Sealing strip for vehicle-mounted refrigerator and preparation method of sealing strip
The on-board refrigerator seal strips prepared with raw materials such as silicone and nano-solid fillers have been solved, and the problems of seal strips are achieved are achieved in a good sealing effect in complex environments and weather resistance and earthquake resistance for long-term use.
Patent Information
- Application Number
- CN202411144181.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The seal strips of the on-board refrigerator are prone to aging and wear during frequent bumps, climate change, temperature changes and long-term use, resulting in a degradation of sealing performance and unable to effectively maintain the temperature in the refrigerator, affecting the refrigeration effect.
The sealing strip is prepared using raw materials such as silicone, vulcanizing agent, hydrogen-containing silicone oil, vinyl trimethoxysilane and nano-solid fillers. The three-dimensional network structure is formed through vulcanization reaction, which improves the seismic resistance, weather resistance and elasticity of the sealing strip, and passes through nano-solids. Pretreatment of fillers improves sealing performance.
The sealing strip maintains a good sealing effect in complex environments, has excellent shock resistance, wear resistance and elasticity, and can be used for a long time without losing sealing performance, which improves the refrigeration efficiency and service life of the refrigerator.
Smart Images

Figure BDA0005001763750000051 
Figure BDA0005001763750000061 
Figure BDA0005001763750000091
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of refrigerator sealing material processing, and more specifically, to a sealing strip for a vehicle refrigerator and a preparation method thereof. Background Art
[0002] The car sealing strip is a refrigerator sealing strip designed specifically for the car environment to meet the special requirements of vibration, temperature changes and space limitations that the car may encounter during driving. It can ensure that the car refrigerator maintains good sealing performance during driving, prevent cold air leakage, keep the temperature inside the box stable, and reduce the impact of noise and vibration on the sealing effect. Therefore, for long-distance travelers who need to be on the road for a long time, the importance of the car refrigerator sealing strip is self-evident.
[0003] However, in actual use, it is found that frequent bumps, climate changes, temperature changes, long-term use and frequent opening and closing of the door will cause the sealing strip to gradually age and wear, and then lose its original elasticity and sealing performance, and easily deform, dent and other problems, resulting in the refrigerator door cannot be closed tightly, cold air overflows, and seriously affects the refrigeration effect of the refrigerator. Summary of the invention
[0004] In order to solve the problem that frequent bumps, climate changes, temperature changes, long-term use and frequent door opening and closing operations may cause the sealing strip of a vehicle refrigerator to gradually age and wear, the present application provides a sealing strip for a vehicle refrigerator and a preparation method thereof.
[0005] In a first aspect, the present application provides a sealing strip for a vehicle refrigerator, which adopts the following technical solution: A sealing strip for a car refrigerator is prepared from the following raw materials in percentage by weight: Silicone 60-70% Vulcanizing agent 0.1-0.3% Accelerator 0.5-1% Hydrogen silicone oil 4-8% Dimethicone 0.8-1% Masterbatch 0.2-0.3% Vinyltrimethoxysilane 5-6% The remaining amount is nano solid filler; The silica gel is obtained by mixing silica gel I, silica gel II and silica gel III in a weight ratio of (5-8): (2-5): 1; Silicone rubber I is methyl vinyl silicone rubber with a molecular weight of 80,000-150,000 and a vinyl molar content of 0.1-0.5%; Silicone rubber II is methylphenyl vinyl silicone rubber with a molecular weight of 200,000-500,000, a phenyl molar content of 10-15%, and a vinyl molar content of 0.6-1.5%; Silicone rubber III is methyl vinyl silicone rubber with a molecular weight of 300,000-500,000 and a vinyl molar content of 0.3-0.6%.
[0006] By adopting the above technical solution, the sealing strip for the vehicle refrigerator has good shock resistance, weather resistance, drop resistance and elasticity, can be used in relatively complex environments, and can maintain the sealing effect for a long time.
[0007] Among them, the low molecular weight silicone I contains a proper amount of vinyl, which provides good processing performance and preliminary cross-linking points, helps the fluidity of the sealing strip during the molding process and the strength after curing, and gives the sealing strip better deformation recovery ability; methylphenyl vinyl silicone rubber contains phenyl and vinyl. The introduction of phenyl enhances the oxidation resistance and weather resistance of silicone, making the sealing strip still stable under extreme climatic conditions, and vinyl further promotes the cross-linking reaction, improving the strength and elasticity of the sealing strip; silicone III enhances the overall toughness and wear resistance of the sealing strip, ensuring long-term stability. The combination of the three enables the sealing strip to effectively absorb energy and quickly return to its original state when it is vibrated, thereby showing excellent anti-seismic performance and elasticity, ensuring that even under the deformation caused by frequent opening and closing of the door, the sealing strip can quickly return to its original shape and maintain the sealing effect.
[0008] Vulcanizing agent is the key substance that promotes cross-linking reaction between silicone molecules, forming a three-dimensional network structure, thereby improving the strength and elasticity of the sealing strip. The right amount of vulcanizing agent can ensure the complete vulcanization process without causing excessive cross-linking and making the material brittle. It accelerates the vulcanization reaction, shortens the vulcanization time, and improves production efficiency. At the same time, it can also help the vulcanizing agent to be more evenly dispersed in the silicone to ensure the uniformity of the vulcanization process. Hydrogen-containing silicone oil undergoes an addition reaction with vinyl, participates in the vulcanization process, and enhances the cross-linking density, thereby improving the strength and weather resistance of the sealing strip. Dimethyl silicone oil improves the processing properties of silicone, and also helps to improve the softness and smoothness of the sealing strip. Vinyl trimethoxysilane: As a cross-linking agent, it reacts with the vinyl in silicone to promote the vulcanization process, while improving the cross-linking density, elasticity and weather resistance of the sealing strip.
[0009] Nano solid fillers are filled in the silica gel matrix, which can significantly improve the hardness, wear resistance, tensile strength and dimensional stability of the sealing strip. At the same time, nano-scale particles can effectively block the penetration of gas and water, improving the sealing performance.
[0010] Masterbatch is used to adjust the color of silicone.
[0011] Preferably, the nano solid filler is pretreated by the following method: 1) soaking the nano solid filler in hydrogen peroxide, filtering, and drying to obtain a hydroxylated nano solid filler; 2) mixing the hydroxylated nano solid filler and divinyltetramethyldisilazane, heating to 70-80° C., and stirring until no liquid is present, thereby obtaining a pretreated nano solid filler; The weight ratio of the nano solid filler to divinyltetramethyldisilazane is (10-12):3.
[0012] By adopting the above technical solution, hydroxyl groups are introduced on the surface of the nano solid filler by immersing it in hydrogen peroxide. The introduction of hydroxyl groups enhances the interaction between the nano solid filler and silica gel, and improves the compatibility and bonding strength between the two. At the same time, hydroxylation also helps to improve the dispersibility of the nano solid filler in silica gel, reduce agglomeration, and make the composite material more uniform.
[0013] The hydroxylated nano solid filler is mixed with divinyltetramethyldisilazane and stirred at a certain temperature to make the two react. That is, silazane is introduced on the surface of the nano solid filler to form an organic silicon layer on the surface, which helps the nano solid filler to better fuse with silica gel. The formed composite material has better density and elasticity, which can effectively improve the sealing performance of the sealing strip, reduce cold air leakage, and improve the refrigeration efficiency of the car refrigerator. At the same time, the addition of silazane gives the composite material a certain hydrophobicity and aging resistance, which is conducive to the use of the car refrigerator sealing strip in a humid environment with large temperature changes.
[0014] At the same time, hydrogen peroxide and divinyltetramethyldisilazane are both environmentally friendly materials, and the pretreatment process does not produce harmful substances, which meets environmental protection requirements.
[0015] Preferably, the average particle size of the nano solid filler is 20-500 nm.
[0016] By adopting the above technical solution, the average particle size of the nano solid filler is optimized, so that it can be dispersed more evenly in the silica gel, reducing voids and defects, thereby improving the density of the sealing strip. At the same time, within this particle size range, the sealing strip can also have good toughness and strength.
[0017] Preferably, the nano solid filler is obtained by mixing zinc oxide whiskers and silicon dioxide in a weight ratio of (2-4):3.
[0018] By adopting the above technical solution, the types of nano solid fillers are optimized, and the strength, weather resistance, high and low temperature resistance and drop resistance of the sealing strip of the car refrigerator are further improved.
[0019] Preferably, the hydrogen content of the hydrogen-containing silicone oil is 1.5-4%, and the molecular weight is 15000-30000.
[0020] By adopting the above technical solution, the parameters of hydrogen-containing silicone oil are optimized, and the strength and elasticity of the sealing strip are further improved, making it more durable and able to withstand the deformation caused by temperature changes and mechanical stress during the use of the car refrigerator. At the same time, the aging resistance of the sealing strip can also be improved.
[0021] Preferably, the viscosity of the dimethyl silicone oil at 25° C. is 1000-5000 mPa.s.
[0022] By adopting the above technical scheme, the viscosity of dimethyl silicone oil is optimized, which helps to form a stable structure in silica gel. Preferably, the accelerator is one of 2-thiolbenzothiazole, N-oxydiethylene-2-benzothiazolesulfenamide, N-cyclohexyl-2-benzothiazolesulfenamide or tetramethylthiuram disulfide.
[0023] By adopting the above technical solution, the types of accelerators are optimized, the vulcanization reaction process is accelerated, and the production efficiency is improved. At the same time, it helps to obtain a uniform and dense vulcanization network, thereby enhancing the elasticity, weather resistance and sealing of the sealing strip.
[0024] Preferably, the vulcanizing agent is a platinum vulcanizing agent.
[0025] By adopting the above technical solution, the platinum vulcanizer has the characteristics of low vulcanization temperature and fast vulcanization speed, which greatly improves production efficiency. It can complete the vulcanization process in a short time, reduce the production cycle, and meet the needs of rapid production. At the same time, the platinum vulcanizer does not contain toxic and harmful substances and is more environmentally friendly.
[0026] In a second aspect, the present application provides a method for preparing a sealing strip for a vehicle refrigerator, using the following technical solution: A method for preparing a sealing strip for a vehicle refrigerator comprises the following steps: S1, stirring and mixing hydrogen-containing silicone oil, masterbatch, nano solid filler and vinyltrimethoxysilane to obtain mixture 1; S2, mixing silica gel, vulcanizing agent, accelerator, dimethyl silicone oil and the mixture to obtain mixture 2; S3, vulcanizing the mixture 2 to obtain a sealing strip for a vehicle refrigerator.
[0027] By adopting the above technical scheme, the sealing strip for the vehicle refrigerator has good strength, weather resistance, elasticity, high and low temperature resistance and drop resistance, can have good shock resistance, can be used in various complex environments, and can still maintain good sealing.
[0028] Preferably, in step S3, the vulcanization includes a first vulcanization and a second vulcanization performed sequentially, wherein the first vulcanization temperature is 170-190°C, the time is 10-15min, and the pressure is 12-15MPa; the second vulcanization temperature is 120-150°C, the time is 30-40min, and the pressure is 8-10MPa.
[0029] By adopting the above technical solution, the silicone can be fully cross-linked. The two vulcanization processes make the cross-linking structure inside the silicone product more perfect and the cross-linking density increased, which helps to improve the strength, high and low temperature resistance, aging resistance and other properties of the silicone sealing strip used for car refrigerators.
[0030] In summary, this application has the following beneficial effects: 1. Excellent aging resistance and wear resistance: The polymer chain structure of the silicone matrix and the addition of nanofillers enable the sealing strip to withstand various challenges of the vehicle environment for a long time and maintain stable physical properties.
[0031] 2. Excellent elasticity and sealing performance: The mixed use of multiple silicones and the synergistic effect of vulcanizers, accelerators and cross-linking agents ensure that the sealing strip can quickly return to its original shape when subjected to external forces such as extrusion and stretching, maintaining a tight sealing effect.
[0032] 3. Good processing performance: The addition of dimethyl silicone oil and internal lubricant makes the rubber have good fluidity during processing, which is convenient for molding and demoulding. DETAILED DESCRIPTION Example
[0033] Example 1 A sealing strip for a vehicle refrigerator is prepared by the following method: S1, 400 g of hydrogenated silicone oil, 20 g of masterbatch, 2940 g of nano solid filler (silicon dioxide), and 500 g of vinyltrimethoxysilane were stirred and mixed at a stirring temperature of 60° C. for 30 min to obtain a mixture 1; S2, mixing 60000 g of silica gel, 10 g of vulcanizing agent (platinum catalyst), 50 g of accelerator (2-mercaptobenzothiazole), 80 g of dimethyl silicone oil and the mixture at a stirring temperature of 40° C. for 15 min to obtain a mixture 2; S3, vulcanizing the mixture 2 to obtain a sealing strip for a vehicle refrigerator.
[0034] The silica gel is obtained by mixing silica gel I, silica gel II and silica gel III in a weight ratio of 5:2:1; Silicone rubber I is methyl vinyl silicone rubber with a molecular weight of 80,000 and a vinyl molar content of 0.1%; Silicone II is methylphenyl vinyl silicone rubber with a molecular weight of 200,000, a phenyl molar content of 10%, and a vinyl molar content of 0.6%; Silicone rubber III is methyl vinyl silicone rubber with a molecular weight of 300,000 and a vinyl molar content of 0.3%.
[0035] The hydrogen content of hydrogen-containing silicone oil is 1.5% and the molecular weight is 15,000.
[0036] The viscosity of dimethyl silicone oil at 25°C is 1000mpa.s.
[0037] The CAS number of the platinum catalyst is 68478-92-2, which was purchased from Hubei Shineng Chemical Technology Co., Ltd.
[0038] The difference between Example 2-3 and Example 1 is that the types, amounts and experimental parameters of some raw materials used to prepare the sealing strip for the vehicle refrigerator are different. The specific differences are shown in Table 1: Table 1 Raw material types, amounts and experimental parameters for preparing sealing strips for vehicle refrigerators in Examples 1-3 In Example 2, the silica gel is obtained by mixing silica gel I, silica gel II and silica gel III in a weight ratio of 7:4:1; Silicone rubber I is methyl vinyl silicone rubber with a molecular weight of 120,000 and a vinyl molar content of 0.3%; Silicone II is methylphenyl vinyl silicone rubber with a molecular weight of 350,000, a phenyl molar content of 12%, and a vinyl molar content of 1%; Silicone rubber III is methyl vinyl silicone rubber with a molecular weight of 400,000 and a vinyl molar content of 0.5%.
[0039] In Example 3, the silica gel is obtained by mixing silica gel I, silica gel II and silica gel III in a weight ratio of 8:5:1; Silicone rubber I is methyl vinyl silicone rubber with a molecular weight of 150,000 and a vinyl molar content of 0.5%; Silicone II is methylphenyl vinyl silicone rubber with a molecular weight of 500,000, a phenyl molar content of 15%, and a vinyl molar content of 1.5%; Silicone rubber III is methyl vinyl silicone rubber with a molecular weight of 500,000 and a vinyl molar content of 0.6%.
[0040] Example 4 A sealing strip for a vehicle refrigerator, the difference between this embodiment and embodiment 1 is that the nano solid filler is pretreated by the following method: 1) soaking 2940 g of nano solid filler (silicon dioxide, average particle size of 20-100 nm) in hydrogen peroxide (mass fraction of 15%), filtering, and drying to obtain hydroxylated nano solid filler; 2) Mixing the hydroxylated nano solid filler and 882 g of divinyltetramethyldisilazane, heating to 70° C., and stirring until there is no liquid, thereby obtaining a pretreated nano solid filler; The weight ratio of the nano solid filler to divinyltetramethyldisilazane is 10:3.
[0041] Example 5 A sealing strip for a vehicle refrigerator, the difference between this embodiment and embodiment 4 is that the nano solid filler is pretreated by the following method: 1) soaking 2940 g of nano solid filler (silicon dioxide, average particle size of 20-100 nm) in hydrogen peroxide (mass fraction of 20%), filtering, and drying to obtain hydroxylated nano solid filler; 2) Mixing the hydroxylated nano solid filler and 1176 g of divinyltetramethyldisilazane, heating to 80° C., and stirring until there is no liquid, thereby obtaining a pretreated nano solid filler; The weight ratio of the nano solid filler to divinyltetramethyldisilazane is 12:3.
[0042] Example 6 A sealing strip for a vehicle refrigerator. The difference between this embodiment and embodiment 1 is that the nano solid filler is obtained by mixing zinc oxide whiskers and silicon dioxide in a weight ratio of 2:3.
[0043] Example 7 A sealing strip for a vehicle refrigerator. The difference between this embodiment and embodiment 4 is that the nano solid filler is obtained by mixing zinc oxide whiskers and silicon dioxide in a weight ratio of 4:3.
[0044] Example 8 A sealing strip for a vehicle refrigerator. The difference between this embodiment and embodiment 1 is that the nano solid filler is zinc oxide whisker.
[0045] Example 9 A sealing strip for a vehicle refrigerator. The difference between this embodiment and embodiment 1 is that the hydrogen content of the hydrogen-containing silicone oil is 1% and the molecular weight is 15,000.
[0046] Example 10 A sealing strip for a vehicle refrigerator, the difference between this embodiment and embodiment 1 is that the average particle size of the nano solid filler is 15 nm.
[0047] Embodiment 11 A sealing strip for a vehicle refrigerator. The difference between this embodiment and embodiment 1 is that the viscosity of the dimethyl silicone oil at 25° C. is 800 mPa.s.
[0048] Comparative Example Comparative Example 1 A sealing strip for a car refrigerator. The difference between this comparative example and Example 1 is that methyl vinyl silicone rubber is used instead of an equal amount of methyl phenyl vinyl silicone rubber.
[0049] The molecular weight of methyl vinyl silicone rubber is 200,000 and the vinyl molar content is 0.6%.
[0050] Comparative Example 2 A sealing strip for a car refrigerator. The difference between this comparative example and Example 1 is that the silica gel is obtained by mixing silica gel I and silica gel II in a weight ratio of 5:3.
[0051] Comparative Example 3 A sealing strip for a car refrigerator. The difference between this comparative example and Example 1 is that the silica gel is obtained by mixing silica gel I and silica gel III in a weight ratio of 5:1.
[0052] Comparative Example 4 A sealing strip for a car refrigerator. The difference between this comparative example and Example 1 is that the silica gel is obtained by mixing silica gel II and silica gel III in a weight ratio of 2:1.
[0053] Comparative Example 5 A sealing strip for a car refrigerator. The difference between this comparative example and Example 1 is that all the silica gel is silica gel I.
[0054] Comparative Example 6 A sealing strip for a car refrigerator. The difference between this comparative example and Example 1 is that fatty acid monoglyceride is used instead of vinyltrimethoxysilane of the same mass.
[0055] Performance testing The sealing strips for vehicle refrigerators prepared in Examples 1-11 and Comparative Examples 1-6 were subjected to compression permanent deformation test, tensile strength test, weather resistance test, high and low temperature resistance test and drop resistance test.
[0056] Detection method / test method Compression set: According to GB / T7759.2-2014 standard, it is expressed by testing its compression set percentage at 0℃ / 72 hours.
[0057] Tensile strength: According to the provisions of GB / T 528-2009, the specimen is a type A ring specimen, and its tensile strength is tested in MPa.
[0058] Weather resistance test: According to the provisions of GB T 3511-2018 and GB / T16422.2-2014, irradiate the sample for 168 hours, test and calculate the performance retention percentage of its tensile strength in %.
[0059] High and low temperature resistance test: The sealing strips for car refrigerators prepared in the examples and comparative examples were placed in a 100°C environment for 5 hours, and then placed in a -20°C environment for 5 hours, and the cycle was repeated 100 times. The tensile strength retention percentage was tested and calculated in %.
[0060] Drop resistance test: The sealing strips for car refrigerators prepared in the examples and comparative examples were dropped from a height of 0.5 m by an iron sheet with a length, width and thickness of 50 cm*cm*0.5 cm. After 5000 times, the tensile strength retention percentage was tested and calculated. The experimental data are shown in Table 2: Table 2 Experimental data of Examples 1-11 and Comparative Examples 1-6 It can be seen from Examples 1-11 and Comparative Examples 1-6 in combination with Table 2 that the sealing strip for a car refrigerator prepared by the formula in the present application has good elasticity and drop resistance, so that the sealing strip can maintain good sealing after long-distance travel. At the same time, it also has good weather resistance and high and low temperature resistance, so that the sealing strip can adapt to different complex environments and has a long service life.
[0061] By comparing Example 1 with Comparative Examples 1-6, in the tensile strength test, the tensile strength of Example 1 is higher than that of Comparative Examples 1-6; in the rebound resilience test, the compression permanent deformation in Example 1 is significantly smaller than that of Comparative Examples 1-6, indicating that the sealing strip for the vehicle refrigerator prepared by the present application has good elasticity; in the weather resistance test, the tensile strength retention rate of Example 1 is higher than that of Comparative Examples 1-6; in the high and low temperature resistance test, the tensile strength retention rate of Example 1 is higher than that of Comparative Examples 1-6; in the drop resistance test, the tensile strength retention rate of Example 1 is higher than that of Comparative Examples 1-6; from the experimental results of Example 1 and Comparative Examples 1-6, the sealing strip of the vehicle refrigerator prepared by the present application has good strength, good elasticity, good weather resistance, good high and low temperature resistance and good drop resistance, and is suitable for long-distance use.
[0062] Compared with Example 1 and Example 4-5, in the tensile strength test, the tensile strength of Example 4-5 is improved; in the compression permanent deformation test, the compression permanent deformation of Example 4-5 is reduced; in the weather resistance test, the tensile strength retention rate of Example 4-5 is improved; in the high and low temperature resistance test, the tensile strength retention rate of Example 4-5 is improved; in the drop resistance test, the tensile strength retention rate of Example 4-5 is improved; from the experimental results of Example 1 and Example 4-5, it can be seen that pre-treating the nano solid filler by the method in the present application is beneficial to improving the strength, elasticity, weather resistance, high and low temperature resistance and drop resistance of the sealing strip of the car refrigerator.
[0063] Comparing Example 1 with Example 6, in the tensile strength test, the tensile strength of Example 6 is improved; in the compression permanent deformation test, the compression permanent deformation of Example 6 is reduced; in the weather resistance test, the tensile strength retention rate of Example 6 is improved; in the high and low temperature resistance test, the tensile strength retention rate of Example 6 is improved; in the drop resistance test, the tensile strength retention rate of Example 6 is improved; Comparing Example 4 with Example 7, in the tensile strength test, the tensile strength of Example 7 is improved; in the compression permanent deformation test, the compression permanent deformation of Example 7 is reduced; in the weather resistance test, the tensile strength retention rate of Example 7 is improved; in the high and low temperature resistance test, the tensile strength retention rate of Example 7 is improved; in the drop resistance test, the tensile strength retention rate of Example 7 is improved.
[0064] Comparing Example 1 with Example 8, in the tensile strength test, the tensile strength of Example 8 decreased; in the compression permanent deformation test, the compression permanent deformation of Example 8 decreased; in the weather resistance test, the tensile strength retention rate of Example 8 increased; in the high and low temperature resistance test, the tensile strength retention rate of Example 8 decreased; in the drop resistance test, the tensile strength retention rate of Example 8 decreased.
[0065] From the experimental results of Examples 1 and 6, 4 and 7, and 1 and 8, it can be seen that optimizing the type and amount of nano solid fillers is beneficial to improving the strength, elasticity, weather resistance, high and low temperature resistance, and drop resistance of the sealing strip of the car refrigerator.
[0066] Comparing Example 1 with Example 9, in the tensile strength test, the tensile strength of Example 9 is reduced; in the compression permanent deformation test, the compression permanent deformation of Example 9 is increased; in the weather resistance test, the tensile strength retention rate of Example 9 is reduced; in the high and low temperature resistance test, the tensile strength retention rate of Example 9 is reduced; in the drop resistance test, the tensile strength retention rate of Example 9 is reduced; this indicates that optimizing the hydrogen content of hydrogen-containing silicone oil is beneficial to improving the strength, elasticity, weather resistance, high and low temperature resistance and drop resistance of the sealing strip of the car refrigerator.
[0067] Comparing Example 1 with Example 10, in the tensile strength test, the tensile strength of Example 10 decreased; in the compression permanent deformation test, the compression permanent deformation of Example 10 increased; in the weather resistance test, the tensile strength retention rate of Example 10 decreased; in the high and low temperature resistance test, the tensile strength retention rate of Example 10 decreased; in the drop resistance test, the tensile strength retention rate of Example 10 decreased; This indicates that optimizing the average particle size of the nano solid filler is beneficial to improving the strength, elasticity, weather resistance, high and low temperature resistance and drop resistance of the sealing strip of the car refrigerator.
[0068] Comparing Example 1 with Example 11, in the tensile strength test, the tensile strength of Example 11 is basically consistent with that of Example 1; in the compression permanent deformation test, the compression permanent deformation of Example 11 increases; in the weather resistance test, the tensile strength retention rate of Example 11 is basically consistent with that of Example 1; in the high and low temperature resistance test, the tensile strength retention rate of Example 11 is basically consistent with that of Example 1; in the drop resistance test, the tensile strength retention rate of Example 11 decreases; This indicates that by optimizing the viscosity of dimethyl silicone oil, it is beneficial to improve the strength, elasticity, weather resistance, high and low temperature resistance and drop resistance of the sealing strip of the car refrigerator.
[0069] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A sealing strip for a vehicle refrigerator, characterized in that: Prepared from the following raw materials in weight percentage: Silicone 60-70% Vulcanizing agent 0.1-0.3% Accelerator 0.5-1% Hydrogen silicone oil 4-8% Dimethyl silicone oil 0.8-1% Masterbatch 0.2-0.3% Vinyltrimethoxysilane 5-6% The remaining amount is nano solid filler; The silica gel is obtained by mixing silica gel I, silica gel II and silica gel III in a weight ratio of (5-8): (2-5): 1; Silicone rubber I is methyl vinyl silicone rubber with a molecular weight of 80,000-150,000 and a vinyl molar content of 0.1-0.5%; Silicone II is methylphenyl vinyl silicone rubber with a molecular weight of 200,000-500,000, a phenyl molar content of 10-15%, and a vinyl molar content of 0.6-1.5%; Silicone rubber III is methyl vinyl silicone rubber with a molecular weight of 300,000-500,000 and a vinyl molar content of 0.3-0.6%.
2. A sealing strip for a vehicle refrigerator according to claim 1, characterized in that: The nano solid filler is pretreated by the following method: 1) Soaking the nano solid filler in hydrogen peroxide, filtering, and drying to obtain a hydroxylated nano solid filler; 2) Mixing the hydroxylated nano solid filler and divinyltetramethyldisilazane, heating to 70-80°C, and stirring until there is no liquid, thereby obtaining a pretreated nano solid filler; Wherein, the weight ratio of the nano solid filler to divinyltetramethyldisilazane is (10-12):
3.
3. A sealing strip for a vehicle refrigerator according to claim 2, characterized in that: The average particle size of the nano solid filler is 20-500nm.
4. The sealing strip for a vehicle refrigerator according to claim 1, characterized in that: The nano solid filler is obtained by mixing zinc oxide whiskers and silicon dioxide in a weight ratio of (2-4):
3.
5. The sealing strip for a vehicle refrigerator according to claim 4, characterized in that: The hydrogen content of the hydrogen-containing silicone oil is 1.5-4%, and the molecular weight is 15000-30000.
6. The sealing strip for a vehicle refrigerator according to claim 4, characterized in that: The viscosity of the dimethyl silicone oil at 25° C. is 1000-5000 mPa.s.
7. The sealing strip for a vehicle refrigerator according to claim 1, characterized in that: The accelerator is one of 2-thiolbenzothiazole, N-oxydiethylene-2-benzothiazole sulfenamide, N-cyclohexyl-2-benzothiazole sulfenamide or tetramethylthiuram disulfide.
8. The sealing strip for a vehicle refrigerator according to claim 1, characterized in that: The vulcanizing agent is a platinum vulcanizing agent.
9. A method for preparing a sealing strip for a vehicle refrigerator according to any one of claims 1 to 8, characterized in that: The method comprises the following preparation steps: S1, stirring and mixing hydrogen-containing silicone oil, masterbatch, nano solid filler and vinyltrimethoxysilane to obtain mixture 1; S2, mixing silica gel, vulcanizing agent, accelerator, dimethyl silicone oil and the mixture to obtain mixture 2; S3, vulcanizing the mixture 2 to obtain a sealing strip for a vehicle refrigerator.
10. The method for preparing a sealing strip for a vehicle refrigerator according to claim 9, characterized in that: In step S3, the vulcanization includes a first vulcanization and a second vulcanization performed sequentially, wherein the first vulcanization temperature is 170-190°C, the time is 10-15min, and the pressure is 12-15MPa; the second vulcanization temperature is 120-150°C, the time is 30-40min, and the pressure is 8-10MPa.
Citation Information
Patent Citations
Single-component liquid silicone rubber and preparation method thereof
CN111171577A
Organosilicon modified acrylic acid secondary dispersion and preparation method thereof
CN112940203A
High-resilience flame-retardant silicone rubber foam and preparation method thereof
CN117683357A