Water-based environment-friendly weather-resistant intumescent fireproof coating and preparation method thereof
By using crosslinked melamine polyphosphate and lignin sulfonate components in aqueous fire-resistant coatings, combining vapor phase silica and rutile titanium dioxide to form high weather-resistant expansion fire-resistant coatings, the problem of ammonium polyphosphate precipitation is solved. , improves the weather resistance and heat resistance of the coating and enhances the fire resistance of flammable materials.
Patent Information
- Application Number
- CN202411114391.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-01
AI Technical Summary
The existing water-based fire-resistant coatings are prone to cracking during use, the film has low strength, and fire-retardant flame retardant is easy to precipitate. Especially in the environment of rising temperatures and alternating temperature and humidity transformation, ammonium polyphosphate is easily migrated to the surface of the fire-resistant coating and precipitated, resulting in the coating. Gradually ineffective.
Using components such as aqueous acrylic resin, crosslinked melamine polyphosphate, lignin sulfonate, vapor phase silica and rutile titanium dioxide, etc., through crosslinking and coating technology, an expansion-type fire-resistant with high thermal decomposition temperature and weather resistance is formed. Paint improves the viscosity, thixotropy and heat resistance of fire-retardant coatings, slows down the settlement of flame retardant fillers, and enhances the ablation resistance and heat insulation properties of the carbon layer.
It significantly improves the weather resistance and heat resistance of fire-resistant coatings, weakens external heat source conduction and combustible gas diffusion, extends the service life of the coatings, and enhances the fire resistance of flammable products such as wood and plastics.
Smart Images

Figure BDA0004993218380000051 
Figure BDA0004993218380000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flame retardant coatings, and in particular to a water-based, environmentally friendly, weather-resistant intumescent fire retardant coating and a preparation method thereof. Background Art
[0002] The occurrence of fire can easily cause huge losses of people's lives and property, especially indoor buildings. Flammable products in indoor buildings are very likely to cause fires. Due to the low limiting oxygen index of the material, the fire will spread quickly and a large amount of toxic and harmful gases will be released. Once a fire occurs, it will spread very quickly. In order to avoid frequent fire accidents, indoor flammable products urgently need to improve the flame retardant effect of the material through modification to reduce the significant losses caused by fire. The traditional method of improving the flame retardant effect of flammable products is to apply a layer of flame retardant coating on the surface of the flammable products. This is an effective solution. However, traditional fire retardant coatings are mainly solvent-based fire retardant coatings. With the tightening of environmental protection VOC release, fire retardant coatings need to gradually shift to water-based halogen-free, formaldehyde-free, and VOC-free water-based fire retardant coatings. However, water-based fire retardant coatings have problems such as easy cracking, low film strength, and easy precipitation of fire retardants during use, especially water-based environmentally friendly flame retardants based on ammonium polyphosphate system. Due to the large solubility of ammonium polyphosphate in water, its solubility increases with the increase of temperature. In order to solve the dissolution and precipitation of ammonium polyphosphate, melamine resin coating, epoxy resin coating, silane coating and other methods are usually used to treat it, which to a certain extent eliminates the dispersibility of ammonium polyphosphate in the resin system and the migration and precipitation of ammonium polyphosphate. However, the cumbersome preparation process and mediocre performance limit its application scope to a certain extent. At the same time, the precipitation of ammonium polyphosphate still exists, especially in the alternating temperature and humidity environment, ammonium polyphosphate is easy to migrate to the surface of the fire retardant coating and precipitate in the form of crystals, causing the water-based fire retardant coating to gradually fail with the migration of time. Therefore, it is crucial to develop a water-based environmentally friendly weather-resistant fire retardant coating for the fire prevention of indoor flammable products. In particular, it is crucial to improve the fire resistance level and safety of flammable products such as wood, plastic products, walls, and floors. Summary of the invention
[0003] The purpose of the present invention is to provide a water-based, environmentally friendly and weather-resistant intumescent fire retardant coating and a preparation method thereof, so as to solve the problem in the prior art that fire retardants are easily dissolved out from the surface of the fire retardant coating.
[0004] To achieve the above object, the present invention provides the following technical solutions:
[0005] The invention provides a water-based environmentally friendly and weather-resistant intumescent fire-retardant coating, which comprises the following components in weight percentage: 30-40% of water-based acrylic resin, 30-45% of melamine polyphosphate, 15-30% of a carbon former, 0.5-3% of fumed silica, 0.5-3% of rutile titanium dioxide, 0.5-2% of lignin sulfonate, 0.5-1.5% of a dispersant, 0.5-2% of a defoamer, 0.5-2% of a wetting agent, 0.2-1% of a coupling agent, 0.2-1% of a leveling agent and 0.5-1.5% of a cross-linking agent.
[0006] Furthermore, the water-based acrylic resin includes one or more of epoxy-modified acrylic resin, polyurethane-modified acrylic resin, and non-modified water-based acrylic resin, wherein the solid content of the active ingredient is 20-40%.
[0007] Furthermore, the melamine polyphosphate has an average particle size D50 of less than 10 μm, a solubility in water of less than 0.1 g / 100 g, a thermal decomposition temperature of greater than 300° C., a nitrogen content of greater than 37%, and a phosphorus content of greater than 14%.
[0008] Furthermore, the carbon-forming agent includes one or more of pentaerythritol, dipentaerythritol, chitosan, lignin, and sodium alginate, and the purity thereof is greater than 98%.
[0009] Furthermore, the specific surface area of the fumed silica is 100-400m 2 / g, surface hydrophilicity / lipophilicity, the particle size of the rutile titanium dioxide is less than 15 μm, and the solid content of the slurry is greater than 55%.
[0010] Furthermore, the lignin sulfonate includes one or more of sodium lignin sulfonate, potassium lignin sulfonate, and calcium lignin sulfonate, and the sulfur content is 5-10%.
[0011] Furthermore, the dispersant is a silicone-modified acrylic dispersant, the wetting agent is a polyether / modified silicone wetting agent, and the coupling agent is one or more of KH550, KH560, KH570, and WD70 silane coupling agents.
[0012] Furthermore, the leveling agent is a silicone-modified polyether, and the cross-linking agent is one or more cross-linking agents selected from the group consisting of aziridine, polyaziridine, and polycarbodiimide.
[0013] The present invention also provides a method for preparing a water-based, environmentally friendly and weather-resistant intumescent fire-retardant coating, comprising the following steps: weighing a given amount of water-based acrylic resin, adding fumed silica and stirring and dispersing it uniformly at high speed, adding a dispersant, a wetting agent, a leveling agent, a defoamer, a coupling agent, and a lignin sulfonate and stirring and dispersing it uniformly at high speed, adding a carbonizing agent and stirring and dispersing it uniformly at high speed, and then adding a cross-linking agent and stirring and dispersing it uniformly at high speed, sand-grinding the obtained slurry with a sand mill, and finally adding water to adjust the viscosity of the fire-retardant coating to 3000-6000 Pa.s to obtain a final coating.
[0014] Based on the above technical solution, the embodiments of the present invention can at least produce the following technical effects:
[0015] Water-based acrylic resin has excellent weather resistance, and the water resistance and weather resistance of the resin are further improved by cross-linking; in the prepared fire-retardant coating, the surface of the melamine polyphosphate flame retardant has a positive charge and is not easy to disperse in the water-based resin system; lignin sulfonate has good water solubility and a high carbon content, and can be used as a carbon source in the flame-retardant coating. Since the sulfonic acid group of the lignin after sulfonation is negatively charged, it can be adsorbed to the surface of the melamine polyphosphate through electrostatic action, thereby improving the dispersion performance of the melamine polyphosphate in the resin matrix; fumed silica has a large specific surface area and rich hydroxyl groups on the surface. When added to the water-based acrylic fire-retardant coating, it can form hydrogen bonds with water and acrylic acid through the hydroxyl groups on the surface, thereby improving the viscosity and thixotropy of the fire-retardant coating and slowing down the sedimentation and stratification of the flame-retardant filler in the coating. At the same time, during the fire-proof heating process, the fumed silica has good heat resistance The rutile titanium dioxide has excellent ultraviolet absorption ability, which can improve the ultraviolet resistance of the fire-retardant coating. At the same time, the polyphosphoric acid produced by the thermal decomposition of the fire-retardant coating combines with titanium dioxide to form titanium pyrophosphate, which can improve the ablation resistance of the carbon layer. The water solubility of melamine polyphosphate itself is low, and the hydrolysis product melamine is slightly soluble in water. Unlike the ammonium phosphate produced by the hydrolysis of ammonium polyphosphate, which is highly soluble in water, the dissolution, migration and precipitation of melamine polyphosphate in a humid alternating environment is kinetically weaker than that of ammonium polyphosphate. In the process of thermal decomposition of the fire-retardant coating, the thermal decomposition temperature of melamine polyphosphate is about 320°C, which is significantly higher than the thermal decomposition temperature of ammonium polyphosphate (about 225°C). The polyphosphoric acid produced by the decomposition combines with dipentaerythritol to form phosphate ester. As the temperature rises, the polyphosphate ester is dehydrated and carbonized, and the gas source melamine is thermally decomposed to produce nitrogen, which expands under the action of ammonia. A porous carbon layer is formed, and the structural strength and ablation resistance of the carbon layer are improved under the action of titanium dioxide and fumed silica, and a carbon layer with excellent ablation resistance, heat insulation and barrier properties is formed on the surface of the substrate, which can greatly reduce the conduction of external heat sources to the fire-retardant coating substrate and reduce the thermal decomposition of the substrate. At the same time, to a certain extent, it blocks the diffusion of combustible gases generated by the substrate to the surface and reduces the heat release rate. The organic combination of acid source (polyphosphoric acid) and gas source (melamine) can better coordinate the formation of fire-retardant carbon layer, reducing the uneven distribution of components caused by physical mixing when used alone, thereby causing the inhomogeneity of the expanded carbon layer. DETAILED DESCRIPTION
[0016] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0017] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0018] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0019] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0020] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0021] Example 1
[0022] Water-based acrylic resin 34%, melamine polyphosphate 42%, chitosan 14%, fumed silica 2%, rutile titanium dioxide 2%, calcium lignin sulfonate 1%, silicone-modified acrylic dispersant 1%, silicone defoamer 0.5%, polyether wetting agent 1%, coupling agent KH550 0.5%, silicone-modified polyether leveling agent 1%, polycarbodiimide crosslinking agent 1%.
[0023] Example 2
[0024] 30% water-based acrylic resin, 30% melamine polyphosphate, 30% pentaerythritol, 1.5% fumed silica, 2.5% rutile titanium dioxide, 1% sodium lignin sulfonate, 1% silicone-modified acrylic dispersant, 0.5% silicone defoamer, 1% polyether wetting agent, 0.5% KH560 coupling agent, 1% modified silicone leveling agent, and 1% aziridine crosslinking agent.
[0025] Example 3
[0026] 30% water-based acrylic resin, 30% melamine polyphosphate, 30% dipentaerythritol, 1.5% fumed silica, 2.5% rutile titanium dioxide, 1% sodium lignin sulfonate, 1% organosilicon-modified acrylic dispersant, 0.5% organosilicon defoamer, 1% modified organosilicon wetting agent, 0.5% KH570 coupling agent, 1% organosilicon-modified polyether leveling agent, and 1% polyaziridine crosslinking agent.
[0027] Example 4
[0028] Water-based acrylic resin 30%, melamine polyphosphate 40%, dipentaerythritol 20%, fumed silica 2%, rutile titanium dioxide 2%, sodium lignin sulfonate 1%, silicone-modified acrylic dispersant 1%, silicone defoamer 0.5%, modified silicone wetting agent 1%, KH550 coupling agent 0.5%, silicone-modified polyether leveling agent 1%, aziridine crosslinking agent 1%.
[0029] Example 5
[0030] Water-based acrylic resin 33%, melamine polyphosphate 38%, dipentaerythritol 19%, fumed silica 2%, rutile titanium dioxide 2%, calcium lignin sulfonate 1%, silicone-modified acrylic dispersant 1%, silicone defoamer 0.5%, modified silicone wetting agent 1%, KH550 coupling agent 0.5%, silicone-modified polyether leveling agent 1%, aziridine crosslinking agent 1%.
[0031] Example 6
[0032] Water-based acrylic resin 36%, melamine polyphosphate 40.5%, dipentaerythritol 13.5%, fumed silica 2%, rutile titanium dioxide 2%, calcium lignin sulfonate 1%, silicone-modified acrylic dispersant 1%, silicone defoamer 0.5%, modified silicone wetting agent 1%, KH550 coupling agent 0.5%, silicone-modified polyether leveling agent 1%, aziridine crosslinking agent 1%.
[0033] Example 7
[0034] Water-based acrylic resin 40%, melamine polyphosphate 37.5%, dipentaerythritol 12.5%, fumed silica 2%, rutile titanium dioxide 2%, calcium lignin sulfonate 1%, silicone-modified polyacrylic acid dispersant 1%, silicone defoamer 0.5%, modified silicone wetting agent 1%, KH550 coupling agent 0.5%, silicone-modified polyether leveling agent 1%, aziridine crosslinking agent 1%.
[0035] Example 8
[0036] Water-based acrylic resin 34%, ammonium polyphosphate (polymerization degree n>1000) 42%, dipentaerythritol 14%, fumed silica 2%, rutile titanium dioxide 2%, calcium lignin sulfonate 1%, organosilicon-modified polyacrylic acid dispersant 1%, organosilicon-type defoaming agent 0.5%, modified organosilicon-type wetting agent 1%, KH550 coupling agent 0.5%, organosilicon-modified polyether leveling agent 1%, and aziridine cross-linking agent 1%.
[0037] Example 9
[0038] Water-based acrylic resin 34%, melamine resin coated ammonium polyphosphate (polymerization degree n>1000) 42%, dipentaerythritol 14%, fumed silica 2%, rutile titanium dioxide 2%, calcium lignin sulfonate 1%, silicone-modified acrylic dispersant 1%, silicone defoamer 0.5%, modified silicone wetting agent 1%, KH550 coupling agent 0.5%, silicone-modified polyether leveling agent 1%, aziridine crosslinking agent 1%.
[0039] The components of Examples 1-9 were made into water-based, environmentally friendly, weather-resistant intumescent fire retardant coatings according to the following preparation method, and performance tests were carried out. The results are shown in Table 1:
[0040]
[0041]
[0042] Finally, it should be noted that:
[0043] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that the technical solutions described in the above embodiments may still be modified, or some or all of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A water-based, environmentally friendly, weather-resistant, intumescent fire-retardant coating, characterized in that: The invention comprises the following components in weight percentage: 30-40% of waterborne acrylic resin, 30-45% of melamine polyphosphate, 15-30% of carbon former, 0.5-3% of fumed silica, 0.5-3% of rutile titanium dioxide, 0.5-2% of lignin sulfonate, 0.5-1.5% of dispersant, 0.5-2% of defoamer, 0.5-2% of wetting agent, 0.2-1% of coupling agent, 0.2-1.5% of leveling agent and 0.5-1.5% of cross-linking agent.
2. The water-based, environmentally friendly, weather-resistant, intumescent fire retardant coating according to claim 1, characterized in that: The water-based acrylic resin includes one or more of epoxy-modified acrylic resin, polyurethane-modified acrylic resin and non-modified water-based acrylic resin, wherein the solid content of the active ingredient is 20-40%.
3. The water-based, environmentally friendly, weather-resistant, intumescent fire-retardant coating according to claim 1, characterized in that: The melamine polyphosphate has an average particle size D50 of less than 10 μm, a solubility in water of less than 0.1 g / 100 g, a thermal decomposition temperature of greater than 300° C., a nitrogen content of greater than 37%, and a phosphorus content of greater than 14%.
4. The water-based, environmentally friendly, weather-resistant, intumescent fire retardant coating according to claim 1, characterized in that: The carbon-forming agent includes one or more of pentaerythritol, dipentaerythritol, chitosan, lignin, and sodium alginate, and the purity thereof is greater than 98%.
5. The water-based, environmentally friendly, weather-resistant, intumescent fire-retardant coating according to claim 1, characterized in that: The specific surface area of the fumed silica is 100-400m 2 / g, the particle size of the rutile titanium dioxide is less than 15 μm, and the solid content of the slurry is greater than 55%.
6. The water-based, environmentally friendly, weather-resistant, intumescent fire-retardant coating according to claim 1, characterized in that: The lignin sulfonate includes one or more of sodium lignin sulfonate, potassium lignin sulfonate and calcium lignin sulfonate, and has a sulfur content of 5-10%.
7. The water-based, environmentally friendly, weather-resistant, intumescent fire-retardant coating according to claim 1, characterized in that: The dispersant is a silicone acrylic modified dispersant, the wetting agent is a polyether / modified silicone wetting agent, the coupling agent is one or more of KH550, KH560, KH570, and WD70 silane coupling agents, the leveling agent is a silicone modified polyether, and the crosslinking agent is one or more of aziridine, polyaziridine, and polycarbodiimide crosslinking agents.
8. The method for preparing the water-based environmentally friendly weather-resistant intumescent fire retardant coating according to any one of claims 1 to 7, characterized in that: The following steps are involved: Weigh a given amount of water-based acrylic resin, add fumed silica, stir and disperse evenly at high speed, add a dispersant, a wetting agent, a leveling agent, a defoamer, a coupling agent, and a lignin sulfonate, stir and disperse evenly at high speed, add a carbonizing agent, stir and disperse evenly at high speed, then add a cross-linking agent, stir and disperse evenly at high speed, grind the obtained slurry with a sand mill, and finally add water to adjust the viscosity of the fire retardant coating to 3000-6000 Pa.s to obtain a final coating.
Citation Information
Patent Citations
Water-based expansive high-temperature-resistant fire retardant paint and preparation process thereof
CN108715705A
Waterborne intumescent finishing fireproof paint
CN110256927A
Grid-free thick fireproof coating for steel structure and preparation method thereof
CN110511635A
Water-based intumescent fire retardant coating for indoor steel structure and preparation method thereof
CN112980262A
Water-based ultra-thin indoor fireproof coating for steel structure surface and preparation method of water-based ultra-thin indoor fireproof coating
CN114133802A
Cited By
Water-based inner cabin coating based on nano titanium dioxide and phosphorus-nitrogen synergistic flame-retardant system and preparation method of water-based inner cabin coating
CN120505013A