide, mix them, pass dry nitrogen protection, heat to 50°C, stir at 240rpm, slowly add dialkyldichlorosilane to react for 1.5h, then continue to heat to 120°C and continue to react for 3h, wherein the amount ratio of intermediate 2, dialkyldichlorosilane, triethylamine and dimethylacetamide is 0.1mol:85mmol:20mL:100mL, and dialkyldichlorosilane is selected from dihexyldichlorosilane. After the reaction, wash with water and dry to obtain a comb-type high-temperature lubricant.
[0042] (2) Preparation of high magnetic permeability PPS composite materials
[0043] Ingredients: raw materials are taken according to weight percentage, 87.47wt% of magnetic powder, 2000 mesh NdFeB magnetic powder is used in the implementation process; 11.5wt% of PPS resin, Toray A900 pure resin raw material is used in the implementation process; 0.9wt% of comb-type high-temperature lubricant is made by this embodiment; 0.13wt% of antioxidant, antioxidant 1098 and antioxidant 168 are premixed in equal weight in the implementation process;
[0044] Compounding: PPS resin, comb-type high-temperature lubricant and antioxidant are mixed and melted, and then the magnetic powder is preheated to 300°C and added. The target temperature is controlled to 300°C, and the allowable error is 5°C. Mix until the torque tends to be stable, and cut into pellets to obtain a high magnetic permeability PPS composite material.
[0045] Example 4, preparation of high magnetic permeability PPS composite material, the specific implementation process is as follows:
[0046] (1) Preparation of comb-type high-temperature lubricant
[0047] Step A1: Mix diallylamine, potassium carbonate and anhydrous tetrahydrofuran, introduce dry nitrogen for protection, control the temperature at 15°C in an ice-water bath, apply stirring at 120rpm, add alkyl acid chloride to react for 1.2h, then heat and reflux for 3h, wherein the amount ratio of diallylamine, alkyl acid chloride, potassium carbonate and anhydrous tetrahydrofuran is 0.1mol:0.104mol:3.2g:50mL, and the alkyl acid chloride is selected from hexadecanoyl chloride. After the reaction, remove tetrahydrofuran by rotary evaporation, wash the rotary evaporation substrate with water and dry it to obtain intermediate 1.
[0048] Step A2: Mix the intermediate 1, mercaptoethanol, benzoyl peroxide and toluene, raise the temperature to 85°C, apply stirring at 180 rpm and 240 W / m 2 The reaction was carried out under ultraviolet irradiation for 6.5 hours, wherein the usage ratio of intermediate 1, mercaptoethanol, benzoyl peroxide and toluene was 0.1 mol: 0.2 mol: 25 mg: 150 mL. After the reaction was completed, toluene was removed by vacuum rotary evaporation to obtain intermediate 2.
[0049] Step A3: Take intermediate 2, triethylamine and dimethylacetamide, mix them, pass dry nitrogen protection, heat to 50°C, stir at 240rpm, slowly add dialkyldichlorosilane to react for 1.6h, then continue to heat to 130°C and continue to react for 2.8h, wherein the amount ratio of intermediate 2, dialkyldichlorosilane, triethylamine and dimethylacetamide is 0.1mol:90mmol:25mL:100mL, and dialkyldichlorosilane is selected from dihexyldichlorosilane. After the reaction, wash with water and dry to obtain a comb-type high-temperature lubricant.
[0050] (2) Preparation of high magnetic permeability PPS composite materials
[0051] Ingredients: raw materials are taken according to weight percentage, 86.36wt% of magnetic powder, 2000 mesh NdFeB magnetic powder is used in the implementation process; 12.5wt% of PPS resin, Toray A900 pure resin raw material is used in the implementation process; 1wt% of comb-type high-temperature lubricant is made by this embodiment; 0.14wt% of antioxidant, antioxidant 1098 and antioxidant 168 are premixed in equal weight in the implementation process;
[0052] Compounding: PPS resin, comb-type high-temperature lubricant and antioxidant are mixed and melted, and then the magnetic powder is preheated to 300°C and added. The target temperature is controlled to 300°C, and the allowable error is 5°C. Mix until the torque tends to be stable, and cut into pellets to obtain a high magnetic permeability PPS composite material.
[0053] Comparative Example
[0054] This comparative example refers to Example 4, except that the comb-type high-temperature lubricant is replaced with the same weight of TAF-A type lubricant, and the rest of the implementation process is exactly the same.
[0055] The high magnetic permeability PPS composite material prepared above was hot-pressed by a flat vulcanizer at a temperature of 320±5°C and a pressure of 3MPa. The impact performance of the samples was tested according to GB / T 1043.1-2008; the magnetic performance of the samples was tested according to GB / T3658-2022, and the test frequency was 75kHz. The specific test results are shown in the following table:
[0056] <![CDATA[Impact strength / kJ·m -2 > Magnetic Permeability Remanence / T <![CDATA[Intrinsic coercivity / kA·m -1 > Example 1 8.04 85.1 0.829 255 Example 2 9.37 79.6 0.773 219 Example 3 8.85 83.3 0.810 251 Example 4 9.12 84.5 0.841 264 Comparative Example 7.26 65.9 0.702 173
[0057] It can be seen from the test data in the above table that the composite material of the embodiment has higher impact resistance after molding. Compared with the comparative example, under the same magnetic powder content and dispersion process, the magnetic properties of the embodiment are significantly improved, which is related to the uniform distribution of the magnetic powder.
[0058] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0059] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing a high magnetic permeability PPS composite material, characterized in that: Specifically, the PPS resin, comb-type high-temperature lubricant and antioxidant are mixed and melted, and then the magnetic powder is preheated and added, and mixed at 300±5℃ until the torque is stable, and the material is discharged and pelletized to make a high magnetic permeability PPS composite material; The comb-type high-temperature lubricant is prepared by the following method: Step A1: diallylamine, potassium carbonate and anhydrous tetrahydrofuran are mixed, and dry nitrogen is introduced for protection. The temperature is controlled at 5-15°C in an ice-water bath, and alkyl acyl chloride is added with stirring for 1-1.5 hours. The temperature is then raised to reflux for 3-4 hours. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation, and the rotary evaporation substrate is washed with water and dried to obtain intermediate 1; Step A2: Mix the intermediate 1, mercaptoethanol, benzoyl peroxide and toluene, raise the temperature to 70-90°C, stir and apply 200-300W / m 2 UV irradiation, reaction for 5-7h, after the reaction is completed, toluene is removed by vacuum rotary evaporation to obtain intermediate 2; Step A3: Mix intermediate 2, triethylamine and dimethylacetamide, pass dry nitrogen protection, heat to 40-55°C, stir and slowly add dialkyldichlorosilane to react for 1.2-1.8h, then continue to heat to 110-130°C and continue to react for 2.5-3.5h. After the reaction is completed, wash with water and dry to obtain a comb-shaped high-temperature lubricant.
2. The method for preparing a high magnetic permeability PPS composite material according to claim 1, characterized in that: The usage ratio of diallylamine, alkyl acid chloride, potassium carbonate and anhydrous tetrahydrofuran is 0.1 mol: 0.102-0.105 mol: 2-3.5 g: 40-55 mL.
3. The method for preparing a high magnetic permeability PPS composite material according to claim 2, characterized in that: The alkyl chain length of the alkyl acid chloride is C12-C18.
4. The method for preparing a high magnetic permeability PPS composite material according to claim 3, characterized in that: The usage ratio of intermediate 1, mercaptoethanol, benzoyl peroxide and toluene is 0.1 mol: 0.2 mol: 15-30 mg: 110-160 mL.
5. The method for preparing a high magnetic permeability PPS composite material according to claim 4, characterized in that: The usage ratio of intermediate 2, dialkyldichlorosilane, triethylamine and dimethylacetamide is 0.1 mol: 85-90 mmol: 15-25 mL: 80-120 mL.
6. The method for preparing a high magnetic permeability PPS composite material according to claim 5, characterized in that: The alkyl chain length of dialkyldichlorosilane is C4-C8.
7. A method for preparing a high magnetic permeability PPS composite material according to any one of claims 1 to 6, characterized in that: The proportions of the components in the high magnetic permeability PPS composite material are: 9.5-14wt% of PPS resin, 0.8-1.2wt% of comb-shaped high-temperature lubricant, 0.11-0.15wt% of antioxidant, and the balance of magnetic powder.
8. The method for preparing a high magnetic permeability PPS composite material according to claim 1, characterized in that: The antioxidant is compounded by antioxidant 1098 and antioxidant 168.
Citation Information
Patent Citations
Preparation of softly magnetic granules for injection molding
CN105885359A
Controlling cure rate using polyether synergists
CN113785019A
Modified polyphenylene sulfide magnetic composite material and preparation method thereof
CN114015235A
Neodymium iron boron magnetic composite material and preparation method thereof
CN114806157A
Magnetic powder containing coating layer as well as preparation method and application of magnetic powder
CN115109438A