Carbon-ceramic brake disc coating repairing agent and carbon-ceramic brake disc coating repairing method

By using silicon carbide, resin, carbon powder and silicon powder repair agents, combined with pressing, silicon permeation and grinding steps, the problem of oxidation of carbon ceramic brake discs in high temperature environments is solved, and effective coating repair and oxygen barrier are achieved. Reduces operating complexity and cost and extends the service life of the brake disc.

CN118879151APending Publication Date: 2024-11-01福建康碳防务材料科技有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411191626.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Carbon ceramic brake discs are prone to oxidation in high temperature environments, resulting in coating damage, affecting the density and strength of the material, and even leading to brake failure. The existing coating repair methods have problems of high cost and complex operation.

Method used

Provide a carbon ceramic brake disc coating repair agent, containing 70-85% silicon carbide, 5-20% resin, 5-10% carbon powder, and 5-10% silicon powder, through mixing, coating, pressing, and permeation of silicon and polishing steps to repair to prevent oxygen from entering and prevent carbon fiber oxidation.

Benefits of technology

It realizes effective repair of carbon ceramic brake disc coating, blocks oxygen inlet and prevents carbon fiber oxidation, is simple to operate, short cycle and low cost, is suitable for online repair, extending the service life of the brake disc.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879151A_ABST
    Figure CN118879151A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of carbon-ceramic brake discs, and particularly relates to a carbon-ceramic brake disc coating repairing agent and a carbon-ceramic brake disc coating repairing method. The carbon ceramic brake disc coating repairing agent provided by the invention comprises 70-85% of silicon carbide, 5-20% of resin, 5-10% of carbon powder and 5-10% of silicon powder. The carbon-ceramic brake disc coating repairing agent provided by the invention is suitable for repairing carbon-ceramic brake discs of which the coatings are damaged during installation and carbon-ceramic brake discs of which the coatings are cracked by unknown objects and fall off during use. The invention provides a method for repairing a coating of a carbon-ceramic brake disc, which comprises the following steps of: coating a damaged coating area of the carbon-ceramic brake disc with a damaged coating with a repairing agent, and then sequentially pressing, siliconizing and polishing. The carbon-ceramic brake disc coating repairing agent provided by the invention can effectively repair a carbon-ceramic brake disc coating, is convenient and easy to implement, and can effectively prevent oxygen from entering the carbon-ceramic brake disc coating after repairing and prevent carbon fibers from being oxidized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of carbon-ceramic brake discs, and in particular relates to a carbon-ceramic brake disc coating repair agent and a carbon-ceramic brake disc coating repair method. Background Art

[0002] In recent years, the market share of carbon-ceramic brake discs for automobiles has been increasing. Due to their excellent properties such as wear resistance, light weight and high temperature resistance, carbon-ceramic brake discs are widely used as a new generation of high-performance friction materials in the braking field.

[0003] The remarkable feature of carbon materials is that they remain stable over a wide temperature range, but their biggest disadvantage is that they are easily oxidized in air above 400°C. If there are exposed carbon fibers and carbon matrices on the surface of carbon-ceramic brake materials, these exposed carbon fibers and carbon matrices are easily oxidized in a high-temperature oxidative environment. When slightly oxidized, the density of the material decreases and the strength decreases. As the temperature rises, the oxidation of the brake disc material intensifies. When severely oxidized, the material will be delaminated and even become flocculent, completely losing the mechanical properties of the material, resulting in brake failure and even accidents.

[0004] Therefore, it is generally necessary to prepare a coating on the surface of the brake disc. The main coating preparation methods include chemical vapor deposition, sol-gel, liquid phase, solid infiltration, etc. The coatings prepared by these methods can protect the substrate to a certain extent. However, the problem is that the surface coating will be damaged during the equipment process of the brake disc, thereby affecting the protective effect of the coating and the normal use of the carbon ceramic material. Summary of the invention

[0005] The purpose of the present invention is to provide a carbon-ceramic brake disc coating repair agent and a carbon-ceramic brake disc coating repair method. The carbon-ceramic brake disc coating repair agent provided by the present invention can effectively repair the carbon-ceramic brake disc coating. It is not only convenient and easy, but also can effectively block the entry of oxygen and prevent the oxidation of carbon fiber after repair. It is suitable for carbon-ceramic brake discs whose coating is damaged during installation and some carbon-ceramic brake discs whose coating is cracked and detached by unknown objects during use.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] The invention provides a carbon ceramic brake disc coating repair agent, which comprises the following components in percentage by mass: 70-85% of silicon carbide, 5-20% of resin, 5-10% of carbon powder and 5-10% of silicon powder.

[0008] Preferably, the resin is a phenolic resin.

[0009] The present invention provides a method for preparing the carbon-ceramic brake disc coating repair agent described in the above technical solution, comprising the following steps:

[0010] The silicon carbide, resin, carbon powder and silicon powder are mixed to obtain the carbon-ceramic brake disc coating repair agent.

[0011] Preferably, the mixing temperature is room temperature and the mixing time is 8 to 10 hours.

[0012] The present invention provides a carbon-ceramic brake disc coating repair method, comprising the following steps:

[0013] Applying the carbon-ceramic brake disc coating repair agent described in the above technical solution or the carbon-ceramic brake disc coating repair agent prepared by the preparation method described in the above technical solution to the damaged coating area of ​​the carbon-ceramic brake disc with damaged coating to obtain a carbon-ceramic brake disc coated with the repair agent;

[0014] The carbon-ceramic brake disc coated with the repairing agent is pressed, siliconized and polished in sequence.

[0015] Preferably, the pressing temperature is 130-150° C., the pressure is 2-5 MPa, and the pressing time is 20-30 min.

[0016] Preferably, the insulation temperature of the siliconizing is 1400-1500° C., and the insulation time is 1-2 hours.

[0017] Preferably, the siliconizing includes the following steps: evacuating the environment of the pressed carbon-ceramic brake disc to 1-2 kPa and maintaining the pressure for 30-40 minutes; then starting the timing, maintaining the pressure increase rate ≤ 700 Pa / 30 min, maintaining the pressure of the environment of the pressed carbon-ceramic brake disc at 70-80 kPa from 0 to 13.5 hours but not 13.5 hours, and evacuating the environment of the pressed carbon-ceramic brake disc to the ultimate vacuum from 13.5 to 19.67 hours; maintaining the ultimate vacuum to raise the temperature of the environment of the pressed carbon-ceramic brake disc from room temperature to the insulation temperature of the siliconizing.

[0018] Preferably, before the coating, the method further comprises: cleaning and drying the carbon-ceramic brake disc with damaged coating in sequence, wherein the cleaning is performed under ultrasonic conditions for 30 to 40 minutes; and the drying temperature is 130 to 150° C. for 30 to 70 minutes.

[0019] Preferably, the grinding includes sequentially performing coarse grinding and fine grinding.

[0020] The present invention provides a carbon-ceramic brake disc coating repair agent, comprising the following components in percentage by mass: 70-85% silicon carbide, 5-20% resin, 5-10% carbon powder, and 5-10% silicon powder. The carbon-ceramic brake disc coating repair agent provided by the present invention is suitable for repairing carbon-ceramic brake discs whose coating is damaged during installation and some carbon-ceramic brake discs whose coating is cracked and detached by unknown objects during use. The carbon-ceramic brake disc coating repair agent provided by the present invention can effectively repair the carbon-ceramic brake disc coating, which is not only convenient and easy to operate, but also can effectively block the entry of oxygen after repair to prevent the oxidation of carbon fiber.

[0021] The present invention provides a carbon-ceramic brake disc coating repair method, comprising the following steps: applying the carbon-ceramic brake disc coating repair agent described in the above technical solution or the carbon-ceramic brake disc coating repair agent prepared by the preparation method described in the above technical solution to the damaged coating area of ​​the carbon-ceramic brake disc with damaged coating to obtain a carbon-ceramic brake disc coated with the repair agent; and sequentially pressing, siliconizing and polishing the carbon-ceramic brake disc coated with the repair agent. The repair method provided by the present invention has a simple operation process, a short cycle, and low cost, and can be repaired online, which is convenient and easy. At the same time, it can effectively repair the carbon-ceramic brake disc coating, and after repair, it can effectively block the entry of oxygen and prevent the oxidation of carbon fiber. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a physical picture of the sample before glue repair in Example 1 of the present invention;

[0023] Figure 2 This is a real picture of the sample after glue repair in Example 1 of the present invention;

[0024] Figure 3 This is a physical picture of the sample before siliconization in Example 1 of the present invention;

[0025] Figure 4 This is a physical picture of the sample after siliconization in Example 1 of the present invention;

[0026] Figure 5 This is a physical picture of the sample after grinding in Example 1 of the present invention. DETAILED DESCRIPTION

[0027] The invention provides a carbon ceramic brake disc coating repair agent, which comprises the following components in percentage by mass: 70-85% of silicon carbide, 5-20% of resin, 5-10% of carbon powder and 5-10% of silicon powder.

[0028] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.

[0029] In terms of mass percentage, the carbon ceramic brake disc coating repair agent provided by the present invention comprises 70-85% silicon carbide, and is preferably 70%, 75%, 80% or 85%. The silicon carbide is preferably silicon carbide powder. The particle size of the silicon carbide powder is preferably 10-20 μm.

[0030] In terms of mass percentage, the carbon ceramic brake disc coating repair agent provided by the present invention includes 5-20% of resin, and is preferably 5%, 10%, 15% or 20%. In the present invention, the resin is a phenolic resin. The solid content of the phenolic resin is preferably 55-65%, and is more preferably 60%. The phenolic resin is preferably purchased from Shandong Shengquan New Materials Co., Ltd.

[0031] The carbon ceramic brake disc coating repair agent provided by the present invention comprises 5-10% carbon powder, preferably 5%, by mass percentage. In the present invention, the particle size of the carbon powder is preferably 10-15 μm.

[0032] The carbon ceramic brake disc coating repair agent provided by the present invention comprises 5-10% silicon powder, preferably 5%, by mass percentage. In the present invention, the particle size of the silicon powder is preferably 2-3 mm.

[0033] The present invention provides a method for preparing the carbon-ceramic brake disc coating repair agent described in the above technical solution, comprising the following steps:

[0034] The silicon carbide, resin, carbon powder and silicon powder are mixed to obtain the carbon-ceramic brake disc coating repair agent.

[0035] In the present invention, the mixing is preferably carried out in a mixer. The mixing temperature is preferably room temperature, and the mixing time is preferably 8 to 10 hours.

[0036] The present invention provides a carbon-ceramic brake disc coating repair method, comprising the following steps:

[0037] Applying the carbon-ceramic brake disc coating repair agent described in the above technical solution or the carbon-ceramic brake disc coating repair agent prepared by the preparation method described in the above technical solution to the damaged coating area of ​​the carbon-ceramic brake disc with damaged coating to obtain a carbon-ceramic brake disc coated with the repair agent;

[0038] The carbon-ceramic brake disc coated with the repairing agent is pressed, siliconized and polished in sequence.

[0039] In the present invention, before the coating, the present invention preferably further comprises: washing and drying the carbon ceramic brake disc with damaged coating in sequence. The washing is preferably carried out with water, the washing is preferably carried out under ultrasonic conditions, and the washing time is preferably 30 to 40 minutes. The drying is preferably carried out in an oven, the drying temperature is preferably 120 to 150°C, and the drying time is preferably 30 to 70 minutes.

[0040] The present invention has no special requirements for the specific implementation of the coating. During the coating, the coating amount of the carbon ceramic brake disc coating repair agent is preferably 2 to 2.5 g / cm 2 .

[0041] In the present invention, the pressing is preferably performed by a hot press, and the hot press is preferably a small hot press of 150T. The pressing is preferably performed on the entire carbon-ceramic brake disc coated with a repair agent. The pressing temperature is preferably 130-150°C, the pressure is preferably 2-5MPa, and the time is preferably 20-30min. In the present invention, the pressing is performed on the two disc surfaces of the carbon-ceramic brake disc coated with a repair agent.

[0042] In the present invention, the insulation temperature of the siliconizing is preferably 1400-1500°C, and the insulation time is preferably 1-2h. The siliconizing preferably includes the following steps: evacuating the environment of the pressed carbon-ceramic brake disc to 1-2kPa, and maintaining the pressure for 30-40min; then starting the timing, maintaining the pressure increase rate ≤700Pa / 30min, maintaining the pressure of the environment of the pressed carbon-ceramic brake disc at 70-80kPa from 0 to 13.5h and not 13.5h, and evacuating the environment of the pressed carbon-ceramic brake disc to the ultimate vacuum from 13.5 to 19.67h; maintaining the ultimate vacuum to raise the temperature of the environment of the pressed carbon-ceramic brake disc from room temperature to the insulation temperature of the siliconizing. In the present invention, the siliconizing is to siliconize the two disc surfaces of the carbon-ceramic brake disc coated with a repair agent after pressing.

[0043] In the present invention, the grinding is performed on the area of ​​the carbon ceramic brake disc surface coated with the repair agent. The grinding preferably includes coarse grinding and fine grinding in sequence. The present invention has no special requirements for the specific implementation process of the coarse grinding and fine grinding.

[0044] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0045] Example 1

[0046] First, put the brake disc with damaged coating into ultrasonic cleaning for 30 minutes, and then bake it in a 150℃ oven for 70 minutes.

[0047] Preparation of repair agent: 80% of silicon carbide, 10% of phenolic resin, 5% of carbon powder and 5% of silicon powder are put into a mixer for 8 hours to obtain a carbon-ceramic brake disc coating repair agent (rubber).

[0048] Put the gap of the brake disc into the mixed carbon ceramic brake disc coating repair agent, and then put it into a 150T small hot press, adjust the temperature to the actual temperature of 150°C, adjust the pressure to 2-5MPa, and perform siliconization for 20 minutes. The temperature of the siliconization treatment is 1500°C and the time is 2h. The specific operation steps of the siliconization are preferably: pumping to 2kPa, maintaining pressure for 30 minutes, pressure rise rate ≤700Pa / 30min, vacuum gauge pressure of 70-80kPa for 0-13.5 hours, extreme vacuum for 13.5-19.67 hours, and temperature reaching 1500°C.

[0049] After siliconizing, rough grinding and fine grinding are carried out.

[0050] Figure 1 This is a physical picture of the sample before glue filling in Example 1; Figure 2 This is a real picture of the sample after the glue repair (coating of carbon ceramic brake disc coating repair agent) in Example 1; Figure 3 This is a real picture of the sample of Example 1 before siliconization (i.e. after pressing); Figure 4 This is a real picture of the sample after siliconization in Example 1; Figure 5 This is a physical picture of the sample after grinding (i.e., coarse grinding and fine grinding) in Example 1.

[0051] Example 2

[0052] The base fabric is the same as that in Example 1, except that the proportion of phenolic resin powder is adjusted to 5%, silicon carbide is adjusted to 85%, and other operations are the same.

[0053] Example 3

[0054] The base fabric is the same as that in Example 1, except that the proportion of phenolic resin powder is adjusted to 20%, silicon carbide is adjusted to 70%, and other operations are the same.

[0055] Example 4

[0056] The base fabric is the same as that in Example 1, except that the proportion of phenolic resin powder is adjusted to 15%, silicon carbide is adjusted to 75%, and other operations are the same.

[0057] From the repair results of Examples 1 to 4 above, it can be seen that: the percentage of phenolic resin in the repair agent used in Example 3 is too high, resulting in fine bubbles in the coating when hot pressing. The percentage of phenolic resin powder in Example 2 is too low, resulting in insufficient adhesion of the coating, and the coating is prone to cracking after hot pressing. The coatings of Examples 1 and 4 are in good condition without abnormalities.

[0058] From the above embodiments, it can be seen that the carbon-ceramic brake disc coating repair method provided by the present invention is to apply a repair agent composed of silicon carbide, resin, carbon powder and silicon powder to the damaged coating area of ​​the carbon-ceramic brake disc with damaged coating, and then press, siliconize and polish the damaged area coated with the repair agent in sequence. The repair method provided by the present invention has a simple operation process, a short cycle, low cost, and can be repaired online, which is convenient and easy. At the same time, it can effectively repair the carbon-ceramic brake disc coating, and after repair, it can effectively block the entry of oxygen and prevent the oxidation of carbon fiber.

[0059] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A carbon ceramic brake disc coating repair agent, characterized in that: The invention comprises the following components in percentage by mass: 70-85% of silicon carbide, 5-20% of resin, 5-10% of carbon powder and 5-10% of silicon powder.

2. The carbon-ceramic brake disc coating repair agent according to claim 1, characterized in that: The resin is a phenolic resin.

3. The method for preparing the carbon ceramic brake disc coating repair agent according to claim 1 or 2, characterized in that: The following steps are involved: The silicon carbide, resin, carbon powder and silicon powder are mixed to obtain the carbon-ceramic brake disc coating repair agent.

4. The preparation method according to claim 3, characterized in that: The mixing temperature is room temperature and the mixing time is 8 to 10 hours.

5. A method for repairing a carbon-ceramic brake disc coating, characterized in that: The following steps are involved: Applying the carbon-ceramic brake disc coating repair agent according to claim 1 or 2 or the carbon-ceramic brake disc coating repair agent prepared by the preparation method according to claim 3 or 4 to the damaged coating area of ​​a carbon-ceramic brake disc with damaged coating to obtain a carbon-ceramic brake disc coated with the repair agent; The carbon-ceramic brake disc coated with the repairing agent is pressed, siliconized and polished in sequence.

6. The carbon ceramic brake disc coating repair method according to claim 5, characterized in that: The pressing temperature is 130-150° C., the pressure is 2-5 MPa, and the pressing time is 20-30 min.

7. The carbon ceramic brake disc coating repair method according to claim 5 or 6, characterized in that: The insulation temperature of the siliconizing is 1400-1500° C., and the insulation time is 1-2 hours.

8. The carbon-ceramic brake disc coating repair method according to claim 7, characterized in that: The siliconizing comprises the following steps: evacuating the environment of the pressed carbon ceramic brake disc to 1-2 kPa and maintaining the pressure for 30-40 minutes; then starting the timing, maintaining the pressure increase rate ≤ 700 Pa / 30 minutes, maintaining the pressure of the environment of the pressed carbon ceramic brake disc at 70-80 kPa from 0 to 13.5 hours but not 13.5 hours, and evacuating the environment of the pressed carbon ceramic brake disc to the ultimate vacuum from 13.5 to 19.67 hours; maintaining the ultimate vacuum to raise the temperature of the environment of the pressed carbon ceramic brake disc from room temperature to the insulation temperature of the siliconizing.

9. The carbon-ceramic brake disc coating repair method according to claim 5, characterized in that: Before the coating, the method further includes: cleaning and drying the carbon ceramic brake disc with damaged coating in sequence, wherein the cleaning is performed under ultrasonic conditions for 30 to 40 minutes; and the drying temperature is 130 to 150° C. for 30 to 70 minutes.

10. The carbon ceramic brake disc coating repair method according to claim 5, characterized in that: The grinding includes sequentially performing rough grinding and fine grinding.

Citation Information

Cited By

  • Composite slurry, preparation method therefor, and use thereof

    WO2026137957A1