Coating material, carbon-ceramic brake disc with wear-resistant coating formed by coating material in one time and preparation method of carbon-ceramic brake disc
By using composite coating materials of silicon carbide, carbon black, polyvinyl alcohol and glycerol on the carbon ceramic brake disc, combined with vacuum and high temperature treatment, the friction coefficient fluctuation of the carbon ceramic brake disc is solved, and stable and wear-resistant are achieved The carbon ceramic brake disc extends the service life and reduces production costs.
Patent Information
- Application Number
- CN202410941124.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-01
AI Technical Summary
The friction surface of traditional carbon ceramic brake discs fluctuate greatly due to uneven phase distribution, which affects the stability and service life of the braking process.
Using a coating material, including 20-40 wt% silicon carbide, 10-20 wt% carbon black, 5-15 wt% polyvinyl alcohol and 5-10 wt% glycerol, through a single-mold coating technology, combined with vacuum treatment With high-temperature ceramicization treatment, a uniform composite phase system is formed, overcoming the problem of uneven phase distribution.
It effectively stabilizes the friction coefficient, extends the service life of the carbon ceramic brake disc, simplifies the preparation process, reduces costs, and achieves good friction performance and wear resistance.
Smart Images

Figure CN118879136A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon-ceramic brake discs, and in particular to a coating material, a carbon-ceramic brake disc with a wear-resistant coating formed by the coating material in a single step, and a preparation method thereof. Background Art
[0002] Carbon fiber reinforced silicon carbide (C / SiC) and carbon fiber reinforced carbon / silicon carbide dual-base (C / C-SiC) composites are collectively referred to as carbon-ceramic composites. Carbon-ceramic composites have the advantages of high strength, low density, and high temperature resistance. Carbon-ceramic composites have a lower density than cast iron materials (2.0-2.5g / cm 3 ), and because an appropriate amount of SiC hard phase is introduced as a matrix on the basis of C / C composite materials, the friction coefficient and oxidation resistance of the material can be effectively improved, and the sensitivity of the friction performance of the material to external conditions (temperature, humidity, etc.) can be significantly reduced. Among them, carbon ceramic brake discs are widely used in the field of vehicle braking.
[0003] However, the friction surface of the carbon-ceramic brake disc prepared by traditional technology is usually composed of three phases: carbon phase, silicon phase and silicon carbide phase. The uneven distribution of the three phases leads to large fluctuations in the friction coefficient of the friction pair during the braking process. Under continuous high-speed braking conditions, the energy generated during the braking process will cause the surface of the carbon-ceramic brake disc to heat up rapidly, thereby affecting the poor friction stability and service life of the carbon-ceramic brake disc. Summary of the invention
[0004] The invention solves the technical problem of large fluctuation of friction coefficient on the friction surface of the existing carbon-ceramic brake disc by disclosing a coating material, a carbon-ceramic brake disc with a single-shot wear-resistant coating formed therefrom and a preparation method thereof.
[0005] To solve the above technical problems, the present invention provides a coating material in the first aspect. The coating material comprises the following components by weight percentage: 20-40wt% silicon carbide, 10-20wt% carbon black, 5-15wt% polyvinyl alcohol, 5-10wt% glycerol, and 25-60wt% water.
[0006] In some embodiments, the coating material consists of 30 wt % silicon carbide, 15 wt % carbon black, 10 wt % polyvinyl alcohol, 5 wt % glycerol, and 40 wt % water, by weight percentage.
[0007] In some embodiments, the silicon carbide has a particle size of 20-50 μm.
[0008] In some embodiments, the silicon carbide has a particle size of 20 μm.
[0009] In a second aspect, the present invention provides a method for preparing the coating material, comprising: dissolving polyvinyl alcohol in water and mixing the mixture evenly to obtain a polyvinyl alcohol solution; then sequentially adding silicon carbide and carbon black to the polyvinyl alcohol solution, stirring the mixture evenly, and then adding glycerol and mixing the mixture evenly to obtain the coating material.
[0010] The present invention provides a carbon-ceramic brake disc with a single-molded wear-resistant coating in a third aspect, comprising the coating material.
[0011] In a fourth aspect, the present invention provides a method for preparing the carbon-ceramic brake disc with a single-molded wear-resistant coating, comprising the following steps:
[0012] preparing a carbon / carbon composite material preform;
[0013] Machining the carbon / carbon composite material preform and providing grooves on the designed upper and lower surfaces thereof to obtain a carbon / carbon preformed disk;
[0014] The grooves on the upper and lower surfaces of the carbon / carbon prefabricated disc are respectively coated and filled with the coating material once, and after filling, vacuum treatment and drying are performed to obtain a carbon / carbon prefabricated disc with a single molding prefabricated coating;
[0015] The carbon / carbon prefabricated disc body with the single-molded prefabricated coating is subjected to a carbonization treatment and a high-temperature ceramicization treatment in sequence to obtain a carbon-ceramic brake disc with a single-molded wear-resistant coating.
[0016] The present invention illustratively provides a method for preparing a carbon / carbon composite material preform, preferably comprising:
[0017] The carbon fiber mat and the carbon fiber free weft fabric are alternately layered in a stacking manner of carbon fiber mat layer / 0° carbon fiber free weft fabric layer / carbon fiber mat layer / 90° carbon fiber free weft fabric layer, and then needle-punched with a needle with barbed edges in a direction perpendicular to the stacking layer to obtain a carbon fiber preform;
[0018] Then, the carbon fiber preform is deposited at 1000-1200° C. for 200-600 hours by chemical vapor infiltration with natural gas as a gas source to obtain a carbon / carbon composite material preform.
[0019] It should be noted that the carbon / carbon composite material preform described in the embodiment of the present invention is a hollow circular ring structure; the grooves (upper surface grooves, lower surface grooves) are opened along the circumference of the circular ring; the depth of the grooves (upper surface grooves, lower surface grooves) is 2 mm, the distance from the inner edge of the grooves (upper surface grooves, lower surface grooves) to the inner edge of the carbon / carbon composite material preform is 5 mm, and the distance from the outer edge of the grooves (upper surface grooves, lower surface grooves) to the outer edge of the carbon / carbon composite material preform is 5 mm.
[0020] In some embodiments, the vacuum treatment is performed at a pressure of 5-6 Pa and for a time of 1-1.3 h.
[0021] In some embodiments, the carbonization treatment is carried out at a temperature of 900-1000°C, for a time of 3-4 hours, and at a heating rate of 1-5°C / min.
[0022] In some embodiments, the high temperature ceramic treatment is carried out at a temperature of 1450-1700° C., for a time of 1-2 h, and at a heating rate of 1-5° C. / min.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) The coating material provided by the present invention can make the components interact with each other and form a dispersed, uniform and stable composite phase system through the compounding of silicon carbide, carbon black, polyvinyl alcohol and glycerol, effectively overcoming the uneven distribution of different phases on the surface of the carbon ceramic brake disc, thereby effectively alleviating the problem of large fluctuations in the friction coefficient of the friction pair, and the coating material has good wear resistance and can extend its service life. In addition, when preparing the coating material, the present invention uses non-toxic, harmless, environmentally friendly and easily degradable polyvinyl alcohol to prepare a water-based slurry to replace the currently commonly used organic slurries such as phenolic resin and furan resin, and the cost of the water-based slurry is also reduced compared to the ethanol resin slurry.
[0025] (2) The coating material provided by the present invention removes bubbles in the coating material by applying the coating material in combination with vacuum treatment, so that the coating material can form a prefabricated coating by a single coating, thus overcoming the problem that the existing slurry method preparation process inevitably requires repeated coating to form a prefabricated coating of the required thickness. In addition, the coating thickness can be controlled by adjusting the amount of the coating material, the preparation process is simple, and large-scale industrial production can be easily realized.
[0026] (3) The present invention provides a carbon-ceramic brake disc with a wear-resistant coating formed by a single-shot molding of a coating material. The carbon-ceramic brake disc has excellent friction performance. After testing, the friction coefficient of the wear-resistant coating brake disc is 0.44, the wear amount is 0.0005 mm, and the peak value extreme difference of the instantaneous friction coefficient during a single braking process is stable within 0.1, and has good friction stability. This shows that the carbon-ceramic brake disc prepared by the present invention has a higher friction coefficient and a lower wear rate, and can effectively extend the service life of the carbon-ceramic brake disc. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0028] Figure 1 This is a SEM spectrum of the surface micromorphology of the coated carbon-ceramic brake disc prepared in Example 2.
[0029] Figure 2 This is a SEM spectrum of the surface micromorphology of the coated carbon-ceramic brake disc prepared in Comparative Example 4.
[0030] Figure 3 This is a SEM spectrum of the surface micromorphology of the coated carbon-ceramic brake disc prepared in Comparative Example 5.
[0031] Figure 4 This is a braking curve diagram of 6 braking times of the coated carbon-ceramic brake disc prepared in Example 2. DETAILED DESCRIPTION
[0032] The present invention is described in detail below in conjunction with the accompanying drawings and specific examples, but should not be construed as limiting the present invention. Unless otherwise specified, the technical means used in the following examples are conventional means well known to those skilled in the art, and the raw materials, components, etc. used in the following examples, unless otherwise specified, can be obtained from commercial sources.
[0033] It should be noted that the specific preparation scheme of the carbon-ceramic brake disc is not particularly limited by those skilled in the art, and can be implemented in combination with the preparation methods known in the art. For example, a preparation method of a carbon-ceramic brake disc with a single-molded wear-resistant coating provided by the present invention comprises the following steps:
[0034] Step 1: Preparation of carbon / carbon composite material preform:
[0035] The carbon fiber mat and the carbon fiber free weft fabric are alternately layered in a stacking manner of carbon fiber mat layer / 0° carbon fiber free weft fabric layer / carbon fiber mat layer / 90° carbon fiber free weft fabric layer, and then needle-punched with a needle with barbed edges in a direction perpendicular to the stacking layer to obtain a carbon fiber preform;
[0036] The carbon fiber preform is deposited at 1000-1200° C. for 200-600 hours using chemical vapor infiltration (CVI) with natural gas as the gas source to obtain a carbon / carbon composite material preform;
[0037] The density of the carbon fiber mesh is 0.1-0.4 g / cm 3The density of the carbon fiber non-woven fabric is 0.4-0.8g / cm 3 .
[0038] Step 2: Machining:
[0039] The carbon / carbon composite material preform is machined, and grooves (upper surface grooves and lower surface grooves) are respectively formed on the upper and lower surfaces of the carbon / carbon composite material preform, and then the preform is cleaned by an ultrasonic cleaner for 1-2 hours and then dried in an oven at 150° C. for 2-4 hours to obtain a carbon / carbon preformed disc;
[0040] The carbon / carbon composite material preform is a hollow circular ring structure; the grooves (upper surface grooves, lower surface grooves) are opened along the circumference of the circular ring; the depth of the grooves (upper surface grooves, lower surface grooves) is 2 mm, the distance from the inner edge of the grooves (upper surface grooves, lower surface grooves) to the inner edge of the carbon / carbon composite material preform is 5 mm, and the distance from the outer edge of the grooves (upper surface grooves, lower surface grooves) to the outer edge of the carbon / carbon composite material preform is 5 mm.
[0041] Step 3: Preparation of coating slurry:
[0042] In terms of weight percentage, the coating slurry is composed of 20-40wt% of silicon carbide powder (SiC powder) with a particle size of 20 μm, 10-20wt% of carbon black powder, 5-15wt% of polyvinyl alcohol, 5-10wt% of glycerol, and 25-60wt% of distilled water;
[0043] Preparation process of coating slurry: Mix polyvinyl alcohol and distilled water evenly and heat to 90°C to completely dissolve the polyvinyl alcohol to obtain a polyvinyl alcohol solution, and let it stand to cool to room temperature; add silicon carbide powder and carbon black powder in sequence to the polyvinyl alcohol solution cooled to room temperature, and stir continuously for 1-2 hours to make the components evenly distributed to obtain a slurry; then add glycerol to the slurry and stir continuously for 1-2 hours to obtain a coating slurry.
[0044] Step 4: Single application of coating slurry:
[0045] The upper surface grooves of the carbon / carbon preformed disk are filled with a single coating slurry. After filling, it is placed under vacuum conditions with a pressure of 5-6Pa for 1-1.3h to discharge the bubbles inside the coating slurry. It is then placed in an oven at 80°C. After drying, the carbon / carbon preformed disk is turned over. The lower surface grooves are then filled with a single coating in the same way and dried to obtain a carbon / carbon preformed disk with a single molded prefabricated coating.
[0046] Step 5: Carbonization treatment:
[0047] The single-molded pre-coated carbon / carbon preformed disc is placed in an inert gas, heated to 900-1000°C at a heating rate of 1-5°C / min for carbonization treatment for 3-4 hours (the carbonization treatment is to convert the organic components in the carbon / carbon preformed disc into pyrolytic carbon), and a carbon / carbon preformed disc after carbonization treatment is obtained.
[0048] Step 6: High temperature ceramic treatment:
[0049] The carbonized carbon / carbon prefabricated disc is embedded in silicon powder and then placed in a graphite crucible. The graphite crucible is sent into a vacuum sintering furnace (the pressure in the vacuum sintering furnace is 100 Pa) by high-temperature siliconization. The temperature is raised to 1450-1700°C at a heating rate of 1-5°C / min for high-temperature ceramicization treatment for 1-2h (the high-temperature ceramicization treatment is to make the silicon powder "embedded in the silicon powder" melt into liquid silicon, i.e. molten silicon, after reaching the melting point, and then the molten silicon infiltrates into the pores in the carbon / carbon prefabricated disc to form a dense ceramic), so as to obtain a carbon-ceramic brake disc with a single-molded wear-resistant coating.
[0050] The technical solution of the present invention will be further described below in conjunction with specific embodiments.
[0051] Embodiment 1: A method for preparing a carbon-ceramic brake disc with a single-molded wear-resistant coating, comprising the following steps:
[0052] Step 1: Preparation of carbon / carbon composite material preform:
[0053] The carbon fiber mat and the carbon fiber free weft fabric are alternately layered in a stacking manner of carbon fiber mat layer / 0° carbon fiber free weft fabric layer / carbon fiber mat layer / 90° carbon fiber free weft fabric layer, and then acupuncture is performed with a needle with barbed edges in a direction perpendicular to the stacking direction to obtain a carbon fiber preform;
[0054] The carbon fiber preform was deposited at 1000°C for 600h using natural gas as the gas source to obtain a carbon / carbon composite material preform.
[0055] The density of the carbon fiber mesh is 0.1 g / cm 3 The density of the carbon fiber non-woven fabric is 0.4 g / cm 3 .
[0056] Step 2: Machining:
[0057] The carbon / carbon composite material preform is machined, and grooves (upper surface grooves and lower surface grooves) are formed on the upper and lower surfaces of the carbon / carbon composite material preform, and then the preform is cleaned by an ultrasonic cleaner for 1 hour and then dried in an oven at 150° C. for 2 hours to obtain a carbon / carbon preformed disk;
[0058] The carbon / carbon composite material preform is a hollow circular ring structure; the grooves (upper surface grooves, lower surface grooves) are opened along the circumference of the circular ring; the depth of the grooves (upper surface grooves, lower surface grooves) is 2 mm, the distance from the inner edge of the grooves (upper surface grooves, lower surface grooves) to the inner edge of the carbon / carbon composite material preform is 5 mm, and the distance from the outer edge of the grooves (upper surface grooves, lower surface grooves) to the outer edge of the carbon / carbon composite material preform is 5 mm.
[0059] Step 3: Preparation of coating slurry:
[0060] In terms of weight percentage, the coating slurry consists of 20wt% silicon carbide powder (SiC powder) with a particle size of 20 μm, 10wt% carbon black powder, 5wt% polyvinyl alcohol, 5wt% glycerol, and 60wt% distilled water;
[0061] 5 wt% polyvinyl alcohol and 60 wt% distilled water were mixed evenly and heated to 90°C to completely dissolve the polyvinyl alcohol to obtain a polyvinyl alcohol solution, which was allowed to stand and cool to room temperature; 20 wt% silicon carbide powder with a particle size of 20 μm and 10 wt% carbon black powder were added to the polyvinyl alcohol solution in sequence, and the mixture was stirred continuously for 1 hour to obtain a slurry so that the components were evenly distributed; then 5 wt% glycerol was added to the slurry and stirred continuously for 1 hour to obtain a coating slurry;
[0062] Step 4: Single application of coating slurry:
[0063] The upper surface grooves of the carbon / carbon preformed disk are filled with a single coating slurry. After filling, it is placed under a vacuum condition with a pressure of 5 Pa for 1 hour to discharge the bubbles inside the coating slurry. It is then placed in an oven at 80°C. After drying, the carbon-carbon preformed disk is turned over, and the lower surface grooves are filled with a single coating and dried in the same way to obtain a carbon / carbon preformed disk with a single molding prefabricated coating.
[0064] Step 5: Carbonization treatment:
[0065] The single-molded pre-coated carbon / carbon preformed disk is placed in an inert gas and heated to 1000°C at a heating rate of 5°C / min for carbonization treatment for 3 hours (the carbonization treatment is to convert the organic components in the carbon / carbon preformed disk into pyrolytic carbon) to obtain a carbon / carbon preformed disk after carbonization treatment.
[0066] Step 6: High temperature ceramic treatment:
[0067] The carbon / carbon prefabricated disc after carbonization treatment is embedded in silicon powder, and then placed in a graphite crucible. The graphite crucible is sent into a vacuum sintering furnace (the pressure in the vacuum sintering furnace is 100 Pa) by high-temperature silicon infiltration. The temperature is raised to 1450°C at a heating rate of 1°C / min for high-temperature ceramic treatment for 2 hours (the high-temperature ceramic treatment is to make the silicon powder "embedded in the silicon powder" melt into liquid silicon, i.e. molten silicon, after reaching the melting point, and then the molten silicon infiltrates into the pores in the carbon / carbon prefabricated disc to form a dense ceramic), thereby obtaining a carbon-ceramic brake disc with a single-molded wear-resistant coating.
[0068] Embodiment 2: A method for preparing a carbon-ceramic brake disc with a single-molded wear-resistant coating, comprising the following steps:
[0069] Step 1: Preparation of carbon / carbon composite material preform:
[0070] The carbon fiber mat and the carbon fiber free weft fabric are alternately layered in a stacking manner of carbon fiber mat layer / 0° carbon fiber free weft fabric layer / carbon fiber mat layer / 90° carbon fiber free weft fabric layer, and then acupuncture is performed with a needle with barbed edges in a direction perpendicular to the stacking direction to obtain a carbon fiber preform;
[0071] The carbon fiber preform was deposited at 1200°C for 200h using natural gas as the gas source to obtain a carbon / carbon composite material preform.
[0072] The density of the carbon fiber mesh is 0.1 g / cm 3 The density of the carbon fiber non-woven fabric is 0.4 g / cm 3 .
[0073] Step 2: Machining:
[0074] The carbon / carbon composite material preform is machined, and grooves (upper surface grooves and lower surface grooves) are formed on the upper and lower surfaces of the carbon / carbon composite material preform, and then the preform is cleaned by an ultrasonic cleaner for 2 hours and then dried in an oven at 150° C. for 4 hours to obtain a carbon / carbon preformed disk;
[0075] The carbon / carbon composite material preform is a hollow circular ring structure; the grooves (upper surface grooves, lower surface grooves) are opened along the circumference of the circular ring; the depth of the grooves (upper surface grooves, lower surface grooves) is 2 mm, the distance from the inner edge of the grooves (upper surface grooves, lower surface grooves) to the inner edge of the carbon / carbon composite material preform is 5 mm, and the distance from the outer edge of the grooves (upper surface grooves, lower surface grooves) to the outer edge of the carbon / carbon composite material preform is 5 mm.
[0076] Step 3: Preparation of coating slurry:
[0077] In terms of weight percentage, the coating slurry consists of 30wt% of silicon carbide powder (SiC powder) with a particle size of 20 μm, 15wt% of carbon black powder, 10wt% of polyvinyl alcohol, 5wt% of glycerol, and 40wt% of distilled water;
[0078] 10wt% polyvinyl alcohol and 40wt% distilled water were mixed evenly and heated to 90°C to completely dissolve the polyvinyl alcohol to obtain a polyvinyl alcohol solution, which was allowed to stand and cool to room temperature; 30wt% silicon carbide powder with a particle size of 20μm and 15wt% carbon black powder were added to the polyvinyl alcohol solution in sequence, and the mixture was stirred continuously for 2h to uniformly distribute the components to obtain a slurry; then 5wt% glycerol was added to the slurry and stirred continuously for 2h to obtain a coating slurry.
[0079] Step 4: Single application of coating slurry:
[0080] The upper surface grooves of the carbon / carbon preformed disk are filled with a single coating slurry. After filling, it is placed under vacuum conditions with a pressure of 6 Pa for 1.2 hours to expel the bubbles inside the coating slurry. It is then placed in an oven at 80°C. After drying, the carbon / carbon preformed disk is turned over, and the lower surface grooves are filled with a single coating in the same way and dried to obtain a carbon / carbon preformed disk with a single molding prefabricated coating.
[0081] Step 5: Carbonization treatment:
[0082] The single-molded pre-coated carbon / carbon preformed disk is placed in an inert gas, heated to 900°C at a heating rate of 1°C / min for carbonization treatment for 4 hours (the carbonization treatment is to convert the organic components in the carbon / carbon preformed disk into pyrolytic carbon), and a carbon / carbon preformed disk after carbonization is obtained.
[0083] Step 6: High temperature ceramic treatment:
[0084] The carbon / carbon prefabricated disc body after carbonization treatment is embedded in silicon powder, and then placed in a graphite crucible. The graphite crucible is sent into a vacuum sintering furnace (the pressure in the vacuum sintering furnace is 100 Pa) by high-temperature silicon infiltration. The temperature is raised to 1700°C at a heating rate of 5°C / min for high-temperature ceramic treatment for 1 hour (the high-temperature ceramic treatment is to make the silicon powder "embedded in the silicon powder" melt into liquid silicon, i.e. molten silicon, after reaching the melting point, and then the molten silicon infiltrates into the pores in the carbon / carbon prefabricated disc body to form a dense ceramic), so as to obtain a carbon-ceramic brake disc with a single-molded wear-resistant coating.
[0085] Embodiment 3: A method for preparing a carbon-ceramic brake disc with a single-molded wear-resistant coating, comprising the following steps:
[0086] Step 1: Preparation of carbon / carbon composite material preform:
[0087] The carbon fiber mat and the carbon fiber free weft fabric are alternately layered in a stacking manner of carbon fiber mat layer / 0° carbon fiber free weft fabric layer / carbon fiber mat layer / 90° carbon fiber free weft fabric layer, and then acupuncture is performed with a needle with barbed edges in a direction perpendicular to the stacking direction to obtain a carbon fiber preform;
[0088] The carbon fiber preform was deposited at 1200°C for 600h using natural gas as the gas source to obtain a carbon / carbon composite material preform.
[0089] The density of the carbon fiber mesh is 0.4g / cm 3 The density of the carbon fiber non-woven fabric is 0.8 g / cm 3 .
[0090] Step 2: Machining:
[0091] The carbon / carbon composite material preform is machined, and grooves (upper surface grooves and lower surface grooves) are formed on the upper and lower surfaces of the carbon / carbon composite material preform, and then the preform is cleaned by an ultrasonic cleaner for 2 hours and then dried in an oven at 150° C. for 4 hours to obtain a carbon / carbon preformed disk;
[0092] The carbon / carbon composite material preform is a hollow circular ring structure; the grooves (upper surface grooves, lower surface grooves) are opened along the circumference of the circular ring; the depth of the grooves (upper surface grooves, lower surface grooves) is 2 mm, the distance from the inner edge of the grooves (upper surface grooves, lower surface grooves) to the inner edge of the carbon / carbon composite material preform is 5 mm, and the distance from the outer edge of the grooves (upper surface grooves, lower surface grooves) to the outer edge of the carbon / carbon composite material preform is 5 mm.
[0093] Step 3: Preparation of coating slurry:
[0094] In terms of weight percentage, the coating slurry consists of 40wt% of silicon carbide powder (SiC powder) with a particle size of 20 μm, 20wt% of carbon black powder, 5wt% of polyvinyl alcohol, 10wt% of glycerol, and 25wt% of distilled water;
[0095] 5 wt% polyvinyl alcohol and 25 wt% distilled water were mixed evenly and heated to 90°C to completely dissolve the polyvinyl alcohol to obtain a polyvinyl alcohol solution, which was allowed to stand and cool to room temperature; 40 wt% silicon carbide powder with a particle size of 20 μm and 20 wt% carbon black powder were added to the polyvinyl alcohol solution in sequence, and stirred continuously for 2 hours to make the components evenly distributed to obtain a slurry; then 10 wt% glycerol was added to the slurry and stirred continuously for 2 hours to obtain a coating slurry;
[0096] Step 4: Single application of coating slurry:
[0097] The upper surface grooves of the carbon / carbon preformed disk are filled with a single coating slurry. After filling, it is placed under vacuum conditions with a pressure of 6 Pa for 1.3 hours to discharge the bubbles inside the coating slurry. It is then placed in an oven at 80°C. After drying, the carbon / carbon preformed disk is turned over, and the lower surface grooves are filled with a single coating and dried in the same way to obtain a carbon / carbon preformed disk with a single molding prefabricated coating.
[0098] Step 5: Carbonization treatment:
[0099] The single-molded pre-coated carbon / carbon preformed disk is placed in an inert gas and heated to 900°C at a heating rate of 3°C / min for carbonization treatment for 4 hours (the carbonization treatment is to convert the organic components in the carbon / carbon preformed disk into pyrolytic carbon) to obtain a carbon / carbon preformed disk after carbonization treatment.
[0100] Step 6: High temperature ceramic treatment:
[0101] The carbon / carbon prefabricated disc after carbonization treatment is embedded in silicon powder, and then placed in a graphite crucible. The graphite crucible is sent into a vacuum sintering furnace (the pressure in the vacuum sintering furnace is 100 Pa) by high-temperature siliconization. The temperature is raised to 1600°C at a heating rate of 5°C / min for high-temperature ceramic treatment for 1 hour (the high-temperature ceramic treatment is to make the silicon powder "embedded in the silicon powder" melt into liquid silicon, i.e. molten silicon, after reaching the melting point, and then the molten silicon infiltrates into the pores in the carbon / carbon prefabricated disc to form a dense ceramic), so as to obtain a carbon-ceramic brake disc with a single-molded wear-resistant coating.
[0102] Comparative Example 1: A method for preparing a carbon-ceramic brake disc with a single-molded wear-resistant coating, comprising the following steps:
[0103] The carbon fiber mat and the carbon fiber free weft fabric are alternately layered in a stacking manner of carbon fiber mat layer / 0° carbon fiber free weft fabric layer / carbon fiber mat layer / 90° carbon fiber free weft fabric layer, and then acupuncture is performed with a needle with barbed edges in a direction perpendicular to the stacking direction to obtain a carbon fiber preform;
[0104] The carbon fiber preform was deposited at 1200°C for 200h using natural gas as the gas source to obtain a carbon / carbon composite material preform.
[0105] The density of the carbon fiber mesh is 0.1 g / cm 3 The density of the carbon fiber non-woven fabric is 0.4 g / cm 3 .
[0106] Step 2: Machining:
[0107] The carbon / carbon composite material preform is machined, and grooves (upper surface grooves and lower surface grooves) are formed on the upper and lower surfaces of the carbon / carbon composite material preform, and then the preform is cleaned by an ultrasonic cleaner for 2 hours and then dried in an oven at 150° C. for 4 hours to obtain a carbon / carbon preformed disk;
[0108] The carbon / carbon composite material preform is a hollow circular ring structure; the grooves (upper surface grooves, lower surface grooves) are opened along the circumference of the circular ring; the depth of the grooves (upper surface grooves, lower surface grooves) is 2 mm, the distance from the inner edge of the grooves (upper surface grooves, lower surface grooves) to the inner edge of the carbon / carbon composite material preform is 5 mm, and the distance from the outer edge of the grooves (upper surface grooves, lower surface grooves) to the outer edge of the carbon / carbon composite material preform is 5 mm.
[0109] Step 3: Preparation of slurry:
[0110] In terms of weight percentage, the coating slurry consists of 30wt% of silicon carbide powder (SiC powder) with a particle size of 20 μm, 20wt% of carbon black powder, 10wt% of glycerol, and 40wt% of distilled water;
[0111] To 40wt% distilled water, 30wt% silicon carbide powder with a particle size of 20μm and 20wt% carbon black powder were added in sequence and stirred continuously for 2h to make the components evenly distributed to obtain a slurry; then 10wt% glycerol was added to the slurry and stirred continuously for 2h to obtain a slurry.
[0112] When polyvinyl alcohol is not added, different powder particles are completely separated after the slurry is dried due to the lack of polyvinyl alcohol (binder), and cannot form a good bond with the carbon / carbon prefabricated disc body, that is, the slurry cannot be used for single coating to fill the upper and lower surface grooves to form a coating. Therefore, it is impossible to prepare a carbon-ceramic brake disc with a single-molded wear-resistant coating, and therefore, the subsequent single-coating coating slurry, carbonization treatment and high-temperature ceramic treatment steps are not performed.
[0113] Comparative Example 2: A method for preparing a carbon-ceramic brake disc with a single-molded wear-resistant coating, comprising the following steps:
[0114] Step 1: Preparation of carbon / carbon composite material preform:
[0115] The carbon fiber mat and the carbon fiber free weft fabric are alternately layered in a stacking manner of carbon fiber mat layer / 0° carbon fiber free weft fabric layer / carbon fiber mat layer / 90° carbon fiber free weft fabric layer, and then acupuncture is performed with a needle with barbed edges in a direction perpendicular to the stacking direction to obtain a carbon fiber preform;
[0116] The carbon fiber preform was deposited at 1200°C for 200h using natural gas as the gas source to obtain a carbon / carbon composite material preform.
[0117] The density of the carbon fiber mesh is 0.1 g / cm 3 The density of the carbon fiber non-woven fabric is 0.4 g / cm 3 .
[0118] Step 2: Machining:
[0119] The carbon / carbon composite material preform is machined, and grooves (upper surface grooves and lower surface grooves) are formed on the upper and lower surfaces of the carbon / carbon composite material preform, and then the preform is cleaned by an ultrasonic cleaner for 2 hours and then dried in an oven at 150° C. for 4 hours to obtain a carbon / carbon preformed disk;
[0120] The carbon / carbon composite material preform is a hollow circular ring structure; the grooves (upper surface grooves, lower surface grooves) are opened along the circumference of the circular ring; the depth of the grooves (upper surface grooves, lower surface grooves) is 2 mm, the distance from the inner edge of the grooves (upper surface grooves, lower surface grooves) to the inner edge of the carbon / carbon composite material preform is 5 mm, and the distance from the outer edge of the grooves (upper surface grooves, lower surface grooves) to the outer edge of the carbon / carbon composite material preform is 5 mm.
[0121] Step 3: Preparation of coating slurry:
[0122] In terms of weight percentage, the coating slurry consists of 30wt% of silicon carbide powder (SiC powder) with a particle size of 20 μm, 20wt% of carbon black powder, 10wt% of polyvinyl alcohol, and 40wt% of distilled water;
[0123] 10wt% polyvinyl alcohol and 40wt% distilled water were evenly mixed and heated to 90°C to completely dissolve the polyvinyl alcohol to obtain a polyvinyl alcohol solution, which was allowed to stand and cool to room temperature; 30wt% silicon carbide powder with a particle size of 20μm and 20wt% carbon black powder were successively added to the polyvinyl alcohol solution, and stirred continuously for 2h to evenly distribute the components to obtain a coating slurry.
[0124] Step 4: Single application of coating slurry:
[0125] The upper surface groove of the carbon / carbon prefabricated disc is filled with a coating slurry for a single coating, and then placed in an oven at 80° C., and after drying, the carbon / carbon prefabricated disc is turned over, and the lower surface groove is filled with a single coating in the same manner and dried, to obtain a carbon / carbon prefabricated disc with a single molding prefabricated coating;
[0126] When glycerol was not added, continuous through cracks appeared in the prefabricated coating on the carbon / carbon prefabricated disc body, so the carbon / carbon prefabricated disc body could not be used to prepare a carbon-ceramic brake disc with a single-molded wear-resistant coating. Therefore, the subsequent carbonization treatment and high-temperature ceramic treatment steps were not performed.
[0127] Comparative Example 3: A method for preparing a carbon-ceramic brake disc with a single-molded wear-resistant coating, comprising the following steps:
[0128] The carbon fiber mat and the carbon fiber free weft fabric are alternately layered in a stacking manner of carbon fiber mat layer / 0° carbon fiber free weft fabric layer / carbon fiber mat layer / 90° carbon fiber free weft fabric layer, and then acupuncture is performed with a needle with barbed edges in a direction perpendicular to the stacking direction to obtain a carbon fiber preform;
[0129] The carbon fiber preform was deposited at 1200°C for 200h using natural gas as the gas source to obtain a carbon / carbon composite material preform.
[0130] The density of the carbon fiber mesh is 0.1 g / cm 3 The density of the carbon fiber non-woven fabric is 0.4 g / cm 3 .
[0131] Step 2: Machining:
[0132] The carbon / carbon composite material preform is machined, and grooves (upper surface grooves and lower surface grooves) are formed on the upper and lower surfaces of the carbon / carbon composite material preform, and then the preform is cleaned by an ultrasonic cleaner for 2 hours and then dried in an oven at 150° C. for 4 hours to obtain a carbon / carbon preformed disk;
[0133] The carbon / carbon composite material preform is a hollow circular ring structure; the grooves (upper surface grooves, lower surface grooves) are opened along the circumference of the circular ring; the depth of the grooves (upper surface grooves, lower surface grooves) is 2 mm, the distance from the inner edge of the grooves (upper surface grooves, lower surface grooves) to the inner edge of the carbon / carbon composite material preform is 5 mm, and the distance from the outer edge of the grooves (upper surface grooves, lower surface grooves) to the outer edge of the carbon / carbon composite material preform is 5 mm.
[0134] Step 3: Preparation of slurry:
[0135] In terms of weight percentage, the coating slurry consists of 30wt% of silicon carbide powder (SiC powder) with a particle size of 20 μm, 20wt% of carbon black powder, and 50wt% of distilled water;
[0136] To 50 wt % of distilled water, 30 wt % of silicon carbide powder with a particle size of 20 μm and 20 wt % of carbon black powder were added in sequence and stirred continuously for 2 h to make a slurry with uniform distribution of each component.
[0137] When polyvinyl alcohol and glycerol are not added, the slurry cannot adhere to the upper and lower surface grooves of the carbon / carbon prefabricated disc after drying, that is, the slurry cannot be used for single coating filling to form a coating. Therefore, it is impossible to prepare a carbon-ceramic brake disc with a single-molded wear-resistant coating, and therefore, the subsequent single-coating coating slurry, carbonization treatment and high-temperature ceramic treatment steps are not performed.
[0138] Comparative Example 4: A method for preparing a carbon-ceramic brake disc, comprising the following steps:
[0139] The carbon fiber mat and the carbon fiber free weft fabric are alternately layered in a stacking manner of carbon fiber mat layer / 0° carbon fiber free weft fabric layer / carbon fiber mat layer / 90° carbon fiber free weft fabric layer, and then acupuncture is performed with a needle with barbed edges in a direction perpendicular to the stacking direction to obtain a carbon fiber preform;
[0140] The carbon fiber preform was deposited at 1200°C for 200h using natural gas as the gas source to obtain a carbon / carbon composite material preform.
[0141] The density of the carbon fiber mesh is 0.1 g / cm 3 The density of the carbon fiber non-woven fabric is 0.4 g / cm 3 .
[0142] Step 2: Machining:
[0143] The carbon / carbon composite material preform is machined, and grooves (upper surface grooves and lower surface grooves) are formed on the upper and lower surfaces of the carbon / carbon composite material preform, and then the preform is cleaned by an ultrasonic cleaner for 2 hours and then dried in an oven at 150° C. for 4 hours to obtain a carbon / carbon preformed disk;
[0144] The carbon / carbon composite material preform is a hollow circular ring structure; the grooves (upper surface grooves, lower surface grooves) are opened along the circumference of the circular ring; the depth of the grooves (upper surface grooves, lower surface grooves) is 2 mm, the distance from the inner edge of the grooves (upper surface grooves, lower surface grooves) to the inner edge of the carbon / carbon composite material preform is 5 mm, and the distance from the outer edge of the grooves (upper surface grooves, lower surface grooves) to the outer edge of the carbon / carbon composite material preform is 5 mm.
[0145] Step 3: Preparation of coating slurry:
[0146] In terms of weight percentage, the coating slurry consists of 30wt% of silicon carbide powder (SiC powder) with a particle size of 50 μm, 15wt% of carbon black powder, 10wt% of polyvinyl alcohol, 5wt% of glycerol, and 40wt% of distilled water;
[0147] 10wt% polyvinyl alcohol and 40wt% distilled water were mixed evenly and heated to 90°C to completely dissolve the polyvinyl alcohol to obtain a polyvinyl alcohol solution, which was allowed to stand and cool to room temperature; 30wt% silicon carbide powder with a particle size of 50μm and 15wt% carbon black powder were added to the polyvinyl alcohol solution in sequence, and the mixture was stirred continuously for 2h to uniformly distribute the components to obtain a slurry; then 5wt% glycerol was added to the slurry and stirred continuously for 2h to obtain a coating slurry.
[0148] Step 4: Single application of coating slurry:
[0149] The upper surface grooves of the carbon / carbon preformed disk are filled with a single coating slurry. After filling, it is placed under a vacuum condition with a pressure of 6 Pa for 1.2 hours to discharge the bubbles inside the coating slurry. It is then placed in an oven at 80°C. After drying, the carbon / carbon preformed disk is turned over, and the lower surface grooves are filled with a single coating and dried in the same way to obtain a carbon / carbon preformed disk with a single-molded prefabricated coating.
[0150] Step 5: Carbonization treatment:
[0151] The single-molded pre-coated carbon / carbon preformed disk is placed in an inert gas, heated to 900°C at a heating rate of 1°C / min for carbonization treatment for 4 hours (the carbonization treatment is to convert the organic components in the carbon / carbon preformed disk into pyrolytic carbon), and a carbon / carbon preformed disk after carbonization is obtained.
[0152] Step 6: High temperature ceramic treatment:
[0153] The carbon / carbon prefabricated disc body after carbonization treatment is embedded in silicon powder, and then placed in a graphite crucible. The graphite crucible is sent into a vacuum sintering furnace (the pressure in the vacuum sintering furnace is 100 Pa) by high-temperature silicon infiltration. The temperature is raised to 1700°C at a heating rate of 5°C / min for high-temperature ceramic treatment for 1 hour (the high-temperature ceramic treatment is to make the silicon powder "embedded in the silicon powder" melt into liquid silicon, i.e. molten silicon, after reaching the melting point, and then the molten silicon infiltrates into the pores in the carbon / carbon prefabricated disc body to form a dense ceramic), so as to obtain a carbon-ceramic brake disc with a single-molded wear-resistant coating.
[0154] Comparative Example 5: A method for preparing a carbon-ceramic brake disc with a single-molded wear-resistant coating, comprising the following steps:
[0155] The carbon fiber mat and the carbon fiber free weft fabric are alternately layered in a stacking manner of carbon fiber mat layer / 0° carbon fiber free weft fabric layer / carbon fiber mat layer / 90° carbon fiber free weft fabric layer, and then acupuncture is performed with a needle with barbed edges in a direction perpendicular to the stacking direction to obtain a carbon fiber preform;
[0156] The carbon fiber preform was deposited at 1200°C for 200h using natural gas as the gas source to obtain a carbon / carbon composite material preform.
[0157] The density of the carbon fiber mesh is 0.1 g / cm 3 The density of the carbon fiber non-woven fabric is 0.4 g / cm 3 .
[0158] Step 2: Machining:
[0159] The carbon / carbon composite material preform is machined, and grooves (upper surface grooves and lower surface grooves) are formed on the upper and lower surfaces of the carbon / carbon composite material preform, and then the preform is cleaned by an ultrasonic cleaner for 2 hours and then dried in an oven at 150° C. for 4 hours to obtain a carbon / carbon preformed disk;
[0160] The carbon / carbon composite material preform is a hollow circular ring structure; the grooves (upper surface grooves, lower surface grooves) are opened along the circumference of the circular ring; the depth of the grooves (upper surface grooves, lower surface grooves) is 2 mm, the distance from the inner edge of the grooves (upper surface grooves, lower surface grooves) to the inner edge of the carbon / carbon composite material preform is 5 mm, and the distance from the outer edge of the grooves (upper surface grooves, lower surface grooves) to the outer edge of the carbon / carbon composite material preform is 5 mm.
[0161] Step 3: Preparation of coating slurry:
[0162] In terms of weight percentage, the coating slurry consists of 15wt% of silicon carbide powder with a particle size of 20μm, 10wt% of silicon carbide powder with a particle size of 50μm, 15wt% of carbon black powder, 10wt% of polyvinyl alcohol, 5wt% of glycerol, and 40wt% of distilled water;
[0163] 10wt% polyvinyl alcohol and 40wt% distilled water were mixed evenly and heated to 90°C to completely dissolve the polyvinyl alcohol to obtain a polyvinyl alcohol solution, and the mixture was allowed to stand and cool to room temperature; 15wt% silicon carbide powder with a particle size of 20μm, 10wt% silicon carbide powder with a particle size of 50μm, and 15wt% carbon black powder were added to the polyvinyl alcohol solution in sequence, and the mixture was stirred continuously for 2h to uniformly distribute the components to obtain a slurry; 5wt% glycerol was then added to the slurry and stirred continuously for 2h to obtain a coating slurry.
[0164] Step 4: Single application of coating slurry:
[0165] The upper surface grooves of the carbon / carbon preformed disk are filled with a single coating slurry. After filling, it is placed under a vacuum condition with a pressure of 6 Pa for 1.2 hours to discharge the bubbles inside the coating slurry. It is then placed in an oven at 80°C. After drying, the carbon / carbon preformed disk is turned over, and the lower surface grooves are filled with a single coating and dried in the same way to obtain a carbon / carbon preformed disk with a single-molded prefabricated coating.
[0166] Step 5: Carbonization treatment:
[0167] The single-molded pre-coated carbon / carbon preformed disk is placed in an inert gas, heated to 900°C at a heating rate of 5°C / min for carbonization treatment for 4 hours (the carbonization treatment is to convert the organic components in the carbon / carbon preformed disk into pyrolytic carbon), and a carbon / carbon preformed disk after carbonization is obtained.
[0168] Step 6: High temperature ceramic treatment:
[0169] The carbon / carbon prefabricated disc body after carbonization treatment is embedded in silicon powder, and then placed in a graphite crucible. The graphite crucible is sent into a vacuum sintering furnace (the pressure in the vacuum sintering furnace is 100 Pa) by high-temperature silicon infiltration. The temperature is raised to 1700°C at a heating rate of 5°C / min for high-temperature ceramic treatment for 1 hour (the high-temperature ceramic treatment is to make the silicon powder "embedded in the silicon powder" melt into liquid silicon, i.e. molten silicon, after reaching the melting point, and then the molten silicon infiltrates into the pores in the carbon / carbon prefabricated disc body to form a dense ceramic), so as to obtain a carbon-ceramic brake disc with a single-molded wear-resistant coating.
[0170] Test Example 1: Scanning electron microscope (SEM) test.
[0171] The invention is described with reference to Example 2 and Comparative Examples 4-5.
[0172] The carbon-ceramic brake discs prepared in Example 2 and Comparative Examples 4-5 were subjected to SEM tests to observe their surface morphologies.
[0173] The SEM test results of the carbon ceramic brake disc prepared in Example 2 are as follows: Figure 1 As shown. Figure 1 It can be seen that the coating surface of the carbon ceramic brake disc is mainly composed of Si and SiC phases, of which the light gray is the Si phase and the dark gray is the SiC phase. The two phases are evenly distributed, and the coating surface is dense and defect-free. The dark gray SiC phase exists in two forms: one is the silicon carbide powder with a particle size of 20μm introduced by the coating slurry itself; the other is the SiC particles generated by the complete reaction of the pyrolytic carbon generated during the carbonization process and the molten silicon generated during the high-temperature ceramicization process.
[0174] The SEM test results of the carbon ceramic brake disc prepared in Comparative Example 4 are as follows: Figure 2 As shown. Figure 2 It can be seen that the overall structure of the prepared wear-resistant coating is similar to that of Example 2, the Si and SiC phases are evenly distributed, the particle size of SiC is 50 μm, and SiC particles generated by the reaction also exist.
[0175] The SEM test results of the carbon ceramic brake disc prepared in Comparative Example 5 are as follows: Figure 3 As shown. Figure 3 It can be seen that the overall structure of the prepared wear-resistant coating is similar to that of Example 2, the Si and SiC phases are evenly distributed, the particle sizes of SiC are 20 μm and 50 μm, and the coating surface is complete, dense and defect-free.
[0176] Test Example 2: Friction and wear performance test.
[0177] The carbon ceramic brake discs for passenger cars currently available on the market and the carbon ceramic brake discs prepared by Examples 1-3 and Comparative Examples 4-5 of the present invention were subjected to AK-Master friction and wear performance test analysis (using the AKMaster program to evaluate the performance of the friction coefficient and wear rate. The entire AKMaster program includes 255 brakings, and each braking will form a braking curve. The peak value extreme difference of the instantaneous friction coefficient of a single braking is the difference between the highest point and the lowest point of the curve). The experiment was tested in accordance with the U.S. SAE-J2522 standard, and the test results are shown in Table 1. Among them, the carbon ceramic brake disc prepared from Example 2 was subjected to AK-Master friction and wear performance test analysis, and 6 brakings included in the AKMaster program were selected. The braking curves of the 6 brakings are shown in Table 1. Figure 4 shown.
[0178] Table 1 Test results of friction coefficient and disc wear
[0179] Product Name Friction coefficient Disc wear(mm) Carbon ceramic brake disc for a passenger car 0.42 0.015 Example 1 0.44 0.0006 Example 2 0.44 0.0005 Example 3 0.44 0.0008 Comparative Example 4 0.43 0.002 Comparative Example 5 0.43 0.0015
[0180] As shown in Table 1, compared with a carbon ceramic brake disc of a passenger car and comparative examples 4-5, the carbon ceramic brake discs prepared by the coating materials of Examples 1-3 of the present invention have a higher friction coefficient and a lower wear rate. The carbon ceramic brake disc prepared by Example 2 of the present invention has a friction coefficient of 0.44 and a wear amount of 0.0005 mm. Figure 4 It can be seen that the peak value difference of the instantaneous friction coefficient during a single braking process is basically stable within 0.1, which has good friction stability, significantly improves the service life of the carbon-ceramic brake disc, and can simultaneously meet the requirements of lightweight and high wear resistance of automobiles.
[0181] From the comparison between Example 2 and Comparative Example 4, it can be seen that as the particle size of SiC powder increases, the powder gap will also increase, resulting in a decrease in the volume ratio of SiC phase to Si phase in the coating. The increase in the content of Si phase with relatively low hardness leads to a decrease in the friction coefficient on the one hand, and an increase in wear on the other hand.
[0182] From the comparison between Example 2 and Comparative Example 5, it can be seen that mixing SiC powders of different particle sizes to prepare the coating cannot achieve the expected effect of relatively dense stacking of the particle grading, and the SiC / Si volume ratio increases instead of decreases, resulting in increased wear.
[0183] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0184] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A coating material, characterized in that: Calculated by weight percentage, the composition includes: 20-40wt% silicon carbide, 10-20wt% carbon black, 5-15wt% polyvinyl alcohol, 5-10wt% glycerol, and 25-60wt% water.
2. The coating material according to claim 1, characterized in that In terms of weight percentage, the coating material consists of 30 wt % silicon carbide, 15 wt % carbon black, 10 wt % polyvinyl alcohol, 5 wt % glycerol, and 40 wt % water.
3. The coating material according to claim 1, characterized in that The particle size of the silicon carbide is 20-50 μm.
4. The coating material according to claim 3, characterized in that The particle size of the silicon carbide is 20 μm.
5. A method for preparing a coating material according to any one of claims 1 to 4, characterized in that: include: Dissolving polyvinyl alcohol in water and mixing well to obtain a polyvinyl alcohol solution; Then, silicon carbide and carbon black are added to the polyvinyl alcohol solution in sequence, and after being stirred evenly, glycerol is added and mixed evenly to obtain a coating material.
6. A carbon-ceramic brake disc with a single-molded wear-resistant coating, characterized in that: The coating material comprises the coating material according to any one of claims 1 to 5.
7. A method for preparing a carbon-ceramic brake disc with a single-molded wear-resistant coating as claimed in claim 6, characterized in that: The following steps are involved: preparing a carbon / carbon composite material preform; Machining the carbon / carbon composite material preform and forming grooves on the designed upper and lower surfaces thereof to obtain a carbon / carbon preformed disc; The grooves on the upper and lower surfaces of the carbon / carbon prefabricated disc are respectively coated and filled with the coating material once, and after filling, vacuum treatment and drying are performed to obtain a carbon / carbon prefabricated disc with a single molding prefabricated coating; The carbon / carbon prefabricated disc body with the single-molded prefabricated coating is subjected to a carbonization treatment and a high-temperature ceramicization treatment in sequence to obtain a carbon-ceramic brake disc with a single-molded wear-resistant coating.
8. The method for preparing a carbon-ceramic brake disc with a single-molded wear-resistant coating according to claim 7, characterized in that: The pressure of the vacuum treatment is 5-6 Pa, and the time is 1-1.3 h.
9. The method for preparing a carbon-ceramic brake disc with a single-molded wear-resistant coating according to claim 7, characterized in that: The temperature of the carbonization treatment is 900-1000°C, the time is 3-4h, and the heating rate is 1-5°C / min.
10. The method for preparing a carbon-ceramic brake disc with a single-molded wear-resistant coating according to claim 7, characterized in that: The temperature of the high temperature ceramic treatment is 1450-1700° C., the time is 1-2 hours, and the heating rate is 1-5° C. / min.
Citation Information
Patent Citations
Methods of forming polymer coatings on metallic substrates
CN107073890A
Carbon-ceramic brake disc with wear-resistant and anti-oxidation coating and preparation method of carbon-ceramic brake disc
CN113277869A
Coating carbon-ceramic brake disc processing technology and coating carbon-ceramic brake disc
CN118221450A
Method for coating substrates with a carbon-based material
US20050079356A1
Cited By
Lightweight carbon ceramic-aluminum composite brake disc and preparation method thereof
CN120885690A