Method for preparing anti-adhesion nano coating based on molecular brush grafting technology

Through molecular brush grafting technology, nano-scale anti-adhesion coating is formed on the surface of the substrate, which solves the problems of substrate limitations and production process complexity in the prior art, and achieves efficient and stable anti-adhesion effect, which is suitable for a variety of purposes Substrate and precision fields.

CN118879199AActive Publication Date: 2024-11-01DALIAN UNIV OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410968516.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-01
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The existing adhesion-free coating preparation process has problems such as substrate limitations, complex preparation process, harsh conditions, long time and difficulty in achieving nanoscale thickness, which limits its application in the fields of energy utilization and precision.

Method used

Using molecular brush grafting technology, by dissolving anti-adhesion polymers in organic solvents and adding them dropwise to the silicone molecular solution to react to form anti-adhesion polymers, and through hydrogen bonding, complexing and π-π bonding, The substrate surface is grafted to achieve the preparation of anti-adhesion coating with nanoscale thickness.

Benefits of technology

The simple and gentle preparation of nano-scale anti-adhesion coatings that are not limited by substrates are achieved, which improves the anti-adhesion effect and stability of the substrates, is suitable for a variety of substrates, and reduces the complexity and time of the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004952428820000061
    Figure BDA0004952428820000061
  • Figure HDA0004952428830000011
    Figure HDA0004952428830000011
  • Figure HDA0004952428830000012
    Figure HDA0004952428830000012
Patent Text Reader

Abstract

The invention belongs to the technical field of nano-coating preparation, and provides a method for preparing an anti-adhesion nano-coating based on a molecular brush grafting technology, which comprises the following steps: coating a clean and dry base material with an anti-adhesion polymer solution, grafting anti-adhesion polymers on the surface of the base material under the actions of hydrogen bonds, complexation and pi-pi bonds to obtain the anti-adhesion nano-coating. And after the organic solvent is completely volatilized, cleaning and removing the anti-adhesion macromolecules which are not stably combined with the base material, namely forming the anti-adhesion nano coating on the surface of the base material. The anti-adhesion polymer is formed by reacting organic silicon molecules with an adhesive, and the adhesive is a compound with hydroxyl and amino on a benzene ring. According to the method, the anti-adhesion coating with the nanoscale thickness can be simply and mildly prepared on the basis of being not limited by a base material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nano coating preparation, and relates to a method for preparing an anti-adhesion nano coating based on a molecular brush grafting technology. Background Art

[0002] The adhesion of pollutants on the surface will cause losses to actual production and life and even threaten personal safety. In the energy field, the deposition of particulate pollutants and the accumulation of ice and snow on solar photovoltaic panels will block the propagation of sunlight, resulting in a decrease in the utilization rate of sunlight and a decrease in the efficiency of photovoltaic power generation; wind turbine blades will lose 10% to 30% of their power generation each year due to surface ice and snow, and in severe cases, the wind turbine may even collapse, causing economic losses. In the field of transportation, ice on the surface of aircraft wings will lead to a loss of lift and increase the risk of crashes. It can be seen that non-adhesive surfaces play a vital role in many fields such as liquid transportation, anti-fouling and inhibition of ice deposition.

[0003] Non-adhesive surfaces are usually required to have liquid repellency. Since the proposal of Young's equation in the 17th century, people have developed a variety of anti-adhesive surfaces, namely liquid repellent surfaces, based on biomimetic principles and surface interface regulation technology. At present, the development of advanced liquid repellent technology has gone through several stages, from air-structure lubrication (Superhydrophobic surface, SHS) in 1996, air-Re-entrant structure (Superomniphobic surface, SOS) in 2007, liquid-structure lubrication (Liquid infused surface, LIS) in 2011, air-Double Re-entrant structure (Superomniphobic surface, SOS) in 2014, to chemical grafted liquid lubrication (Liquid-like surface, LLS) in 2016. In general, the strategies to reduce the adhesion of the surface mainly include regulating the surface geometry and chemical surface modification, the essence of which is to change the interface between the object and the substrate to achieve liquid repellency and anti-adhesion effects. However, super-hydrophobic surfaces based on micro-textures still face challenges in practical applications in certain fields due to their inherent limitations. For example, in low temperature or high humidity environments, water vapor or fine droplets will condense or even freeze in the micro-texture, causing the super-hydrophobic structure to fail. In addition, when liquids with low surface tension flow on the surface of the structure or when droplets hit the surface, they can easily enter the interior of the micro-texture and cause the hydrophobic structure to fail. For liquid-infused surfaces based on liquid lubrication, the lubricant will be lost as the adhesions detach, and there is also the problem of lubricant evaporation. When the lubricant is exhausted, the non-adhesion properties of the surface will also fail.

[0004] Although anti-adhesion technology has made some progress, the preparation process of non-adhesion coatings still faces the following challenges: (1) Substrate limitations. For example, LLS relies on active sites on the surface of the substrate and requires pretreatment of the substrate. In order to accelerate the preparation of the coating, high temperature and acid or base catalysis are often required, which will cause corrosion of the metal substrate. (2) The preparation process is complex. For example, traditional super-hydrophobic surfaces often require secondary modification with low surface energy molecules to achieve the super-hydrophobic effect. For example, the structures of Re-entrant and Doble Re-entrant are complex, and the preparation process is cumbersome and difficult to achieve rapid preparation. For example, LIS requires two stages: structure forming and liquid infusion. (3) Harsh preparation conditions: For example, the use of chemical modification strategies often requires specific conditions, such as high temperature, vacuum environment, ultraviolet light irradiation, etc. (4) Long preparation time: For example, the immersion method for preparing LLS requires 12 hours or even 48 hours to complete the preparation of molecular brush coatings. (5) Coating thickness is relatively large: Except for LLS, which can achieve the preparation of non-adhesive coatings with nanometer thickness, it is difficult to achieve the preparation of nano-anti-adhesive coatings with existing methods, and the large coating thickness will make it impossible to apply it in certain precision fields. Therefore, if a preparation technology for anti-adhesive nano-coatings that is not restricted by substrates, has a simple preparation process and mild preparation conditions can be developed, it will be of great significance to extend the service life and safety of components, improve energy utilization, expand applications in precision fields, and reduce risks! Summary of the invention

[0005] In view of the above problems existing in the existing preparation process of non-adhesion coating, the present invention provides a method for preparing anti-adhesion nanocoating based on molecular brush grafting technology, so as to achieve simple and gentle preparation of anti-adhesion coating with nanometer thickness without being restricted by substrate.

[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology comprises the following steps:

[0008] (1) dissolving an anti-adhesion polymer in an organic solvent to obtain an anti-adhesion polymer solution; the preparation method of the anti-adhesion polymer is as follows:

[0009] Under stirring and protective gas protection, the adhesive solution is added dropwise to the organic silicon molecule solution, the molar ratio of the organic silicon molecule to the adhesive is controlled to be 1: (0.05-5), and the mixture is fully reacted at 0-100° C., unreacted raw materials and solvents are removed, and the mixture is dried to obtain an anti-adhesion polymer; the adhesive is a compound having a hydroxyl group and an amine group on a benzene ring;

[0010] (2) The anti-adhesion polymer solution is coated on a clean, dry substrate, and the anti-adhesion polymer is grafted onto the surface of the substrate through hydrogen bonding, complexation and π-π bonding. After the organic solvent is completely evaporated, the anti-adhesion polymer that is not stably bonded to the substrate is washed away, thereby forming an anti-adhesion nano-coating on the surface of the substrate.

[0011] In the above technical solution, the organic silicon molecule is R1-Si(CH 3 ) 2 -O-Si(CH 3 ) 2 -R1, R2-Si(CH 3 ) 2 -O-Si-(CH 3 ) 3 , H 2 N(CH 2 ) 3 Si[O(CH 2 ) n (CH 3 ) 3 ] 3 Or poly[dimethylsiloxane-co-(3-aminopropyl)methylsiloxane], wherein R1 is -(CH 2 ) 3 NH 2 、-OH、-(CH 2 ) 3 COOH or -CH(O)CH-, wherein R2 is -(CH 2 ) 3 O(CH 2 ) 2 OH, -(CH 2 ) 3 COOH or -(CH 2 ) 3 OCH 2 CH(O)CH).

[0012] Furthermore, in the above technical solution, the H 2 N(CH 2 ) 3 Si[O(CH 2 ) n (CH 3 ) 3 ] 3 Where n=0 or 1.

[0013] In the above technical solution, the adhesive includes any one of dopamine hydrochloride, 6-hydroxydopamine and 3-hydroxy-4-methoxyphenethylamine.

[0014] In the above technical solution, the organic silicon molecule solution is formed by dissolving organic silicon molecules in dichloromethane, and the concentration of the organic silicon molecule solution is preferably 0.01-0.2 mmol / mL; the adhesive solution is formed by dissolving an adhesive in N,N-dimethylformamide, and the concentration of the adhesive solution is preferably 0.01-1 mmol / mL. The adhesive solution is preferably prepared using N,N-dimethylformamide from which oxygen has been removed; before the adhesive solution is added dropwise to the organic silicon molecule solution, it is preferably to remove oxygen from the organic silicon molecule solution.

[0015] In the above technical solution, in step (1), when preparing the anti-adhesion polymer, a chain extender solution can also be added to the organosilicon molecule solution. That is, in step (1), when preparing the anti-adhesion polymer, the adhesive solution and the chain extender solution are added to the organosilicon molecule solution under stirring and protective gas protection, and fully reacted at 0-100°C, unreacted raw materials and solvents are removed, and dried to obtain the anti-adhesion polymer. Preferably, the molar ratio of the organosilicon molecule to the chain extender is controlled to be 1:(1-5).

[0016] In the above technical solution, whether to use a chain extender depends mainly on the specific structure of the organic silicon molecule used. When the organic silicon molecule is R2-Si(CH 3 ) 2 -O-Si-(CH 3 ) 3 When the silicone molecule is H 2 N(CH 2 ) 3 Si[O(CH 2 ) n (CH 3 ) 3 ] 3 or poly[dimethylsiloxane-co-(3-aminopropyl)methylsiloxane], a chain extender is required; when the silicone molecule is R1-Si(CH 3 ) 2 -O-Si(CH 3 ) 2 -R1, a chain extender may be used or not. In practical applications, whether to add a chain extender can be determined based on the structure of the organosilicon molecule and the actual application requirements.

[0017] In the above technical scheme, the chain extender is a commonly used chain extender in the preparation of silicone polymers in the prior art. For example, feasible chain extenders include one or more combinations of 4,4′-methylenebis(phenyl isocyanate), 4,4′-diisocyanate dicyclohexylmethane D, isocycloheximide, isophorone diisocyanate, and toluene diisocyanate.

[0018] In the above technical solution, the chain extender solution is formed by dissolving the chain extender in N,N-dimethylformamide, and the concentration of the chain extender solution is preferably 0.1-1 mmol / mL; the chain extender solution is preferably prepared using N,N-dimethylformamide from which oxygen has been removed.

[0019] In the above technical solution, the protective gas is a non-reactive gas that does not react with the adhesive / silicone molecule system and the adhesive / silicone molecule / chain extender system during the preparation of the anti-adhesion polymer. The protective gas can be an inert gas or nitrogen.

[0020] In the above technical solution, in step (1), when preparing the anti-adhesion polymer, a catalyst for promoting the synthesis of the organosilicon polymer can also be added to the organosilicon molecule solution, wherein the catalyst includes at least one of triethylamine, 4-N,N-dimethylpyridine, trimethylamine and dibutyltin dilaurate. Generally, the amount of catalyst added should be such that the molar ratio of the catalyst to the organosilicon molecule is 1:(2-3).

[0021] In the above technical solution, in step (1) when preparing the anti-adhesion polymer, the reaction time is preferably controlled to be 4 to 8 hours at 0 to 100°C.

[0022] In the above technical solution, in the anti-adhesion polymer solution of step (1), the concentration of the anti-adhesion polymer is preferably 5 to 100 μg / mL.

[0023] In the above technical solution, the coating method in step (2) includes spraying, brushing or dipping.

[0024] In the above technical solution, when the anti-adhesion polymer solution is applied to a clean and dry substrate in step (2), the anti-adhesion polymer solution is controlled to completely cover the portion of the clean and dry substrate where the anti-adhesion nano-coating is to be prepared. For example, when the coating method is spraying or brushing, the anti-adhesion polymer solution is sprayed or brushed onto the portion of the clean and dry substrate where the anti-adhesion nano-coating is to be prepared, so that the anti-adhesion polymer solution completely covers the portion of the anti-adhesion nano-coating to be prepared. For another example, when the coating method is immersion, the portion of the clean and dry substrate where the anti-adhesion nano-coating is to be prepared is completely immersed in the anti-adhesion polymer solution for 5 to 60 seconds.

[0025] In the above technical solution, the substrate is an organic material substrate, an inorganic material substrate or a metal substrate. For example, the material of the substrate can be aluminum, copper, stainless steel, gold, silicon, glass, polyurethane, etc.

[0026] In the above technical solution, the thickness of the anti-adhesion nano-coating formed on the surface of the substrate in step (2) is related to the molecular weight of the anti-adhesion polymer, but has nothing to do with other factors. The thickness of the anti-adhesion nano-coating is at the nanometer level, and the thickness of the coating is usually not more than 1000nm. The specific coating thickness can be determined according to actual application requirements. Furthermore, the thickness of the coating is generally between 20 and 200nm. For example, the thickness of the coating can be between 20 and 50nm.

[0027] In the above technical solution, the clean and dry substrate refers to the substrate that is ultrasonically cleaned with deionized water, ethanol and acetone in sequence to remove organic pollutants and solid particles on the surface of the substrate, and then dried.

[0028] In the above technical solution, when using deionized water, ethanol and acetone to ultrasonically clean the substrate, it is preferred to control the ultrasonic cleaning time to be 10 to 300 seconds.

[0029] In the above technical solution, in step (2), acetone or toluene can be used to clean and remove the anti-adhesion polymer that is not stably bonded to the substrate.

[0030] The present invention is confirmed by experiments:

[0031] The thickness of the anti-adhesion coating prepared by the method of the present invention is at the nanometer level, which can effectively improve the anti-adhesion effect of the substrate without affecting the surface morphology and light transmittance of the substrate. The anti-adhesion nano coating prepared by the method of the present invention has excellent stability and still maintains excellent liquid repellency after long-term immersion in organic solvents. The method of the present invention is not limited by the material of the substrate, and the preparation of the anti-adhesion nano coating can be achieved on organic substrates and inorganic substrates, such as aluminum, copper, stainless steel, gold, silicon, glass, polyurethane and other substrates. The method of the present invention achieves rapid preparation of the anti-adhesion nano coating through simple processes, such as spraying, brushing and soaking.

[0032] Compared with the prior art, the technical solution of the present invention can produce the following beneficial technical effects:

[0033] 1. The present invention provides a method for preparing an anti-adhesion nano coating based on molecular brush grafting technology, using a phenol-terminated organic silicon polymer as an anti-adhesion polymer, applying an anti-adhesion polymer solution on a clean, dry substrate, and grafting the anti-adhesion polymer on the surface of the substrate through hydrogen bonding, complexation and π-π bonding. After the organic solvent is completely volatilized, the anti-adhesion polymer that is not stably bonded to the substrate is washed and removed, that is, an anti-adhesion nano coating is formed on the surface of the substrate. The method of the present invention is not limited by the substrate, the preparation process is simple, the required process time is short, the preparation conditions are mild, and the thickness of the prepared coating is at the nanometer level, which can well solve the problems of the existing non-adhesion coating preparation method being limited to a specific substrate, the preparation process is complex, and the process conditions are harsh.

[0034] 2. The method of the present invention has low requirements on instruments, reagents and process conditions, does not require special instruments and expensive equipment, and can achieve the preparation of anti-adhesion nanocoatings under conventional operating conditions. Therefore, the present invention is suitable for promotion and application under existing simple process conditions and is easy to realize industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is the H-NMR spectrum of the anti-adhesion polymer prepared in Example 1.

[0036] Figure 2 These are the light transmittance test results of the glass substrate in Example 1 before and after modification of the anti-adhesion nanocoating.

[0037] Figure 3 These are the ice shear force test results of the glass substrate in Example 1 before and after being modified with the anti-adhesion nanocoating.

[0038] Figure 4 This is the liquid repellency test result of the coated aluminum substrate in Example 2 after being immersed in toluene for 24 hours.

[0039] Figure 5 304 stainless steel substrate before and after being modified with the anti-adhesion nano coating in Example 3.

[0040] Figure 6 These are the water drop contact angle test results of the 316 stainless steel substrate in Example 4 before and after being modified with the anti-adhesion nanocoating.

[0041] Figure 7 These are the coating thickness test results of the silicon substrate in Example 5 before and after modification of the anti-adhesion nanocoating.

[0042] Figure 8 These are atomic force microscope images of the silicon substrate in Example 6 before and after being modified with the anti-adhesion nanocoating.

[0043] Fig. 9 This is the Fourier transform infrared spectrum of the silicon substrate after being modified with the anti-adhesion nano coating in Example 6.

[0044] Fig.10 These are the test results of the liquid repellency of the polyurethane substrate in Example 7 before and after modification with the anti-adhesion nanocoating.

[0045] Fig.11 This is the stability test result of the anti-adhesion nano-coating on the gold substrate in Example 8. DETAILED DESCRIPTION

[0046] The following examples further illustrate the method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology provided by the present invention. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art can make some non-essential improvements and adjustments to the present invention according to the above invention content and implement them specifically, which still falls within the scope of protection of the present invention.

[0047] Example 1

[0048] In this embodiment, a method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology is provided, and the steps are as follows:

[0049] (1) Preparation of anti-adhesion polymers

[0050] ① The organic silicon molecule R1-Si(CH 3 ) 2 -O-Si(CH 3 ) 2 -R1(where R1 is -(CH 2 ) 3 NH 2 , and the organosilicon molecule is denoted as NH 2 -PDMS-NH 2 ) was dissolved in dichloromethane to obtain an organosilicon molecular solution with a concentration of 0.05 mmol / mL. The organosilicon molecular solution was placed in a three-necked round-bottom flask, and nitrogen was bubbled for 10 minutes to expel the air in the organosilicon molecular solution. At the same time, a magnetic stirrer was used to stir the organosilicon molecular solution.

[0051] Nitrogen was bubbled into N,N-dimethylformamide (DMF) for 10 min to expel the air therein, and the chain extender 4,4′-methylenebis(phenyl isocyanate) (MDI) was dissolved in DMF to obtain a 0.33 mmol / mL MDI solution. Nitrogen was bubbled into DMF for 10 min to expel the air therein, and then dopamine hydrochloride (DOPA) was dissolved in DMF to obtain a 0.0167 mmol / L dopamine hydrochloride solution.

[0052] ② Under stirring, nitrogen protection and ice bath conditions, the MDI solution is added dropwise to a three-necked round-bottom flask containing a silicone molecular solution, and then the dopamine hydrochloride solution is added dropwise to the three-necked round-bottom flask. After the addition is completed, the reaction is carried out under stirring, nitrogen protection and ice bath conditions for 4 hours. The obtained reaction product is repeatedly washed with deionized water, then dried at 30°C using a vacuum rotary evaporator, and then dried in an oven to obtain an anti-adhesion polymer.

[0053] In this step, the amounts of the organosilicon molecule solution, the MDI solution and the dopamine hydrochloride solution are controlled so that the molar ratio of the organosilicon molecule, the MDI and the dopamine hydrochloride is 1:1:0.05.

[0054] The structural formula of the phenol-terminated organosilicon polymer prepared in this step is as follows:

[0055]

[0056] The NMR hydrogen spectrum of the anti-adhesion polymer prepared in this step is as follows Figure 1 As shown, Figure 1 Among them, d (δ3.18ppm), e (δ1.56ppm), f (δ0.6ppm), g (δ0.25ppm) and h (δ0.13ppm) belong to the organic silicon molecule NH 2 -PDMS-NH 2 , a (δ7.36ppm), b (δ7.03ppm) and c (δ3.8ppm) belong to the chain extender MDI, i, j and k (δ6.72ppm) belong to DOPA, which indicates that DOPA, MDI and NH 2 -PDMS-NH 2 participated in the reaction, and the integral ratio of MDI and DOPA was 25:1.

[0057] (2) The anti-adhesion polymer is dissolved in acetone to obtain an anti-adhesion polymer solution with a concentration of 5 μg / mL.

[0058] (3) The glass substrate was ultrasonically cleaned with deionized water, ethanol, and acetone in sequence to remove organic pollutants and solid particles on the surface of the glass substrate, and then N 2 Blow dry to get a clean, dry glass substrate.

[0059] The anti-adhesion polymer solution is sprayed on a clean and dry glass substrate to completely cover the glass substrate. The anti-adhesion polymer is grafted onto the surface of the glass substrate through hydrogen bonding, complexation and π-π bonding. After the acetone is completely volatilized, toluene is used to rinse and remove the anti-adhesion polymer that is not stably bonded to the glass substrate, thereby forming an anti-adhesion nano coating on the surface of the glass substrate.

[0060] The glass substrate used in this embodiment and the glass substrate with an anti-adhesion nano coating formed on the surface were tested for light transmittance. The results are as follows: Figure 2 As shown by Figure 2 It can be seen that the transmittance curves of the glass substrate and the glass substrate with the anti-adhesion nanocoating formed on the surface are basically overlapped, that is, after the anti-adhesion nanocoating is modified, the transmittance is almost unchanged, indicating that the formed anti-adhesion nanocoating is very thin.

[0061] The ice shear force of the glass substrate used in this embodiment and the glass substrate with an anti-adhesion nano coating formed on the surface were measured by an ice shear force device. The results are as follows: Figure 3 As shown in Figures (a) and (b). Figure 3 It can be seen that the ice shear force of the glass substrate used in this embodiment is 57.7N, and the ice shear force of the glass substrate with an anti-adhesion nano-coating formed on the surface is 5.6N. It can be seen that the surface of the glass substrate with an anti-adhesion nano-coating formed on the surface exhibits extremely low adhesion to ice, showing ice-phobicity.

[0062] Example 2

[0063] In this embodiment, a method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology is provided, and the steps are as follows:

[0064] (1) Preparation of anti-adhesion polymers

[0065] ① The organic silicon molecule R1-Si(CH 3 ) 2 -O-Si(CH 3 ) 2 -R1(where R1 is -(CH 2 ) 3 COOH) was dissolved in dichloromethane to obtain an organosilicon molecular solution with a concentration of 0.03 mmol / mL. The organosilicon molecular solution was placed in a three-necked round-bottom flask, and nitrogen was bubbled into it for 5 minutes to expel the air from the organosilicon molecular solution. At the same time, a magnetic stirrer was used to stir the organosilicon molecular solution.

[0066] Nitrogen was bubbled into DMF for 5 min to expel the air therein, and then the chain extender 4,4′-diisocyanate dicyclohexylmethane (HMDI) was dissolved in DMF to obtain an HMDI solution with an HMDI concentration of 1 mmol / mL. Nitrogen was bubbled into DMF for 5 min to expel the air therein, and then dopamine hydrochloride was dissolved in DMF to obtain a 0.1 mmol / L dopamine hydrochloride solution.

[0067] ② Add the HMDI solution dropwise into a three-necked round-bottom flask containing the organosilicon molecule solution, and add the dopamine hydrochloride solution dropwise into the three-necked round-bottom flask. After the addition is complete, add the catalyst triethylamine, and react for 6 hours under nitrogen protection and condensation reflux at 90°C. The obtained reaction product is repeatedly washed with deionized water, and then dried at 60°C using a vacuum rotary evaporator, and then dried in an oven to obtain an anti-adhesion polymer.

[0068] In this step, the amounts of the organosilicon molecule solution, the HMDI solution and the dopamine hydrochloride solution are controlled so that the molar ratio of the organosilicon molecules, HMDI and dopamine hydrochloride is 1:1:0.1; and the amount of triethylamine added is controlled so that the molar ratio of triethylamine to the organosilicon molecules is 1:1.5.

[0069] (2) The anti-adhesion polymer is dissolved in acetone to obtain an anti-adhesion polymer solution with a concentration of 10 μg / mL.

[0070] (3) The aluminum substrate was ultrasonically cleaned with deionized water, ethanol, and acetone in sequence to remove organic pollutants and solid particles on the surface of the aluminum substrate, and then N 2 Blow dry to get a clean, dry aluminum substrate.

[0071] The anti-adhesion polymer solution is sprayed on a clean and dry aluminum substrate to completely cover the aluminum substrate. The anti-adhesion polymer is grafted onto the surface of the aluminum substrate through hydrogen bonding, complexation and π-π bonding. After the acetone is completely volatilized, the anti-adhesion polymer that is not stably bonded to the aluminum substrate is removed by acetone washing, thereby forming an anti-adhesion nano-coating on the surface of the aluminum substrate.

[0072] The aluminum substrate with the anti-adhesion nano coating formed on the surface (coated aluminum substrate) was immersed in toluene for 24 hours, and the liquid repellency of the anti-adhesion nano coating on the surface was tested. 5 μL of hexadecane was dropped on the coated aluminum substrate after immersion, and the movement of the hexadecane droplet on the coated aluminum substrate was observed and recorded using a camera. The results are shown in FIG. Figure 4 As shown. Figure 4 It can be seen that the hexadecane droplets can slide smoothly on the coated aluminum substrate without any traces of droplet retention, which on the one hand shows that the coating has a good anti-fouling effect, and on the other hand shows that the coating has excellent stability.

[0073] Example 3

[0074] In this embodiment, a method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology is provided, and the steps are as follows:

[0075] (1) Preparation of anti-adhesion polymers

[0076] ① The organic silicon molecule R1-Si(CH 3 ) 2 -O-Si(CH 3 ) 2 -R1 (wherein R1 is -OH) was dissolved in dichloromethane to obtain an organosilicon molecular solution with a concentration of 0.013 mmol / mL. The organosilicon molecular solution was placed in a three-necked round-bottom flask, and nitrogen was bubbled for 15 minutes to expel the air in the organosilicon molecular solution, and a magnetic stirrer was used to stir the organosilicon molecular solution.

[0077] Nitrogen was bubbled into DMF for 15 minutes to expel the air therein, and then the chain extender 4,4′-methylenebis(phenyl isocyanate) (MDI) and toluene diisocyanate (TDI) were dissolved in DMF to obtain an MDI-TDI mixed solution with an MDI concentration of 0.2 mmol / mL and a TDI concentration of 0.2 mmol / mL. Nitrogen was bubbled into DMF for 15 minutes to expel the air therein, and then 6-hydroxydopamine was dissolved in DMF to obtain a 0.04 mmol / L 6-hydroxydopamine solution.

[0078] ② Add the MDI-TDI mixed solution dropwise into a three-necked round-bottom flask containing a silicone molecular solution, and then add the 6-hydroxydopamine solution dropwise into the three-necked round-bottom flask. After the addition is complete, add catalyst triethylamine and dibutyltin dilaurate, and react for 8 hours under nitrogen protection and condensation reflux at 100°C. The obtained reaction product is repeatedly washed with deionized water, and then dried at 50°C using a vacuum rotary evaporator, and then dried in an oven to obtain an anti-adhesion polymer.

[0079] In this step, the amounts of the organosilicon molecule solution, the MDI-TDI mixed solution and the 6-hydroxydopamine solution are controlled so that the molar ratio of the organosilicon molecules, MDI, TDI and 6-hydroxydopamine is 2:1:1:0.2; and the amounts of triethylamine and dibutyltin dilaurate are controlled so that the molar ratio of triethylamine, dibutyltin dilaurate and the organosilicon molecules is 1:1:1.

[0080] (2) The anti-adhesion polymer is dissolved in acetone to obtain an anti-adhesion polymer solution with a concentration of 30 μg / mL.

[0081] (3) Ultrasonic cleaning of the 304 stainless steel substrate was performed using deionized water, ethanol, and acetone in sequence to remove organic pollutants and solid particles on the surface of the 304 stainless steel substrate. 2 Blow dry to get a clean and dry 304 stainless steel base.

[0082] The anti-adhesion polymer solution is brushed onto a clean and dry 304 stainless steel substrate to completely cover the 304 stainless steel substrate. The anti-adhesion polymer is grafted onto the surface of the 304 stainless steel substrate through hydrogen bonding, complexation and π-π bonding. After the acetone is completely volatilized, the anti-adhesion polymer that is not stably bonded to the 304 stainless steel substrate is removed by acetone washing, thereby forming an anti-adhesion nano coating on the surface of the 304 stainless steel substrate.

[0083] The 304 stainless steel substrate used in this embodiment and the 304 stainless steel substrate with an anti-adhesion nano coating formed on the surface were tested by scanning electron microscope. The results are as follows: Figure 5 As shown in Figures (a) and (b), Figure 5 It can be seen that after the surface of the 304 stainless steel substrate is modified with the anti-adhesion nano coating, no corrosion spots appear on the 304 stainless steel substrate, indicating that the anti-adhesion nano coating is suitable for modifying the surface of the metal substrate.

[0084] Example 4

[0085] In this embodiment, a method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology is provided, and the steps are as follows:

[0086] (1) Preparation of anti-adhesion polymers

[0087] ① The organic silicon molecule R1-Si(CH 3 ) 2 -O-Si(CH 3 ) 2 -R1 (wherein R1 is -CH(O)CH-) was dissolved in dichloromethane to obtain an organosilicon molecular solution with a concentration of 0.1 mmol / mL. The organosilicon molecular solution was placed in a three-necked round-bottom flask, and nitrogen was bubbled for 5 minutes to expel the air in the organosilicon molecular solution, and a magnetic stirrer was used to stir the organosilicon molecular solution.

[0088] Nitrogen was bubbled into DMF for 5 minutes to expel the air therein, and then the chain extender isophorone diisocyanate (IPDI) and 4,4′-methylenebis(phenyl isocyanate) (MDI) were dissolved in DMF to obtain an IPDI-MDI mixed solution with an IPDI and MDI concentration of 0.167 mmol / mL. Nitrogen was bubbled into DMF for 5 minutes to expel the air therein, and then 3-hydroxy-4-methoxyphenethylamine was dissolved in DMF to obtain a 0.33 mmol / L 3-hydroxy-4-methoxyphenethylamine solution.

[0089] ② Add the IPDI-MDI mixed solution dropwise to a three-necked round-bottom flask containing a silicone molecular solution, and add the 3-hydroxy-4-methoxyphenylethylamine solution dropwise to the three-necked round-bottom flask. After the addition is complete, add the catalyst triethylamine, and react for 8 hours under nitrogen protection and condensation reflux at 80°C. The resulting reaction product is repeatedly washed with deionized water, and then dried at 45°C using a vacuum rotary evaporator, and then dried in an oven to obtain an anti-adhesion polymer.

[0090] In this step, the amounts of the organosilicon molecule solution, the IPDI-MDI mixed solution and the 3-hydroxy-4-methoxyphenethylamine solution are controlled so that the molar ratio of the organosilicon molecules, IPDI, MDI and 3-hydroxy-4-methoxyphenethylamine is 1:0.5:0.5:0.6; and the amount of triethylamine added is controlled so that the molar ratio of triethylamine to the organosilicon molecules is 1:2.5.

[0091] (2) The anti-adhesion polymer is dissolved in acetone to obtain an anti-adhesion polymer solution with a concentration of 10 μg / mL.

[0092] (3) Deionized water, ethanol, and acetone were used to ultrasonically clean the 316 stainless steel substrate to remove organic pollutants and solid particles on the surface of the 316 stainless steel substrate. 2 Blow dry to get a clean, dry 316 stainless steel base.

[0093] The anti-adhesion polymer solution is sprayed on a clean and dry 316 stainless steel substrate to completely cover the 316 stainless steel substrate. The anti-adhesion polymer is grafted onto the surface of the 316 stainless steel substrate through hydrogen bonding, complexation and π-π bonding. After the acetone is completely volatilized, the anti-adhesion polymer that is not stably bonded to the 316 stainless steel substrate is removed by acetone washing, thereby forming an anti-adhesion nano coating on the surface of the 316 stainless steel substrate.

[0094] The contact angle meter was used to characterize the wetting properties of the 316 stainless steel substrate and the 316 stainless steel substrate with an anti-adhesion nano coating formed on the surface. The results are as follows: Figure 6 As shown in Figures (a) and (b), Figure 6 It can be seen that the surface of the 316 stainless steel substrate is relatively hydrophilic, with a water droplet contact angle of 58.6°, while after the surface of the 304 stainless steel substrate is modified with an anti-adhesion nanocoating, the water droplet contact angle is 104.7°, showing a relatively hydrophobic state.

[0095] Example 5

[0096] In this embodiment, a method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology is provided, and the steps are as follows:

[0097] (1) The preparation method of the anti-adhesion polymer is the same as that of Example 4. The anti-adhesion polymer is dissolved in acetone to obtain an anti-adhesion polymer solution with a concentration of 50 μg / mL.

[0098] (2) The copper substrate was ultrasonically cleaned with deionized water, ethanol, and acetone in sequence to remove organic pollutants and solid particles on the surface of the copper substrate, and then N 2 Blow dry to get a clean, dry copper base.

[0099] A clean and dry copper substrate is immersed in an anti-adhesion polymer solution, and the immersion time is controlled to be 5 to 10 seconds. During the immersion process, the anti-adhesion polymer is grafted onto the surface of the copper substrate through hydrogen bonding, complexation and π-π bonding. After the immersion is completed, the copper substrate is taken out, and after the acetone is completely evaporated, toluene is used to rinse and remove the anti-adhesion polymer that is not stably bonded to the copper substrate, thereby forming an anti-adhesion nano coating on the surface of the copper substrate.

[0100] The coating thickness on the silicon substrate and the copper substrate with the anti-adhesion coating formed on the surface used in this embodiment was measured by ellipsometer. The results are as follows: Figure 7 As shown by Figure 7 It can be seen that the coating thickness on the copper substrate with the anti-adhesion coating formed on the surface is 21.65 nm.

[0101] Example 6

[0102] In this embodiment, a method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology is provided, and the steps are as follows:

[0103] (1) Preparation of anti-adhesion polymers

[0104] ① Dissolve the organosilicon molecule poly[dimethylsiloxane-co-(3-aminopropyl)methylsiloxane] with a molecular weight of 209.39 g / mol in dichloromethane to obtain an organosilicon molecule solution with a concentration of 0.1 mmol / mL. Place the organosilicon molecule solution in a three-necked round-bottom flask, introduce nitrogen gas for 15 minutes to expel the air in the organosilicon molecule solution, and use a magnetic stirrer to stir the organosilicon molecule solution.

[0105] Nitrogen was bubbled into DMF for 15 min to expel the air therein, and then the chain extender 4,4′-methylenebis(phenyl isocyanate) (MDI) was dissolved in DMF to obtain a 1 mmol / mL MDI solution. Nitrogen was bubbled into DMF for 15 min to expel the air therein, and then dopamine hydrochloride was dissolved in DMF to obtain a 1 mmol / L dopamine hydrochloride solution.

[0106] ② Under stirring, nitrogen protection and ice bath conditions, the MDI solution is added dropwise to a three-necked round-bottom flask containing the silicone molecular solution, and then the dopamine hydrochloride solution is added dropwise to the three-necked round-bottom flask. After the addition is completed, the reaction is carried out under stirring, nitrogen protection and ice bath conditions for 5 hours. The obtained reaction product is repeatedly washed with deionized water, then dried at 50°C using a vacuum rotary evaporator, and then dried in an oven to obtain an anti-adhesion polymer.

[0107] In this step, the amounts of the organosilicon molecule solution, the MDI solution and the dopamine hydrochloride solution are controlled so that the molar ratio of the organosilicon molecule, the MDI and the dopamine hydrochloride is 1:5:5.

[0108] (2) The anti-adhesion polymer is dissolved in acetone to obtain an anti-adhesion polymer solution with a concentration of 50 μg / mL.

[0109] (3) The silicon substrate was ultrasonically cleaned with deionized water, ethanol, and acetone in sequence to remove organic pollutants and solid particles on the surface of the silicon substrate, and then N 2 Blow dry to get a clean, dry silicone base.

[0110] The anti-adhesion polymer solution is brushed onto a clean and dry silicon substrate to completely cover the silicon substrate. The anti-adhesion polymer is grafted onto the surface of the silicon substrate through hydrogen bonding, complexation and π-π bonding. After the acetone is completely evaporated, toluene is used to rinse and remove the anti-adhesion polymer that is not stably bonded to the silicon substrate, thereby forming an anti-adhesion nano-coating on the surface of the silicon substrate.

[0111] The silicon substrate used in this embodiment and the silicon substrate with an anti-adhesion nano-coating formed on the surface were tested by atomic force microscopy. The results are as follows: Figure 8 As shown in Figures (a) and (b), Figure 8 It can be seen that the surface roughness Ra of the silicon substrate is 0.52nm, and the surface roughness Ra of the silicon substrate modified with the anti-adhesion nano-coating is 0.63nm. The difference in the surface roughness of the two is not obvious, and both are smooth surfaces. The silicon substrate with the anti-adhesion nano-coating formed on the surface was tested by Fourier infrared spectroscopy, and the results are as follows Fig. 9 As shown, Fig. 9 The coating contains Si-O-Si, Si-CH3 、Si-(CH 3 ) 2 and C-H bonds.

[0112] Example 7

[0113] In this embodiment, a method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology is provided, and the steps are as follows:

[0114] (1) Preparation of anti-adhesion polymers

[0115] ① Add the organic silicon molecule (3-aminopropyl) triethoxysilane (i.e. H 2 N(CH 2 ) 3 Si(OC 2 H 5 ) 3 ) was dissolved in dichloromethane to obtain an organosilicon molecular solution with a concentration of 0.2 mmol / mL. The organosilicon molecular solution was placed in a three-necked round-bottom flask, and nitrogen was bubbled in for 10 minutes to expel the air in the organosilicon molecular solution. At the same time, a magnetic stirrer was used to stir the organosilicon molecular solution.

[0116] Nitrogen was bubbled into DMF for 10 min to expel the air therein, and then the chain extender isophorone diisocyanate (IPDI) was dissolved in DMF to obtain an IPDI solution with a concentration of 1 mmol / mL. Nitrogen was bubbled into DMF for 10 min to expel the air therein, and then dopamine hydrochloride was dissolved in DMF to obtain a 0.5 mmol / L dopamine hydrochloride solution.

[0117] ② Under stirring, nitrogen protection and ice bath conditions, the IPDI solution is added dropwise to a three-necked round-bottom flask containing an organosilicon molecule solution, and then the dopamine hydrochloride solution is added dropwise to the three-necked round-bottom flask. After the addition is completed, the reaction is carried out under stirring, nitrogen protection and ice bath conditions for 6 hours. The obtained reaction product is repeatedly washed with deionized water, then dried at 35°C using a vacuum rotary evaporator, and then dried in an oven to obtain an anti-adhesion polymer.

[0118] In this step, the amounts of the organosilicon molecule solution, the IPDI solution and the dopamine hydrochloride solution are controlled so that the molar ratio of the organosilicon molecule, the IPDI and the dopamine hydrochloride is 1:1:0.5.

[0119] (2) The anti-adhesion polymer is dissolved in acetone to obtain an anti-adhesion polymer solution with a concentration of 10 μg / mL.

[0120] (2) Ultrasonic cleaning of the tubular polyurethane substrate was performed using deionized water, ethanol, and acetone in sequence to remove organic pollutants and solid particles on the surface of the polyurethane substrate, and then N 2 Blow dry to get a clean, dry polyurethane base.

[0121] A clean and dry polyurethane substrate is immersed in the anti-adhesion polymer solution, and the immersion time is controlled to be 5 to 10 seconds. During the immersion process, the anti-adhesion polymer is grafted on the surface of the polyurethane substrate through the effects including hydrogen bonding, complexation and π-π bonding. After the immersion is completed, the polyurethane substrate is taken out, and after the acetone is completely evaporated, the anti-adhesion polymer that is not stably combined with the polyurethane substrate is washed with acetone to remove, that is, an anti-adhesion nano coating is formed on the surface of the polyurethane substrate.

[0122] The polyurethane substrate used in this embodiment and the polyurethane substrate with an anti-adhesion nano-coating formed on the surface (coated polyurethane substrate) were tested for liquid repellency. 5 μL of hexadecane was dropped on the polyurethane substrate and the coated polyurethane substrate, respectively, and the movement of the hexadecane droplets on the surfaces of the two was observed and recorded using a camera. The results are shown in FIG. Fig.10 As shown. Fig.10 As shown in Figure (a), the surface of the polyurethane substrate is lipophilic, and the hexadecane droplets leave a large number of marks on the tube wall. Fig.10 As shown in Figure (b), the hexadecane droplet can slide smoothly on the coated polyurethane substrate, and the shape of the droplet remains basically unchanged, showing an oleophobic state.

[0123] Example 8

[0124] In this embodiment, a method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology is provided, and the steps are as follows:

[0125] (1) Preparation of anti-adhesion polymers

[0126] ① The organic silicon molecule R1-Si(CH3)2-O-Si(CH3)2-R1 (where R1 is -(CH 2 ) 3 COOH) was dissolved in dichloromethane to obtain an organosilicon molecular solution with a concentration of 0.03 mmol / mL. The organosilicon molecular solution was placed in a three-necked round-bottom flask, and nitrogen was bubbled for 5 minutes to expel the air in the organosilicon molecular solution. At the same time, a magnetic stirrer was used to stir the organosilicon molecular solution.

[0127] Nitrogen gas was bubbled into DMF for 5 min to expel the air therein, and then dopamine hydrochloride was dissolved in DMF to obtain a 0.06 mmol / L dopamine hydrochloride solution.

[0128] ② Add the dopamine hydrochloride solution dropwise to the three-necked round-bottom flask. After the addition is complete, add the catalyst triethylamine, and react for 6 hours under nitrogen protection and condensation reflux at 90°C. The obtained reaction product is repeatedly washed with deionized water, then dried with a vacuum rotary evaporator at 60°C, and then dried in an oven to obtain the final product, phenol-terminated silicone polymer.

[0129] In this step, the dosage of the organosilicon molecule solution and the dopamine hydrochloride solution is controlled so that the molar ratio of the organosilicon molecule to the dopamine hydrochloride is 1:2; and the amount of triethylamine added is controlled so that the molar ratio of triethylamine to the organosilicon molecule is 1:1.5.

[0130] (2) The anti-adhesion polymer is dissolved in acetone to obtain an anti-adhesion polymer solution with a concentration of 30 μg / mL.

[0131] (3) Ultrasonic cleaning of the gold substrate was performed using deionized water, ethanol, and acetone in sequence to remove organic pollutants and solid particles on the surface of the gold substrate. 2 Blow dry to get a clean, dry gold base.

[0132] The anti-adhesion polymer solution is brushed onto a clean and dry gold substrate to completely cover the gold substrate. The anti-adhesion polymer is grafted onto the surface of the gold substrate through hydrogen bonding, complexation and π-π bonding. After the acetone is completely volatilized, the anti-adhesion polymer that is not stably bonded to the gold substrate is washed away with acetone, thereby forming an anti-adhesion nano-coating on the surface of the gold substrate.

[0133] The stability of the coating on the gold substrate with anti-adhesion nanocoating formed on the surface was tested by quartz crystal microbalance. Fig.11 As shown by Fig.11 It can be seen that in the flowing sodium dodecyl sulfate solution, the frequency of the gold substrate hardly changes, indicating that the anti-adhesion polymer is firmly bonded to the surface of the gold substrate and exhibits excellent stability.

[0134] Example 9

[0135] In this embodiment, a method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology is provided, and the steps are as follows:

[0136] (1) Preparation of anti-adhesion polymers

[0137] ① The organic silicon molecule R2-Si(CH 3 ) 2 -O-Si-(CH 3 ) 3 (where R2 is -(CH 2 ) 3 OCH 2CH(O)CH) was dissolved in dichloromethane to obtain an organosilicon molecular solution with a concentration of 0.1 mmol / mL. The organosilicon molecular solution was placed in a three-necked round-bottom flask, and nitrogen was bubbled for 10 minutes to expel the air in the organosilicon molecular solution. At the same time, a magnetic stirrer was used to stir the organosilicon molecular solution.

[0138] Nitrogen gas was bubbled into DMF for 10 min to expel air therein, and then 6-hydroxydopamine was dissolved in DMF to obtain a 6-hydroxydopamine solution with a concentration of 0.67 mmol / mL.

[0139] ② Add the 6-hydroxydopamine solution dropwise into a three-necked round-bottom flask containing the organosilicon molecule solution. After the addition is complete, add the catalyst triethylamine and react for 8 hours under nitrogen protection and condensation reflux at 80°C. The resulting reaction product is repeatedly washed with deionized water, then dried using a vacuum rotary evaporator at 45°C, and then dried in an oven to obtain an anti-adhesion polymer.

[0140] In this step, the amount of the organic silicon molecule solution and the 6-hydroxydopamine solution is controlled so that the molar ratio of the organic silicon molecule to the 6-hydroxydopamine is 1:1; and the amount of triethylamine added is controlled so that the molar ratio of triethylamine to the organic silicon molecule is 1:1.5.

[0141] (2) The anti-adhesion polymer is dissolved in acetone to obtain an anti-adhesion polymer solution with a concentration of 100 μg / mL.

[0142] (3) The glass substrate was ultrasonically cleaned with deionized water, ethanol, and acetone in sequence to remove organic pollutants and solid particles on the surface of the glass substrate, and then N 2 Blow dry to get a clean, dry glass substrate.

[0143] The anti-adhesion polymer solution is sprayed on a clean and dry glass substrate to completely cover the glass substrate. The anti-adhesion polymer is grafted onto the surface of the glass substrate through hydrogen bonding, complexation and π-π bonding. After the acetone is completely volatilized, the anti-adhesion polymer that is not stably bonded to the glass substrate is washed away by acetone, thereby forming an anti-adhesion nano coating on the surface of the glass substrate.

[0144] Example 10

[0145] In this embodiment, a method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology is provided, and the steps are as follows:

[0146] (1) Preparation of anti-adhesion polymers

[0147] ① The organic silicon molecule R2-Si(CH 3 ) 2-O-Si-(CH 3 ) 3 (where R2 is -(CH 2 ) 3 COOH) was dissolved in dichloromethane to obtain an organosilicon molecular solution with a concentration of 0.1 mmol / mL. The organosilicon molecular solution was placed in a three-necked round-bottom flask, and nitrogen was bubbled in for 20 minutes to expel the air in the organosilicon molecular solution. At the same time, a magnetic stirrer was used to stir the organosilicon molecular solution.

[0148] Nitrogen gas was bubbled into DMF for 20 min to expel air therein, and then 3-hydroxy-4-methoxyphenethylamine was dissolved in DMF to obtain a 0.1 mmol / mL 3-hydroxy-4-methoxyphenethylamine solution.

[0149] ② Add the 3-hydroxy-4-methoxyphenylethylamine solution dropwise into a three-necked round-bottom flask containing the organosilicon molecule solution. After the addition is complete, add the catalyst 4-N,N-dimethylpyridine and react for 6 hours under nitrogen protection and condensation reflux at 60°C. The obtained reaction product is repeatedly washed with deionized water, then dried with a vacuum rotary evaporator at 45°C, and then dried in an oven to obtain an anti-adhesion polymer.

[0150] In this step, the amount of the organic silicon molecule solution and the 3-hydroxy-4-methoxyphenethylamine solution is controlled so that the molar ratio of the organic silicon molecule to the 3-hydroxy-4-methoxyphenethylamine is 1:1; and the amount of 4-N,N-dimethylpyridine added is controlled so that the molar ratio of 4-N,N-dimethylpyridine to the organic silicon molecule is 1:3.

[0151] (2) The anti-adhesion polymer is dissolved in acetone to obtain an anti-adhesion polymer solution with a concentration of 40 μg / mL.

[0152] (3) The glass substrate was ultrasonically cleaned with deionized water, ethanol, and acetone in sequence to remove organic pollutants and solid particles on the surface of the glass substrate, and then N 2 Blow dry to get a clean, dry glass substrate.

[0153] The anti-adhesion polymer solution is sprayed on a clean and dry glass substrate to completely cover the glass substrate. The anti-adhesion polymer is grafted onto the surface of the glass substrate through hydrogen bonding, complexation and π-π bonding. After the acetone is completely volatilized, the anti-adhesion polymer that is not stably bonded to the glass substrate is washed away by acetone, thereby forming an anti-adhesion nano coating on the surface of the glass substrate.

[0154] Embodiment 11

[0155] In this embodiment, a method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology is provided, and the steps are as follows:

[0156] (1) Preparation of anti-adhesion polymers

[0157] ① The organic silicon molecule R2-Si(CH 3 ) 2 -O-Si-(CH 3 ) 3 (where R2 is -(CH 2 ) 3 O(CH 2 ) 2 OH) was dissolved in dichloromethane to obtain an organosilicon molecular solution with a concentration of 0.03 mmol / mL. The organosilicon molecular solution was placed in a three-necked round-bottom flask, and nitrogen was bubbled in for 20 minutes to expel the air in the organosilicon molecules, while a magnetic stirrer was used to stir the organosilicon molecular solution.

[0158] Nitrogen gas was bubbled into DMF for 10 min to expel the air therein, and then dopamine hydrochloride was dissolved in DMF to obtain a 0.33 mmol / L dopamine hydrochloride solution.

[0159] ② Add the dopamine hydrochloride solution dropwise into a three-necked round-bottom flask containing the organosilicon molecule solution. After the addition is complete, add the catalyst triethylamine and react for 8 hours under nitrogen protection and condensation reflux at 80°C. The resulting reaction product is repeatedly washed with deionized water, then dried using a vacuum rotary evaporator at 40°C, and then dried in an oven to obtain an anti-adhesion polymer.

[0160] In this step, the dosage of the organosilicon molecule solution and the dopamine hydrochloride solution is controlled so that the molar ratio of the organosilicon molecule to the dopamine hydrochloride is 1:1, and the amount of triethylamine added is controlled so that the molar ratio of triethylamine to the organosilicon molecule is 1:1.

[0161] (2) The anti-adhesion polymer is dissolved in acetone to obtain an anti-adhesion polymer solution with a concentration of 30 μg / mL.

[0162] (3) The glass substrate was ultrasonically cleaned with deionized water, ethanol, and acetone in sequence to remove organic pollutants and solid particles on the surface of the glass substrate, and then N 2 Blow dry to get a clean, dry glass substrate.

[0163] The anti-adhesion polymer solution is sprayed on a clean and dry glass substrate to completely cover the glass substrate. The anti-adhesion polymer is grafted onto the surface of the glass substrate through hydrogen bonding, complexation and π-π bonding. After the acetone is completely volatilized, the anti-adhesion polymer that is not stably bonded to the glass substrate is washed away by acetone, thereby forming an anti-adhesion nano coating on the surface of the glass substrate.

Claims

1. A method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology, characterized in that: The following steps are involved: (1) dissolving an anti-adhesion polymer in an organic solvent to obtain an anti-adhesion polymer solution; the preparation method of the anti-adhesion polymer is as follows: Under stirring and protective gas protection, the adhesive solution is added dropwise to the organic silicon molecule solution, the molar ratio of the organic silicon molecule to the adhesive is controlled to be 1: (0.05-5), and the mixture is fully reacted at 0-100° C., unreacted raw materials and solvents are removed, and the mixture is dried to obtain an anti-adhesion polymer; the adhesive is a compound having a hydroxyl group and an amine group on a benzene ring; (2) The anti-adhesion polymer solution is coated on a clean, dry substrate, and the anti-adhesion polymer is grafted onto the surface of the substrate through hydrogen bonding, complexation and π-π bonding. After the organic solvent is completely evaporated, the anti-adhesion polymer that is not stably bonded to the substrate is washed away, thereby forming an anti-adhesion nano-coating on the surface of the substrate.

2. The method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology according to claim 1, characterized in that: The organic silicon molecule is R1-Si(CH3)2-O-Si(CH3)2-R1, R2-Si(CH3)2-O-Si-(CH3)3, H2N(CH2)3Si[O(CH2) n (CH3)3]3 or poly[dimethylsiloxane-co-(3-aminopropyl)methylsiloxane], wherein R1 is -(CH2)3NH2, -OH, -(CH2)3COOH or -CH(O)CH-, and R2 is -(CH2)3O(CH2)2OH, -(CH2)3COOH or -(CH2)3OCH2CH(O)CH).

3. The method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology according to claim 1, characterized in that: The adhesive includes any one of dopamine hydrochloride, 6-hydroxydopamine and 3-hydroxy-4-methoxyphenylethylamine.

4. The method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology according to claim 1, characterized in that: In step (1), when preparing the anti-adhesion polymer, a chain extender solution is also added dropwise to the organic silicon molecule solution, and the molar ratio of the organic silicon molecule to the chain extender is controlled to be 1:(1-5).

5. The method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology according to claim 1, characterized in that: In step (1), when preparing the anti-adhesion polymer, a catalyst is added to the organic silicon molecule solution, wherein the catalyst includes at least one of triethylamine, 4-N,N-dimethylpyridine, trimethylamine and dibutyltin dilaurate.

6. The method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology according to claim 1, characterized in that: In step (1), when preparing the anti-adhesion polymer, the reaction time is controlled at 0-100° C. to be 4-8 hours.

7. The method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology according to any one of claims 1 to 6, characterized in that: In the anti-adhesion polymer solution of step (1), the concentration of the anti-adhesion polymer is 5 to 100 μg / mL.

8. The method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology according to any one of claims 1 to 6, characterized in that: The coating method in step (2) includes spraying, brushing or dipping.

9. The method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology according to any one of claims 1 to 6, characterized in that: The substrate is an organic material substrate, an inorganic material substrate or a metal substrate.

10. The method for preparing an anti-adhesion nanocoating based on molecular brush grafting technology according to any one of claims 1 to 6, characterized in that: The thickness of the anti-adhesion nano-coating formed on the surface of the substrate in step (2) does not exceed 1000 nm.

Citation Information

Patent Citations

  • Self-repairing super-hydrophobic coating and preparation method thereof

    CN112778905A

  • Super-lubricating organic gel coating with self-adaptability and wear resistance and preparation method of super-lubricating organic gel coating

    CN115382741A

  • Anti-bioadhesion super-smooth surface and preparation method thereof

    CN116786383A

  • Multi-Functional Anti-Icing Hydrogel Materials and Methods for Controlling Ice Nucleation, Growth and Adhesion

    US20210261838A1

  • Polymer deposition and modification of membranes for fouling resistance

    WO2011005258A1