Method for improving insulating property of high-temperature silicon carbide device by grafting nano siloxane
Through the grafting reaction and cross-linking process of POSS and PMHS, POSS grafted silicon elastomer nanocomposites were prepared, which solved the problem of insufficient insulation performance of packaging materials at high temperatures and achieved higher thermal stability and insulation performance.
Patent Information
- Application Number
- CN202410957256.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-07-03
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-01
AI Technical Summary
The packaging materials of existing high-temperature silicon carbide devices have insufficient insulation performance at high temperatures, and nanofillers such as POSS are prone to agglomeration during filling, reducing the thermal and electrical properties of the materials.
Grafting through the hydrogen silicon addition reaction of POSS and PMHS to form POSS-grafted PMHS solution, and cross-linked with VPDMS and catalyst in a vacuum oven to prepare POSS grafted silicon elastomer nanocomposite material to avoid POSS participating in curing Agglomeration during the process forms a uniform nanospherical structure.
It effectively improves the high-temperature resistance and high-temperature insulation properties of the silicon elastomer material for silicon carbide module packaging, significantly improves the thermal stability and breakdown strength of the material, and reduces the conductivity.
Smart Images

Figure CN118879079A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of material chemistry, and specifically relates to a method for improving the insulation performance of a high-temperature silicon carbide device by grafting nano-siloxane. Background Art
[0002] Wide bandgap silicon carbide electronic power modules are moving towards higher temperatures (>150℃), higher voltages (>6.5kV) and miniaturization to achieve higher power density. High temperatures, high voltages and miniaturization in power modules lead to higher thermal and electrical stress concentrations, requiring packaging materials to have strong resistance to high temperatures and strong electric fields. The selection of high-temperature packaging materials requires a balance between thermal stability and flexibility. Compared with other packaging materials used for high temperatures (such as polyimide, benzocyclobutene and cyanate resins), silicone elastomers have lower hardness and storage modulus. The mechanical stress of the package structure, which is usually caused by the mismatch of thermal expansion coefficients, can be reduced. Although silicone gel, as a traditional soft packaging material, has good mechanical compatibility with other components in power modules, it usually works below a few kV and 150℃. However, during the curing process, silicone elastomers do not shrink in volume due to their excellent viscosity during filling (i.e. potting) and exhibit relatively high breakdown strength at high temperatures above 150℃. The addition of nanofillers (such as boron nitride, aluminum oxide, aluminum nitride, zinc oxide, silicon dioxide, POSS, etc.) can effectively improve the insulating properties of polymers. Polyhedral oligomeric silsesquioxane (POSS) is considered to be the smallest siloxane nanoparticle, only 1 to 3 nanometers. The inorganic core of POSS is a highly symmetrical cage structure with a low real dielectric constant, high thermal stability and good mechanical properties. Its vertex active organic groups can be used as links between polymers and POSS, thereby enhancing the compatibility between polymers and POSS. Physical addition of boron nitride to the epoxy matrix can improve thermal conductivity but reduce dielectric breakdown strength. On the other hand, epoxy-based POSS can form covalent bonds with epoxy resin and modify its structure at the nanoscale, improving thermal conductivity and breakdown strength. In addition, compared with other ceramic nanoparticles, POSS molecules are easily soluble in solvents, thereby simplifying and controlling the processing of composite materials. Therefore, POSS exhibits better thermal and electrical properties than ceramic particles. Octaaminophenyl POSS, triepoxyisobutyl POSS and epoxy POSS form covalent bonds with epoxy resin due to their active organic groups and are dispersed as part of the enhanced cross-linked network at the molecular level. However, the above POSS materials react directly with epoxy resin and curing agent at a high filler content, easily forming agglomerates, which reduces thermal and electrical properties. In addition, due to incompatibility, a clear interface between the agglomerated trisilanephenol-based POSS and the polypropylene matrix was observed in the polypropylene matrix, affecting the high temperature resistance and high temperature insulation properties of the material. Summary of the invention
[0003] The object of the present invention is to provide a method for improving the insulation performance of high-temperature silicon carbide devices by grafting nanosiloxane. The present invention can prevent POSS from participating in the curing process of silicon elastomer and reduce the possibility of agglomeration. The POSS grafted silicon elastomer nanocomposite prepared by the present invention can effectively improve the high temperature resistance and high temperature insulation performance of silicon elastomer materials for silicon carbide module packaging.
[0004] The technical solution of the present invention is a method for improving the insulation performance of high-temperature silicon carbide devices by grafting nano-siloxane, the method comprising the following steps:
[0005] Step 1: POSS filler is grafted onto PMHS molecular chain through hydrosilylation reaction to prepare POSS grafted PMHS solution;
[0006] Step 2: The PMHS solution prepared in step 1 is fully stirred with VPDMS, a catalyst, and an inhibitor at room temperature and subjected to multiple cycles of vacuum degassing to obtain a liquid mixture;
[0007] Step 3: pour the liquid mixture into a polytetrafluoroethylene mold, heat and cross-link and cure in a vacuum oven to obtain a POSS grafted silicon elastomer nanocomposite material, and use the POSS grafted silicon elastomer nanocomposite material as a silicon elastomer material for silicon carbide module packaging.
[0008] In the above-mentioned method for grafting nano-siloxane to improve the insulation performance of high-temperature silicon carbide devices, in step 1, 0.1-0.8 parts of POSS filler and 15-25 parts of PMHS are stirred in 50-70 parts of toluene solvent by mass, 0.01-0.04 parts of Karstedt catalyst are added in a dry nitrogen environment, and refluxed through a condenser at 60-80° C. for 1-3 hours; the solvent is removed by rotary evaporation to obtain a nano-spherical structure polymer with a POSS cage structure as the core and a SE molecular chain as the shell, that is, a POSS-grafted PMHS solution.
[0009] In the aforementioned method of grafting nanosiloxane to improve the insulation performance of high-temperature silicon carbide devices, in step 1, 0.4 g of POSS filler and 20 g of PMHS are stirred in 60 ml of toluene solvent, 0.025 g of Karstedt catalyst is added in a dry nitrogen environment, and refluxed through a condenser at 70° C. for 2 hours; the solvent is removed by rotary evaporation to obtain a nano-spherical structure polymer with a POSS cage structure as the core and a SE molecular chain as the shell, that is, a POSS-grafted PMHS solution.
[0010] In the aforementioned method of grafting nanosiloxane to improve the insulation performance of high-temperature silicon carbide devices, in step 2, 10-40 parts of the PMHS solution prepared in step 1 are mixed with 5-25 parts of VPDMS, 0.01-0.1 parts of Karstedt catalyst, and 0.01-0.04 parts of inhibitor by mass at 20-30° C. and stirred for 20-40 minutes for multiple cycles of vacuum degassing.
[0011] In the aforementioned method of grafting nanosiloxane to improve the insulation performance of high-temperature silicon carbide devices, in step 2, 0.25 g of the PMHS solution prepared in step 1 is mixed with 12 g of VPDMS, 0.05 g of Karstedt catalyst, and 0.025 g of inhibitor by mass at 25° C. and stirred for 30 minutes for multiple cycles of vacuum degassing.
[0012] In the aforementioned method of grafting nanosiloxane to improve the insulation performance of high-temperature silicon carbide devices, in step three, the liquid mixture is poured into a polytetrafluoroethylene mold, and then cured at 100-150° C. for 2-4 hours to obtain a POSS grafted silicon elastomer nanocomposite material.
[0013] In the aforementioned method of grafting nano-siloxane to improve the insulation performance of high-temperature silicon carbide devices, in step three, the liquid mixture is poured into a polytetrafluoroethylene mold, and then cured at 120° C. for 3 hours to obtain a POSS grafted silicon elastomer nanocomposite material.
[0014] Compared with the prior art, the present invention has the following beneficial effects:
[0015] 1. The POSS uniformly distributed in the toluene solvent of the present invention is conducive to the formation of nano-fillers with uniform size, and can effectively avoid the agglomeration of fillers on a microscopic scale. The present invention can prevent POSS from participating in the silicone elastomer curing process and reduce the possibility of agglomeration. The POSS grafted silicone elastomer nanocomposite prepared by the present invention can effectively improve the high temperature resistance and high temperature insulation performance of the silicone elastomer material for silicon carbide module packaging.
[0016] 2. The present invention is characterized by micromorphology, and it can be found that the section of SE is flat and free of impurities. SE-POSS shows a uniform and dense nanostructure and a rough surface, indicating that nano POSS grafting can affect the overall crosslinking process of silicone elastomers and form a dense nanosphere structure. The present invention can show that SE-POSS has better thermal stability by thermogravimetric analysis, and the nanostructure introduced by grafted POSS strengthens the molecular chain crosslinking structure, effectively hindering the high-temperature thermal degradation of silicone elastomers. The present invention is analyzed by insulation properties, and it is concluded that SE-POSS has lower electrical conductivity and higher breakdown strength at high temperatures, indicating that the grafted POSS nanofiller improves the high-temperature insulation properties of silicone elastomers. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a process diagram of the preparation method of the POSS-grafted silicon elastomer nanocomposite material of the present invention;
[0018] Figure 2 This is a microscopic morphology of the pure silicon elastomer of the present invention;
[0019] Figure 3 It is a microscopic morphology diagram of the nanocomposite material of the present invention;
[0020] Figure 4 It is the thermal weight loss curve diagram of the pure silicon elastomer and the nanocomposite material thereof of the present invention;
[0021] Figure 5 The weight loss rate curve of the pure silicon elastomer and the nanocomposite material thereof of the present invention;
[0022] Figure 6 The conductivity discount diagram of the pure silicon elastomer and the nanocomposite material thereof of the present invention;
[0023] Figure 7 It is a column chart of the breakdown electric field of the pure silicon elastomer and its nanocomposite material of the present invention. DETAILED DESCRIPTION
[0024] The present invention is further described below in conjunction with the accompanying drawings and embodiments, but they are not intended to limit the present invention.
[0025] Example 1: A method for grafting nanosiloxane to improve the insulation performance of high-temperature silicon carbide devices. In this example, vinyl-terminated polydimethylsiloxane (VPDMS) (viscosity: 200 mPa·s) and polymethylhydrogensiloxane (PMHS) (viscosity of 22 mPa·s) are selected as silicone elastomer base materials, both of which are provided by Dow Chemical Co., Ltd., USA. Cross-linking reaction occurs through Karstedt catalyst (concentration: 3000 ppm, provided by Beijing Huawei Ruike Chemical Co., Ltd.) and inhibitor (1-ethynyl-1-cyclohexanol, provided by Shanghai Aladdin Biochemical Technology Co., Ltd.); octavinyl POSS nanoparticles are provided by Shanghai Myrel Biochemical Technology Co., Ltd.
[0026] The specific steps are as follows, see Figure 1 :
[0027] Step 1: Stir 0.4 g of OV-POSS filler and 20 g of PMHS in toluene solvent (60 mL), add Karstedt catalyst (0.025 g) under dry nitrogen environment, and reflux through a condenser at 70 ° C for 2 hours. Nano-POSS is grafted onto the PMHS molecular chain through a hydrosilylation reaction, and then the solvent in the resulting mixture is removed by rotary evaporation. The originally loose SE molecular chains are tightly cross-linked around the POSS, forming a nano-spherical structure with a POSS cage structure as the core and a SE molecular chain as the shell, thereby preparing a POSS-grafted PMHS solution. POSS uniformly distributed in the solvent is conducive to the formation of nano-fillers with uniform size and can effectively avoid filler agglomeration on a microscopic scale.
[0028] Step 2: 12 g VPDMS, 0.25 g POSS-grafted PMHS, 0.05 g Karstedt catalyst and 0.025 g inhibitor were stirred at 25 °C for 30 min and vacuum degassed for multiple cycles.
[0029] Step 3: Pour the liquid mixture into a polytetrafluoroethylene mold and then cure it at 120 °C for 3 h to obtain a POSS-grafted silicone elastomer nanocomposite material, labeled as SE-POSS.
[0030] Example 2: The sample used in this example is the same as that in Example 1, and includes the following steps:
[0031] Step 1: Stir 0.1g of OV-POSS filler and 15g of PMHS in toluene solvent (50mL), add Karstedt catalyst (0.015g) under dry nitrogen environment, and reflux through a condenser at 70°C for 2 hours. Nano-POSS is grafted onto the PMHS molecular chain through a hydrosilylation reaction, and then the solvent in the resulting mixture is removed by rotary evaporation. The originally loose SE molecular chains are tightly cross-linked around the POSS, forming a nano-spherical structure with a POSS cage structure as the core and a SE molecular chain as the shell, thereby preparing a POSS-grafted PMHS solution. POSS uniformly distributed in the solvent is conducive to the formation of nano-fillers with uniform size and can effectively avoid filler agglomeration on a microscopic scale.
[0032] Step 2: 5 g VPDMS, 0.10 g POSS-grafted PMHS, 0.01 g Karstedt catalyst and 0.01 g inhibitor were stirred at 25 °C for 30 min and vacuum degassed for multiple cycles.
[0033] Step 3: Pour the liquid mixture into a polytetrafluoroethylene mold and then cure it at 120 °C for 3 h to obtain a POSS-grafted silicone elastomer nanocomposite material, labeled as SE-POSS.
[0034] Example 3: The sample used in this example is the same as that in Example 1, and includes the following steps:
[0035] Step 1: Stir 0.8 g of OV-POSS filler and 25 g of PMHS in toluene solvent (70 mL), add Karstedt catalyst (0.04 g) under dry nitrogen environment, and reflux through a condenser at 70 ° C for 2 hours. Nano-POSS is grafted onto the PMHS molecular chain through a hydrosilylation reaction, and then the solvent in the resulting mixture is removed by rotary evaporation. The originally loose SE molecular chains are tightly cross-linked around the POSS, forming a nano-spherical structure with a POSS cage structure as the core and a SE molecular chain as the shell, thereby preparing a POSS-grafted PMHS solution. POSS uniformly distributed in the solvent is conducive to the formation of nano-fillers with uniform size and can effectively avoid filler agglomeration on a microscopic scale.
[0036] Step 2: 25 g VPDMS, 0.4 g POSS-grafted PMHS, 0.1 g Karstedt catalyst and 0.04 g inhibitor were stirred at 25 °C for 30 min and vacuum degassed for multiple cycles.
[0037] Step 3: Pour the liquid mixture into a polytetrafluoroethylene mold and then cure it at 120 °C for 3 h to obtain a POSS-grafted silicone elastomer nanocomposite material, labeled as SE-POSS.
[0038] Example 4: The sample used in this example is the same as that in Example 1, and includes the following steps:
[0039] Step 1: Stir 0.6 g of OV-POSS filler and 20 g of PMHS in toluene solvent (60 mL), add Karstedt catalyst (0.03 g) under dry nitrogen environment, and reflux through a condenser at 70 ° C for 2 hours. Nano-POSS is grafted onto the PMHS molecular chain through a hydrosilylation reaction, and then the solvent in the resulting mixture is removed by rotary evaporation. The originally loose SE molecular chains are tightly cross-linked around the POSS, forming a nano-spherical structure with a POSS cage structure as the core and a SE molecular chain as the shell, thereby preparing a POSS-grafted PMHS solution. POSS uniformly distributed in the solvent is conducive to the formation of nano-fillers with uniform size and can effectively avoid filler agglomeration on a microscopic scale.
[0040] Step 2: 20 g VPDMS, 0.3 g POSS-grafted PMHS, 0.2 g Karstedt catalyst and 0.03 g inhibitor were stirred at 25 °C for 30 min and vacuum degassed for multiple cycles.
[0041] Step 3: Pour the liquid mixture into a polytetrafluoroethylene mold and then cure it at 120 °C for 3 h to obtain a POSS-grafted silicone elastomer nanocomposite material, labeled as SE-POSS.
[0042] Example 5: The sample used in this example is the same as that in Example 1, and includes the following steps:
[0043] Step 1: Stir 0.3 g of OV-POSS filler and 18 g of PMHS in toluene solvent (55 mL), add Karstedt catalyst (0.02 g) under dry nitrogen environment, and reflux through a condenser at 70 ° C for 2 hours. Nano-POSS is grafted onto the PMHS molecular chain through a hydrosilylation reaction, and then the solvent in the resulting mixture is removed by rotary evaporation. The originally loose SE molecular chains are tightly cross-linked around the POSS, forming a nano-spherical structure with a POSS cage structure as the core and a SE molecular chain as the shell, thereby preparing a POSS-grafted PMHS solution. POSS uniformly distributed in the solvent is conducive to the formation of nano-fillers with uniform size and can effectively avoid filler agglomeration on a microscopic scale.
[0044] Step 2: 10 g VPDMS, 0.2 g POSS-grafted PMHS, 0.05 g Karstedt catalyst and 0.02 g inhibitor were stirred at 25 °C for 30 min and vacuum degassed for multiple cycles.
[0045] Step 3: Pour the liquid mixture into a polytetrafluoroethylene mold and then cure it at 120 °C for 3 h to obtain a POSS-grafted silicone elastomer nanocomposite material, labeled as SE-POSS.
[0046] Comparative example: Pure silicone elastomer, marked as SE, is used. Pure silicone elastomer refers to a polymer elastic material composed mainly of silicon. Due to its unique physical and chemical properties, such as excellent temperature resistance, weather resistance, electrical insulation and good mechanical properties, it is widely used in many high-tech fields.
[0047] Furthermore, the applicant conducted performance tests on the sample SE-POSS marked in Example 1 and the SE in the comparative example.
[0048] In this embodiment, scanning electron microscopy is used to characterize the microscopic cross-sectional morphology of SE and SE-POSS materials. Thermogravimetric analysis is performed in nitrogen by a thermogravimetric analyzer, and the corresponding differential thermogravimetric curve is calculated to characterize the thermal weight loss rate. The temperature range of the test is 0-1000°C, and the heating rate is 0-20°C / min. The room temperature and high temperature insulation properties of SE and SE-POSS are characterized by measuring the conductivity and breakdown strength at room temperature and high temperature; the conductivity is evaluated under different electric fields by a three-electrode device; the breakdown strength of the material is measured by a packaged ball-ball electrode, the voltage rise rate is 0.5-2kV / s, and the breakdown field strength is analyzed by a two-parameter Weibull statistical method.
[0049] In this embodiment, the microscopic cross-sectional morphology of SE and SE-POSS materials was characterized by a Hitachi SU-8010 scanning electron microscope (SEM). Figure 2-3 As shown in the figure, the cross section of SE is smooth and free of impurities, and SE-POSS exhibits a uniform and dense nanostructure with a rough surface, indicating that the nano-POSS grafting affects the overall cross-linking process of the silicone elastomer and forms a dense nanosphere structure, in which the grafted nano-POSS is the core and the densely cross-linked silicone elastomer molecular chains form the shell.
[0050] In this embodiment, thermal gravimetric analysis (TGA) was performed in nitrogen using a US TA Q500 thermogravimetric analyzer, and the corresponding derivative thermogravimetry (DTG) curve was calculated to characterize the thermal weight loss rate. The test temperature range was 50-800°C, and the heating rate was 10°C / min. Figure 4 and Figure 5 The TGA and DTG curves of SE and SE-POSS are shown respectively. The temperature corresponding to the 90% weight loss rate of the TGA curve is generally defined as the thermal decomposition temperature. The thermal decomposition temperature and the temperature corresponding to the maximum weight loss rate of SE-POSS are higher than those of SE, which are increased by 27°C and 35°C respectively, indicating that SE-POSS has better thermal stability. The nanostructure introduced by the grafted POSS strengthens the cross-linked structure of the molecular chain and effectively hinders the high-temperature thermal degradation of the silicone elastomer.
[0051] In this example, the room temperature and high temperature insulation properties of SE and its nanocomposites were characterized by measuring the conductivity and breakdown strength at 30°C, 160°C and 200°C. The conductivity was evaluated at different electric fields of 5, 10, 15 and 20 kV / mm by a three-electrode device. The breakdown strength of the material was measured by encapsulated ball-ball electrodes to avoid surface flashover, with a voltage rise rate of 1 kV / s. The breakdown field strength was analyzed by the two-parameter Weibull statistical method, and the characteristic breakdown strength corresponding to a breakdown field strength of 63.2% breakdown probability was
[0052] Figure 6 and Figure 7 The conductivity and breakdown field strength of SE and SE-POSS are shown respectively. Figure 6 It can be seen that at the same temperature, the conductivity of SE-POSS is lower than that of SE, and the conductivity of both increases with increasing temperature. For example, at 200℃ and 20kV / mm, the conductivity of SE and SE-POSS are 6.8×10-12 and 1.8×10-12S / mm, respectively, and the conductivity of SE is 3.8 times that of SE-POSS. The lower conductivity is beneficial to reduce the power loss of SE nanocomposites. Figure 7 The Weibull distribution and characteristic breakdown strength of SE and SE-POSS. At the same temperature, the breakdown strength of SE-POSS is higher than that of SE, and its breakdown strength decreases with increasing temperature. For example, at a high temperature of 200°C, the breakdown field strengths of SE and SE-POSS are 35.8 and 39.6 kV / mm, respectively. The breakdown field strength of SE-POSS is 3.8 kV / mm higher than that of SE. The higher breakdown field strength is conducive to the reliable operation of high-temperature silicon carbide modules at higher voltages. SE-POSS has lower conductivity and higher breakdown strength at high temperatures, indicating that the grafted POSS nanofiller improves the high-temperature insulation properties of silicone elastomers.
[0053] In summary, the present invention can prevent POSS from participating in the curing process of silicone elastomer and reduce the possibility of agglomeration. The POSS grafted silicone elastomer nanocomposite prepared by the present invention can effectively improve the high temperature resistance and high temperature insulation performance of silicone elastomer materials for silicon carbide module packaging.
Claims
1. A method for improving the insulation performance of high-temperature silicon carbide devices by grafting nano-siloxane, characterized in that: The method comprises the following steps: Step 1: POSS filler is grafted onto PMHS molecular chain through hydrosilylation reaction to prepare POSS grafted PMHS solution; Step 2: The PMHS solution prepared in step 1 is fully stirred with VPDMS, a catalyst, and an inhibitor at room temperature and subjected to multiple cycles of vacuum degassing to obtain a liquid mixture; Step 3: pour the liquid mixture into a polytetrafluoroethylene mold, heat and cross-link and cure in a vacuum oven to obtain a POSS grafted silicon elastomer nanocomposite material, and use the POSS grafted silicon elastomer nanocomposite material as a silicon elastomer material for silicon carbide module packaging.
2. The method for improving the insulation performance of high-temperature silicon carbide devices by grafting nano-siloxane according to claim 1, characterized in that: In the step 1, 0.1-0.8 parts of POSS filler and 15-25 parts of PMHS are stirred in 50-70 parts of toluene solvent by mass, 0.01-0.04 parts of Karstedt catalyst are added in a dry nitrogen environment, and refluxed through a condenser at 60-80° C. for 1-3 hours; the solvent is removed by rotary evaporation to obtain a nano-spherical structure polymer with a POSS cage structure as a core and a SE molecular chain as an outer shell, that is, a POSS-grafted PMHS solution.
3. The method for improving the insulation performance of high-temperature silicon carbide devices by grafting nano-siloxane according to claim 2, characterized in that: In step 1, 0.4 g of POSS filler and 20 g of PMHS are stirred in 60 ml of toluene solvent, 0.025 g of Karstedt catalyst is added in a dry nitrogen environment, and refluxed at 70° C. through a condenser for 2 hours; the solvent is removed by rotary evaporation to obtain a nano-spherical structure polymer with a POSS cage structure as the core and a SE molecular chain as the shell, that is, a POSS-grafted PMHS solution.
4. The method for improving the insulation performance of high-temperature silicon carbide devices by grafting nano-siloxane according to claim 1, characterized in that: In step 2, 0.1-0.4 parts of the PMHS solution prepared in step 1 are mixed with 5-25 parts of VPDMS, 0.01-0.1 parts of Karstedt catalyst, and 0.01-0.04 parts of inhibitor by mass at 20-30° C. and stirred for 20-40 minutes for multiple cycles of vacuum degassing.
5. The method for improving the insulation performance of high temperature silicon carbide devices by grafting nano-siloxane according to claim 4, characterized in that: In step 2, 0.25 g of the PMHS solution prepared in step 1 was mixed with 12 g of VPDMS, 0.05 g of Karstedt catalyst, and 0.025 g of inhibitor at 20-30° C. and stirred for 30 minutes for multiple cycles of vacuum degassing.
6. The method for improving the insulation performance of high temperature silicon carbide devices by grafting nano-siloxane according to claim 1, characterized in that: In step three, the liquid mixture is poured into a polytetrafluoroethylene mold, and then cured at 100-150° C. for 2-4 hours to obtain a POSS-grafted silicone elastomer nanocomposite material.
7. The method for improving the insulation performance of high temperature silicon carbide devices by grafting nano-siloxane according to claim 6, characterized in that: In step three, the liquid mixture is poured into a polytetrafluoroethylene mold and then cured at 120° C. for 3 hours to obtain a POSS-grafted silicone elastomer nanocomposite material.
Citation Information
Patent Citations
Polysilsesquioxane reinforced light emitting diode (LED) encapsulation organic silicon rubber and preparation method thereof
CN102181159A
Vinyl POSS (polyhedral oligomeric silsesquioxane) modified organic silicon resin, and preparation method and application thereof
CN104151763A
Preparation method for high-permeable ultraviolet silicon rubber
CN109180946A
Addition type liquid silicone rubber modified by liquid vinyl polyhedral oligomeric silsesquioxane and preparation method of addition type liquid silicone rubber
CN115960464A
Silica gel insulating material for packaging silicon carbide power device and application of silica gel insulating material
CN116574384A
Cited By
Organic semiconductive micromolecule / silicon elastomer nano composite material as well as preparation method and application thereof
CN122213689A