High temperature resistant acrylate adhesive

Through the two-component adhesive of the two-component preparation, the problems of insufficient strength and complex flammability of the adhesive at high temperature are solved, and the stability and conductivity of the adhesive at high temperature are achieved. It is suitable for various finishing processes .

CN118879207APending Publication Date: 2024-11-01ILLINOIS TOOL WORKS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410183950.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-02-14
Filing Date
2024-02-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing adhesives are insufficient after heating, have short working life and prolong the fixing time, making them difficult to adapt to various finishing processes, and are flammable and complex, affecting industrial processing.

Method used

Using two-component preparation, component A includes reactive methacrylate phosphate monomer, hydroxylated methacrylate monomer, free radical polymerization inhibitor, etc., component B includes impact modifier and polymerization accelerator , bonded to form an adhesive, has electrical conductivity and maintains stability at high temperatures.

Benefits of technology

It realizes that the adhesive maintains strength for a long time at high temperatures, reduces fixing time and increases working life, is suitable for various finishing processes, reduces flammability and exhaust gas, and enhances adhesion and conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004705164670000141
    Figure BDA0004705164670000141
  • Figure BDA0004705164670000151
    Figure BDA0004705164670000151
Patent Text Reader

Abstract

A method of applying an adhesive to a substrate is provided, the method comprising mixing together the ingredients of a two-component formulation of component A and component B. The component A comprises a reactive methacrylate phosphate monomer or oligomer, a methacrylate monomer, a high flash point (meth) acrylate monomer, a free radical polymerization inhibitor, an adhesion promoter, an impact modifier, a flexibilizer and a free radical polymerization initiator. The component B comprises an impact modifier, a flexibilizer and a polymerization accelerator. Component A and component B are combined together to form an adhesive mixture. The adhesive mixture is applied to a substrate. The invention also provides a preparation of the component A and the component B. A bonded structure is provided in which the resulting adhesive is located between the first substrate and the second substrate.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Related Applications

[0002] This application is a non-provisional application, which claims priority to U.S. Provisional Application Serial No. 63 / 446,861 filed on February 19, 2023; the contents of which are incorporated herein by reference. Technical Field

[0003] The present invention relates generally to adhesives and, in particular, to free radical curing adhesives that retain strength after heating. Background Art

[0004] In many industries, manufacturers of mating components have turned to structural adhesives to replace traditional fastening technologies such as rivets, bolts and welds. In theory, adhesives offer many attractive properties, including improved product performance, aesthetics, reduced overall assembly time and reduced production costs. In addition, adhesives can avoid the stress point concentration, corrosion and component damage common to rivets, bolts, welds and other traditional fastening methods. Adhesives have made considerable progress in reducing assembly time compared to some traditional mechanical fastening methods, but depending on the application and assembly time, you may still be adversely affected by the working life of the adhesive. In many applications, if the assembly is not completed before the material becomes a hard or gel solid, the adhesive joint will not provide the strength required to perform as designed. In many cases, if this occurs, it can result in expensive and time-consuming rework costs. To alleviate these problems, manufacturers can use materials with longer working lives. However, in doing so, the material will take longer to achieve sufficient strength to proceed to the next step in the assembly, which is called "fixture time". Generally, for adhesives, the fixture time increases dramatically as the working life increases.

[0005] Sufficient strength to move to the next step in the production process is called the fixing time of the adhesive. The bond strength to transfer to another stage in the production process is uncertain because it depends largely on the specific conditions of the production process and the product. Most often, the bond strength of the metal joint is used to define the bond strength. The American standard test method ASTM D1002, "Standard Test Method for Apparent Shear Strength of Single Lap Bonded Metal Specimens by Tensile Loading (Metal to Metal)" is the recognized standard for testing bond strength. The fixing time can be defined as the time it takes for the adhesive to reach the specified bond strength.

[0006] Typically, acrylic adhesives are used in applications where the fixturing time, or the time the part can be handled, is critical to production or repair. The adhesive can often be accelerated by using catalysts, adding curing agents, or reducing agents, thereby improving the fixturing time. However, doing so also shortens the working life, or the time the material can be used. If the working life is too short, the adhesive may be wasted and the mating parts may not bond properly to each other. If the time until the part can be handled (fixturing time) is too long, repair or production time is wasted.

[0007] In the automotive industry, metal adhesive bonding typically involves steps such as thorough cleaning of the mating surfaces of the substrates, light sanding of the bonding surfaces, and the use of adhesion promoters and / or primers. These steps are performed to make the surfaces of the substrates as receptive to the adhesive as possible. Contaminants left on the surface can reduce bond strength by interfering with the adhesive's ability to form a bond, creating weaker chemical bonds, or reducing the bond area. In addition, when the bond is stressed, contaminants may provide fracture initiation sites, again reducing the load that the joint can withstand. Therefore, to ensure a good adhesive bond, a cleaning step is typically required to remove possible contaminants from the bonding surfaces. Sanding the surface can remove surface roughness defects and promote a bond layer of consistent thickness and intimate contact between the adhesive and the substrate. A primer can be another layer of actual coating that provides a more consistent and bondable surface. Adhesion promoters can be used to "activate" the surface, providing chemical groups to adhere to the adhesive when applied. These preparations occur before the automotive factory is painted, but not before an application such as hem flange bonding.

[0008] Hem flange bonding is performed in the body shop or metal fabrication plant of an assembly plant before painting and shipment to the assembly plant. Steel body panels, usually galvanized, are stamped and formed, and various lubricants, such as mill oils and stretching agents or pre-lubes, are used during the process. One or more lubricants may be present when the adhesive is applied, but there is no cleaning step to remove the lubricant, in part because the lubricant also protects the metal from oxidation.

[0009] During hem flange bonding, after the adhesive is applied to the outer panel, the inner panel is placed and the outer panel is bent or curled around the inner panel, forming the hem flange. The adhesive bead size is carefully controlled to fill the bond line but avoid squeeze-out. Adhesive that escapes the bond line may contaminate equipment and cause cleaning and maintenance problems in the manufacturing plant. A curing step, such as induction curing, can be introduced at this stage. The curing step can be a full cure or just enough to prevent any movement of the inner panel to the outer panel during subsequent processing. The body closure panels are attached to the frame and sent to the paint shop, where they are cleaned, primed and painted. Curing of the adhesive is completed in a paint oven.

[0010] One of the reasons for using adhesives in hem flanges is to reduce or eliminate the use of spot welds to hold the inner and outer panels together. Spot welds on outer panels are sometimes very visible and require a finishing or polishing step prior to painting to make the spot welds nearly invisible. The few remaining welds act as peel stops, reducing the adhesive’s susceptibility to any peel loads and holding the panels together until the adhesive cures. This processing step places new requirements on the adhesive related to weldability. First, the adhesive must not affect the integrity of the spot welds. Second, similar to the forming process, the adhesive must not escape from the seam and onto the welding equipment.

[0011] As adhesives are further used in manufacturing, there is a need for improved adhesive formulations that are suitable for bonding metal substrates and withstanding various finishing processes, including painting, electroplating (E-Coat) / electrostatic painting, and powder coating post-baking. Another problem with existing adhesives is flammability, which complicates their industrial handling and use.

[0012] Electrostatic painting of various vehicle components presents an attractive and cost-effective alternative to using conventional paint lines. Vehicle components such as doors, hoods, side panels and other vehicle skin components can be conventionally electrostatically painted. Due to the high visibility and exposure of such vehicle components to the environment, a high-quality paint surface with high reflectivity and no visual defects is required. Electrostatic painting requires that the parts be conductive and an electrical potential be provided across the parts to attract oppositely charged paint aerosol droplets to the parts. Therefore, the bonding adhesive used to join the parts undergoing painting usually needs to be conductive to ensure that the parts being bonded are charged at the same potential during the painting stage.

[0013] Therefore, there is a need for a structural adhesive formulation that can be used to increase working life while mitigating extended fixture times while being suitable for a variety of finishing processes. There is also a need for a structural adhesive formulation that is electrically conductive so as to bond parts that provide a surface susceptible to receiving a highly uniform coating of paint by electrostatic spray techniques. Summary of the invention

[0014] A method of applying an adhesive to a substrate is provided, the method comprising mixing together the ingredients of a two-component formulation of Part A and Part B. Part A comprises a reactive methacrylate phosphate monomer or oligomer, a Part A methacrylate monomer, a hydroxylated methacrylate monomer, a free radical polymerization inhibitor, an adhesion promoter, a Part A impact modifier, a Part A toughening agent, and a free radical polymerization initiator. Part B comprises a Part B impact modifier and a polymerization accelerator. Part A and Part B are combined together to form an adhesive mixture. The adhesive mixture is applied to a substrate. The adhesive mixture can be cured to form an adhesive that can last up to one hour at a baking temperature of 205°C without adversely affecting the adhesion of the substrate.

[0015] Also provided are formulations of component A and component B. A bonded structure is provided wherein the resulting adhesive is located between a first substrate and a second substrate. DETAILED DESCRIPTION

[0016] The present invention has the use of a curing adhesive particularly suitable for bonding structural substrates. The structural substrates operatively bonded by the adhesive of the present invention may include electrogalvanized steel, hot-dip galvanized steel, cold-rolled steel, aluminum, aluminum alloys, polyacrylonitrile butadiene-styrene (ABS), mild steel (MS), polyvinyl chloride (PVC) and fiberglass. The adhesive formulation of the present invention is believed to be effectively bonded to similar structural substrates, as well as bonding such a substrate to other substrates including other metals, other plastics, and to achieve this through rapid processing strength during the curing process, so as to facilitate handling and removal of fixtures in a manufacturing environment. In a specific embodiment of the invention, conductive fillers are incorporated into the adhesive formulation to control the electrical conductivity and / or thermal conductivity of the high temperature adhesive. The inclusion of conductive fillers in the embodiment of the high temperature adhesive provides a conductive adhesive that forms an adhesive bond to conduct charge between the bonded substrates, and then the bonded substrates can be electroplated (E-Coat) / electrostatically sprayed or powder-coated. The conductive embodiment of the high temperature adhesive of the present invention can also be used to provide electromagnetic field (EMF) shielding by forming a Faraday cage with a bonded conductive surface. Conductive embodiments of the adhesives of the present invention may also provide improved thermal conduction between the bonded materials, which may be advantageous for powder coating or heat dissipation.

[0017] Embodiments of the adhesive formulations of the present invention have high levels of product stability, high flash point (non-flammable), high boiling point (low volatile organic compound (VOC) content and low odor), and have high heat resistance, and present lower health hazards relative to adhesive materials such as tetrahydrofurfuryl methacrylate (THFMA). In some inventive embodiments, these results are achieved by replacing all or part of the methyl methacrylate monomer with a high flash point monomer. Therefore, some inventive embodiments do not contain methyl methacrylate. Embodiments of the adhesive formulations of the present invention have mixing ratios of 1:1, 4:1, 10:1±0.10%, which are convenient for users and provide excellent adhesion to highly contaminated metal surfaces using cutting oils and sampling oils without the use of primers. Embodiments of the adhesive formulations of the present invention can be bonded by a wider variety of stamping oils and cutting oils and are less brittle (higher elongation at break) than existing adhesive formulations. Embodiments of the adhesive formulations of the present invention are suitable for bonding metal substrates and can withstand various processes including painting, electroplating (E-Coat) / electrostatic painting and powder coating post-bake temperatures of 205°C (400°F) for up to one hour without adversely affecting adhesion or physical properties. Embodiments of the adhesive formulations of the present invention are well suited for bonding hem flange joints to metal parts such as doors of various vehicles and also provide the ability to be manipulated to provide different working times to accommodate other transportation and general industrial applications.

[0018] Embodiments of the adhesive formulations of the present invention allow for uniform distribution and flow of the adhesive while also providing longer working time than conventional compositions and having a rapid set after the working time which can be accelerated by post heat curing. The high boiling point of the adhesive formulations of the present invention minimizes off-gassing during application, reduces odor and flammability, and can also impart stability at temperatures of 205°C (400°F) for up to one hour while maintaining adhesion.

[0019] The present invention achieves the seemingly contradictory characteristics of increasing the working life while slowing down the extension of the fixation time by using a transfer agent, an induction retarder or a combination thereof. The present invention does not contain a chain transfer agent, but if it is desired to further increase the working life, it is conceivable that a chain transfer agent could be added, but this has not been experimented with by the present invention. The formulation of the present invention contains inhibitors, antioxidants and stabilizers to help increase the working life while slowing down the extension of the fixation time. Without wishing to be bound by a particular theory through the selection of agents, the characteristics of the fixation time and working time are believed to be the result of a combination of thermodynamically and kinetically controlled processes.

[0020] It should be understood that where a numerical range is provided, the range is intended to include not only the endpoints of the range, but also the intermediate values ​​of the range, i.e., explicitly included in the range and varying according to the last significant figure of the range. For example, the range of 1 to 4 listed is intended to include 1-2, 1-3, 2-4, 3-4 and 1-4.

[0021] For the purpose of defining and defining a strength that is considered appropriate for most production assemblies, fixture time as used herein refers to the time to achieve a strength of 1 MPa as measured in accordance with ASTM D1002 with a half inch overlap using a 0.03 inch bond gap.

[0022] As used herein, (meth)acrylate refers to methacrylate or acrylate.

[0023] As used herein, work life refers to the time it takes for a material to reach a gel state, which is defined as the point in time after the material is first mixed when the storage modulus (G') and the loss modulus (G") are equal, which is defined as the time required for a bead of material (approximately 20 grams) to be dispensed from the barrel and passed through an overhead mixer, and then manually inspected with a tongue depressor for the adhesive to begin to thicken.

[0024] As used herein, maintenance of bond strength at elevated temperatures is defined as strength within 10% of the room temperature strength measured immediately after cure.

[0025] The weight percentages used herein, unless otherwise indicated, refer to the formulation excluding the particle filler contained in the resin matrix during the two-component curing. It is worth noting that the total weight percentage of the particle filler in the fully formulated formulation can be as high as 90%.

[0026] The present invention uses an acrylic adhesive in a two-component adhesive formulation. It is provided in the form of a binary system, including an adhesive component A and an activator component B. Component A includes a methacrylate monomer, a high flash point acrylate monomer; a free radical polymerization inhibitor; and an adhesion promoter. Component B contains a monomer reactant, a high flash point (meth) acrylate monomer, and a polymerization accelerator, with the proviso that the impact modifier and the free radical polymerization initiator are present as separate parts in the fully mixed curable formulation, or in at least one of component A or component B. In some inventive embodiments, component A includes a reactive methacrylate phosphate monomer or oligomer, a hydroxylated methacrylate monomer, or a combination thereof. Various additives are easily included to improve the handling properties of the formulation of the present invention. The amount of component B varies according to the weight ratio relative to component A. Component A and component B each have a separate storage stability of at least 180 days at 23°C. Although the present invention is described in detail herein with respect to a mixture having a weight ratio of 4:1 of component A:component B, it should be understood that other mixing ratios within the range of 10-1:1 of component A:component B can also be easily mixed without departing from the spirit of the present invention. Ingredients common to components A and B, such as monomer reactants, impact modifiers and toughening agents, can be the same in both components, or different compounds, which are present to impart the desired properties to the resulting adhesive.

[0027] A method of applying an adhesive to a substrate is provided, the method comprising combining component A and component B together to form an adhesive mixture, applying the mixture to the substrate and curing the applied mixture.

[0028] Methacrylate phosphate monomers or oligomers, when present and functional herein, illustratively include glyceryl monomethacrylate phosphate; glyceryl dimethacrylate phosphate; hydroxy (C 2-6The invention also provides a plurality of methacrylate phosphates, such as methacrylate phosphates (such as hydroxyethyl methacrylate phosphates); bis-(methacryloyloxyethyl) phosphates; methacryloyloxypropyl phosphates; bis-(methacryloyloxypropyl) phosphates; bis-(methacryloyloxy)propoxy phosphates; methacryloyloxyhexyl phosphates; bis-(methacryloyloxyhexyl) phosphates; methacryloyloxyoctyl phosphates; bis-(methacryloyloxyoctyl) phosphates; methacryloyloxydecyl phosphates; bis-(methacryloyloxydecyl) phosphates; caprolactone methacrylate phosphates; polymethacrylate polycarboxyl polyphosphonic acid; polymethacrylate polychlorophosphoric acid; and any combination thereof. Without intending to be bound by a particular theory, these methacrylate phosphate monomers and oligomers are believed to have a chemical affinity for a variety of metal substrates and act as adhesion promoters that are susceptible to free radical curing. In a 4:1 weight mixture of component A and component B, the typical loading range of methacrylate phosphate monomers and oligomers in the fully formulated adhesive of the present invention is 0-5 total weight percent.

[0029] In some inventive embodiments, adhesive component A comprises a methacrylate monomer that is reactive under curing conditions. The methacrylate monomers used in the present invention include acrylate monomers, methacrylate monomers, acrylic acid monomers, methacrylic acid monomers, or any combination thereof. Specific monomers used in the present invention illustratively include methacrylic acid, C 1-16 Amino acrylate, C 1-16 Secondary amine acrylate, C 1-16 Alkyl acrylic acid, epoxy C 1-16Acrylate, and any combination thereof. In addition to the methyl methacrylate mentioned above, the specific monomers that can be used herein include at least one of the following acrylate or methacrylate monomers: ethyl (meth)acrylate, isobornyl (meth)acrylate, butyl (meth)acrylate, octyl (meth)acrylate, hexylethyl (meth)acrylate, dodecyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, methoxypolyethylene glycol mono(meth)acrylate, isodecyl (meth)acrylate, cyclic trimethylolpropane Formal (meth) acrylate, trimethylcyclohexyl (meth) acrylate, caprolactone (meth) acrylate, tridecyl (meth) acrylate, cyclohexyl (meth) acrylate, 2-hydroxyethyl acrylate, 2-hydroxy (meth) acrylate, 3-hydroxypropyl acrylate, 1-hydroxy-2-aminopropyl methacrylate, 1-amino-2-hydroxypropyl methacrylate, acrylamide, 1-amino-3-hydroxypropyl (meth) acrylate, (meth) acrylate 2-(tert-butylamino) ethyl ester, methacrylic acid and glycidyl methacrylate or any combination thereof. It should be understood that according to the present invention, methyl methacrylate monomers can be excluded in whole or in part and high flash point monomers can be used. In a 4:1 weight mixture of component A and component B, the typical loading range of methacrylate monomers in the fully formulated adhesive of the present invention is 5-40 total weight percent.

[0030] In some inventive embodiments, adhesive component A also includes a hydroxylated methacrylate monomer that is reactive under curing conditions. The hydroxylated methacrylate monomer reactants used herein illustratively include 2-hydroxypropyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxy-1-methylethyl methacrylate, 2,3-dihydroxypropyl methacrylate, 4-hydroxybutyl methacrylate, 1,3-dimethacrylate glycerol, 2-(hydroxymethyl)acrylate bisphenol A ethoxylate dimethacrylate, or any combination thereof. It should be understood that for the purpose of dosage, the hydroxylated methacrylate phosphate in the formulation is also not included in the hydroxylated methacrylate monomer. In a 4:1 weight mixture of component A and component B, the typical loading range of the hydroxylated methacrylate monomer (if present) in the fully formulated adhesive of the present invention is 0-10 total weight percent.

[0031] The flash point of the curable monomers of adhesive component A is generally at least 90°C.

[0032] Adhesive component A comprises a high flash point (meth) acrylate monomer that is reactive under curing conditions. The high flash point (meth) acrylate monomer has a flash point of at least 90°C, and in some embodiments at least 94°C. The high flash point (meth) acrylate monomers used herein illustratively include benzyl methacrylate, benzyl 2-methylpent-2-enoate, benzyl 2-methylhex-2-enoate, benzyl (2E)-2-vinylpent-2,4-dienoate, 5-O-benzyl 1-O-methyl (E)-pent-2-enedioate, benzyl (E)-2-methyl-4-prop-2-enyloxybutyl-2-enoate, benzyl acrylate, methyl (E)-2-methylene-9-phenylmethoxynon-3-enoate, benzyl (E)-3-methoxy-2-methylprop-2-enoate, ethyl 2-methyl-5-phenylmethoxypent-2-enoate. Ester, (2E)-2-methylhexa-2,5-dienoic acid benzyl ester, 2-methylprop-2-enoic acid 4-benzyloxybutyl ester, (2E,4E)-5-fluoro-2-methylhexa-2,4-dienoic acid benzyl ester, (2E)-2-vinyl-3-methylpenta-2,4-dienoic acid benzyl ester, fluorobenzyl methacrylate, 2-(perfluorooctyl)ethyl acrylate, (perfluoroheptyl)methyl methacrylate, 2-(N-ethylperfluorooctylsulfonamido)ethyl acrylate, 2-(perfluorohexyl)ethyl methacrylate, 2-(perfluoroisononyl)ethyl acrylate, isobornyl methacrylate, or any combination thereof. In some embodiments of the present invention, the high flash point acrylate monomer is present in both component A and component B. In a 4:1 weight mixture of component A and component B, the typical loading amount of the high flash point acrylate monomer in the fully formulated adhesive of the present invention ranges from 15 to 35 total weight percent.

[0033] In some exemplary embodiments of the present invention, ultra-high molecular weight polyethylene (UHMW-PE) is present in a total weight percentage of 1-3 after component A and component B are mixed, methacrylate is present in a total weight percentage of up to 10, and there is no curable monomer with a flash point below 65° C. at standard temperature and pressure (STP). In other inventive embodiments, the toughening agent is present in component A, component B, or both component A and component B.

[0034] In some embodiments of the invention, the polymerization initiator provided is sulfonyl chloride. The sulfonyl chloride used herein includes chlorosulfonated polyethylene, p-toluenesulfonyl chloride, methanesulfonyl chloride, benzenesulfonyl chloride, C2-C 14 Alkylsulfonyl chloride and C7-C 14Arylsulfonyl chloride, or any combination thereof, wherein alkyl includes straight chain, branched chain, cyclic chain structure and such structure with pendant groups, and aryl includes diaryl and monoaryl containing pendant groups. Sulfonyl chloride is present in component A of the present invention in an unprotected or encapsulated form, while sulfonyl chloride is present in component B only in an encapsulated form. For a 4:1 volume ratio of component A: component B, the typical loading range of sulfonyl chloride (if present) is 0.0125-3.75 total weight percent of the combination of component A and component B, excluding any encapsulating agent or particulate filler. It is noteworthy that sulfonyl chloride can be used in combination with halogen chain transfer agents and / or multifunctional chain transfer agents to adjust the working time of the resulting preparation. It is worth noting that if chlorosulfonated polyethylene (CSPE) is used instead of toluenesulfonyl chloride, the loading will be higher because the molecular weight per mole of sulfonyl chloride of CSPE is much higher, ranging from 0.1 to 8 total weight percent of the combination of components A and B for a 4:1 volume ratio of component A:component B, excluding any encapsulant.

[0035] Encapsulants useful herein are described in detail in US 3,396,116, the details of which are incorporated herein by reference.

[0036] In some inventive embodiments, the formulation is cured by a polymerization initiator, which is a chemical free radical curing initiator. Chemical free radical curing initiators used herein include organic peroxides, azo-type initiators, and any combination thereof. Peroxide initiators used herein illustratively include diacyl peroxides, hydroperoxides, ketone peroxides, peroxyesters, peroxyketals, dialkyl peroxides, alkyl peresters, and percarbonates. Azo-type initiators used herein illustratively include azobisisobutyronitrile (AIBN). Benzoyl peroxide (BPO) is a typical free radical curing initiator. Chemical curing initiators are generally present in 0.0125-3.75 weight percent of the formulation in which component A and component B are completely mixed. Impact modifiers used herein illustratively include block copolymers of methyl methacrylate-butadiene-styrene, nitrile rubber, styrene or α-methylstyrene with butadiene or hydrogenated butadiene (rubber grafting rate is up to or greater than 50%), ABS, natural rubber, or any combination thereof. It should also be understood that any of the above-mentioned materials terminated with methyl methacrylate can also be used as impact modifiers herein, which are cross-linked with the matrix formed by the solidification of monomers / oligomers. The load of impact modifier depends on factors such as the weight ratio between the adhesive part and the activator part, the impact modifier molecular weight and the impact modifier modulus. For the invention formulation of 4:1, the typical impact modifier load range is 10 to 30 total weight percentages. In some inventive embodiments, the impact modifier exists in combination with a toughening agent as a rubber component, for example, in the form of core-shell rubber particles. In other embodiments, the impact modifier is separated into the activator, i.e., the component B of the formulation of the present invention, but is still used to change the failure mode of the cured adhesive. In some inventive embodiments, the impact modifier is present in both component A and component B.

[0037] In some inventive embodiments, the inventive formulation further comprises a toughening agent. In the present invention, the toughening agent is distinguished from an impact modifier in that the toughening agent is a resin that is mixed or dissolved with a monomer and forms a miscible mixture / solution, and can significantly improve the performance of the cured adhesive at low temperatures (such as -40°F (-40°C)) without negatively affecting the performance of the cured adhesive at high temperatures (such as 180°F), while the impact modifier as a core-shell structure of a rubber particle dispersion provides not only excellent impact strength, but also no dents, excellent thixotropic properties, and improved anti-slip properties. The toughening agent used here can be illustratively selected from a variety of elastic materials that form discrete particles or dual-phase domains in a continuous resin matrix. For example, pre-reacted particles, butadiene-acrylonitrile copolymers, styrene / ethylene / styrene, α-methylstyrene / ethylene / α-methylstyrene, α-methylstyrene / butadiene / α-methylstyrene, styrene / butadiene / styrene (SBS) copolymers, styrene / isoprene / styrene (SIS) copolymers, styrene / ethylene / butadiene / styrene (SEBS) copolymers, styrene / butadiene (SBR) copolymers, styrene-acrylonitrile (SAN), vinyl-terminated butadiene-acrylonitrile copolymers, glycidyl methacrylate functionalized butadiene-acrylonitrile copolymers, hydroxyl-functionalized butadiene, isocyanate-functionalized butadiene, amine-terminated butadiene, epoxy-terminated butadiene, maleic acid acylated polybutadiene or isoprene, or any copolymers thereof. US 6,660,805 includes examples of such maleated polymers and copolymers, as well as other pre-reacted materials that can be added to the resin composition in particle form.

[0038] A partial list of useful pre-reacted elastomeric rubbers that can be used as impact modifiers includes pre-reacted elastomeric particles including: acrylate-butadiene; butadiene; chloroprene; ethylene-propylene; ethylene-propylene-diene; isoprene; isobutylene; isobutylene-isoprene (butyl rubber); styrene-butadiene; styrene-isoprene; acrylonitrile-butadiene; acrylonitrile-chloroprene; vinyl terminated polybutadienes such as vinylpyridine-butadiene, vinylpyridine-styrene-butadiene; carboxyl-styrene-butadiene; chloro-isobutylene-isoprene (chlorobutyl rubber); brominated-isobutylene-isoprene (bromobutyl rubber); dialkylsiloxanes, polypropylene oxide); polyester polyurethanes; polyether polyurethanes; and any mixtures thereof. In addition, reactive liquid polymers (RLPs) can also be incorporated as toughening components. RLPs contain functional groups, usually located at their ends, but occasionally as pendant groups, and react with the resin in situ to form elastomeric domains. Examples of RLPs include, but are not limited to, vinyl terminated butadiene acrylonitrile (VTBN), carboxyl terminated butadiene acrylonitrile (CTBN), amine terminated butadiene acrylonitrile (ATBN), hydroxyl terminated butadiene acrylonitrile (HTBN), epoxy terminated butadiene acrylonitrile (ETBN), mercapto terminated butadiene acrylonitrile (MTPN), vinyl terminated butadiene (VTB), maleated butadiene, phenoxy terminated butadiene acrylonitrile (PTBN). In some specific embodiments of the present invention, the toughening agent includes ultra-high molecular weight polyethylene (UHMW-PE), chlorosulfonated polyethylene, chloroprene rubber, ethylene-acrylic acid elastomeric copolymer, poly(methyl methacrylate) grafted rubber, butadiene-styrene-acrylonitrile copolymer, or any combination thereof. It should also be understood that any of the above substances terminated with methyl methacrylate can also be used as a toughening agent here to crosslink with the matrix formed by the curing of the monomer / oligomer. It should be understood that toughener exists as a component of adhesive component, activator component or bicomponent in the present invention's formulation.In a specific embodiment of the present invention, toughener is only present in the adhesive component, but it should be understood that the consumption of the toughener present depends on the characteristic of toughener.In the adhesive of the present invention prepared completely, the typical toughener loading is 8 to 25 percent by weight in the adhesive of 4:1: the scope of the preparation of activator.In other embodiments, there is ultra-high molecular weight polyethylene (UHMW-PE).

[0039] In order to prepare the adhesive formulation of the present invention that can achieve high strength without separate surface treatment before applying the formulation of the present invention, an adhesion promoter is provided in the formulation of the present invention. The adhesion promoter is conducive to the adhesion of the fully cured formulation of various substrates (including galvanized substrates). The adhesion promoter is easy to be formulated into the adhesive component, activator component or the two components of the formulation of the present invention. In a specific embodiment, the adhesion promoter is only found in the adhesive component. The specific adhesion promoter used in the formulation of the present invention illustratively includes: phosphate, monofunctional phosphate, difunctional phosphate, polymerized phosphate functional polymer, (meth) acrylic acid, polymer materials with organic acid functionalization, maleic acid, acid functionalized polymers (such as maleic anhydride modified polybutadiene), citric acid di- or trimethacrylate, polymethacrylic acid oligomeric maleic acid, polymethacrylic acid polymaleic acid, polymethacrylate polymethacrylic acid, silane or any combination thereof. Silane adhesion promoters useful herein illustratively include: 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane, (3-glycidyloxypropyl)bis(trimethylsiloxy)methylsilane, (3-glycidyloxypropyl)methyldiethoxysilane, (3-glycidyloxypropyl)dimethylethoxysilane, (3-glycidyloxypropyl)methyldimethoxysilane, methacryloxymethyltriethoxysilane, methacryloxymethyltrimethoxysilane, methacryloxypropyldimethoxysilane, and the like. Methylethoxysilane, methacryloxypropyl dimethylmethoxysilane, methacryloxypropyl trimethoxysilane, ethylacryloxypropyl methyldimethoxysilane, methacryloxypropyl triethoxysilane, methoxymethyltrimethylsilane, 3-methoxypropyl trimethoxysilane, 3-methacryloxypropyl dimethylchlorosilane, methacryloxypropyl methyldichlorosilane, methacryloxypropyl trichlorosilane, 3-isocyanopropyl dimethylchlorosilane, 3-isocyanopropyl triethoxysilane, bis(3-triethoxysilylpropyl)tetrasulfide, and any mixtures thereof. In a 4:1 adhesive:activator formulation, the typical loading range of the adhesion promoter in the formulation of the present invention is 0.5 to 10 total weight percent.

[0040] Antioxidants are present in the adhesive and illustratively include: hydroquinone (HQ), butylated hydroxytoluene (BHT), 1,4-naphthoquinone, 2,6-di-tert-butyl-4-(dimethylaminomethyl)phenol, 2,2,6,6-tetramethylpiperidin-1-oxyl free radical or commonly known as TEMPO, 4-hydroxy-TEMPO or TEMPOL, butylated hydroxyanisole, 2,6-di-tert-butylcresol, 2,2′-methylenebis(6-tert-butyl-4-methylphenol), 2,2′-thiobis(6-tert-butyl-4-methylphenol), Tert-butyl hydroquinone, di-tert-butyl hydroquinone, di-tert-amyl hydroquinone, methyl hydroquinone, p-methoxyphenol, tetrakis [methylene-3- (3 ', 5 '-di-tert-butyl-4 '-hydroxyphenyl) propionate] methane, N- (2-aminoethyl) -3- [3, 5-di (tert-butyl) -4-hydroxyphenyl] propionamide, 5, 7-di-tert-butyl-3- (3, 4, - dimethylphenyl) -3H-benzofuran-2-one, dilauryl thiodipropionate, dimyristyl thiodipropionate, tris (nonylphenyl) phosphite, and any combination thereof. In a 4: 1 binder: activator formulation, the typical loading amount of the antioxidant in the formulation of the present invention ranges from 0.05 to 6 total weight percent.

[0041] The polymerization accelerator present in activator component B is limited only by the desired free radical polymerization kinetics and compatibility with the other ingredients of the composition of the present invention. Accelerators that may be used herein illustratively include: dimethylaminopyridine; polyethyleneimine, N,N-dimethylaniline, modified dihydropyridines (such as 3,5-diethyl-1,2-dihydro-1-phenyl-2-propylpyridine), 2-methylimidazole, 2-hydroxyethyl-p-toluidine, ethanolamine, diethanolamine, diethylethanolamine, methyldiethanolamine, butyldiethanolamine, diethylamine, triethylamine, n-butylamine, 2,2-bipyridine, 1,10-phenanthroline, ammonia, alkylene malonates, delta-iminomalonates, ethylenediamine ... Amine (ethylazan), aniline, benzylamine, 1-benzofuran-2-amine, 4-aminoquinoline, pentane-1,2,5-triamine, benzene-1,2,4,5-tetramine, bis(2-chloroethyl)amine, butyl(ethyl)methylamine, (2-chloroethyl) (propyl)amine, hexane-1-imine, isopropylamine, ethane-1,2-diimine, carbodiimide, adjacent acetylhydroxylamine, adjacent carboxyhydroxylamine, hydroxylamine o-sulfonic acid, o-hydroxyaniline, phenylpropanolamine hydrochloride, catecholamine, indoleamine or polyacrylamide and any combination thereof.In the adhesive of 4:1: in the preparation of activator, the typical load capacity range of polymerization accelerator in the preparation of the present invention is 0.3 to 3 total weight percentages.Without intending to be bound by a particular theory, accelerator is considered to react to decompose organic peroxide, thereby improving the cure rate of adhesive.

[0042] In certain embodiments, the preparation of the present invention also includes various additives, such as chelating agents, corrosion inhibitors, thickeners, pigments, thixotropic agents, plasticizers, viscosity modifiers and combinations thereof. Such additives are only subject to the restrictions of the compatibility requirements of other components of the preparation of the present invention. Such additives are provided to balance or otherwise change at least one property of the preparation of the present invention, such as processing, storage, cure rate or bonding properties. In the preparation of 4:1 adhesive: activator, the typical loading range of each additive in the preparation of the present invention is 0 to 5 total weight percentages.

[0043] The particle filler used in the embodiment of the adhesive illustratively includes wollastonite, hollow fly ash, calcium carbonate, calcium silicate, aluminum oxide, trihydrate aluminum oxide (ATH), silicon dioxide, talc, dolomite, vermiculite, diatomaceous earth, kaolin, carbon black, graphene, ceramics, metals, and any combination thereof. The factor relevant to selecting the particle filler illustratively includes the chemical resistance of filler cost, obtained flowability viscosity, obtained shrinkage, surface finish, flame retardancy and thermosetting formulations. Typical filler size is 0.1 to 50 microns. In the preparation of 4: 1 adhesive: activator, the typical loading of the particle filler in the preparation of the present invention is 0 to 10 total weight percentages, but in other embodiments, there can be up to 90 total weight percentages. Such particle fillers are not included in the weight percentage of the curing component of the preparation of the present invention.

[0044] Typical ingredient amounts for Part A and Part B of the adhesives of the present invention are provided in Tables 1A and 1B, respectively.

[0045] Table 1A and 1B. Typical ingredient amounts of binder (component A) and activator (component B), where amounts are given in weight percent unless otherwise stated:

[0046] Table 1A. Adhesive (Component A)

[0047] Element: (4:1 ratio) Reactive methacrylate phosphate monomers or oligomers 0-6.25 Methacrylate monomer 6.25-50 Hydroxylated methacrylate monomer 0-12.5 High flash point (meth)acrylate monomer 0-43.75* Polymerization initiator 0.0125–3.75* Impact modifier 0-37.5* Toughening agent 0-31.25* Adhesion promoter 0-6.25* Antioxidants 0-7.5* Optional additives, up to 5% each 0-Margin

[0048] *Present in at least one of component A or component B or added to their mixture

[0049] Table 1B. Activator (Component B)

[0050] Element: (4:1 ratio) High flash point (meth)acrylate monomer 0-60* Impact modifier 0-50* Toughening agent 0-50* Adhesion promoter 0-25* Antioxidants 0-30* Polymerization accelerator 1.5-15 Optional additives, up to 5% each 0-Margin

[0051] *Present in at least one of component A or component B or added to their mixture

[0052] Table 2 provides the formulation of the present invention when fully formulated after mixing component A and component B in a total weight percentage ratio of 4:1.

[0053] Table 2. Fully formulated but without particulate fillers.

[0054]

[0055]

[0056] Provided is a method for producing an adhesive formulation by free radical polymerization, which is well bonded to the above-mentioned substrate. The formulation of the present invention is a two-component formulation, which is either pre-mixed to start a certain period of pot life, or alternatively the two components are applied to the substrate together under conditions where polymerization occurs between various monomers. In a specific inventive embodiment, polymerization occurs at 24°C in ambient atmosphere, and in other embodiments, polymerization is initiated by energy input (e.g., heating, ultraviolet radiation exposure) or other free radical formation mechanisms. In certain inventive embodiments, adhesive component A and activator component B are present in a volume ratio of 4:1±10%, and a storage stability of more than 180 days is obtained at 23°C. The typical viscosity of component A and component B is independently between 20,000 and 500,000 cPs. In some inventive embodiments, the viscosity of individual components A and B differs within ±50% to facilitate mixing between them.

[0057] Regardless of the form of the formulation of the present invention, when the pot life of the formulation is introduced, the formulation is in contact with two or more substrates at the same time, wherein the substrate is kept in contact with the formulation of the present invention in the curing for a sufficient amount of time to achieve bonding between the substrates. The formulation of the present invention is very suitable for bonding galvanized substrates, cold rolled steel, aluminum, polyvinyl chloride (PVC), acrylonitrile-butadiene-styrene plastics (ABS), mild steel, vinyl polymers, wood and fiberglass. Two such substrates can be combined together to form various adjacent structures, such as lap joints, butt joints, corner joints, edge joints and T-joints. In other embodiments, the formulation of the present invention is applied to a single substrate and allowed to cure to form a coating that provides substrate protection or can be used as a primer for subsequent material application. Because the formulation of the present invention is cured by a free radical mechanism, the formulation of the present invention can be applied to various thicknesses and polymerization can still be achieved throughout. The typical thickness range of the formulation of the present invention between substrates is 0.001-25mm. The resulting adhesive can withstand a baking temperature of 205°C for up to one hour without adversely affecting the adhesion of the substrate.

[0058] In some embodiments, the adhesives of the present invention rapidly build strength for ease of handling, for example, reaching a strength of 0.34 MPa in 30 to 35 minutes and a strength of 3 to 5 MPa in 50 minutes as measured by lap shear on 5 mm thick mild steel.

[0059] Although at least one exemplary embodiment has been presented in the foregoing detailed description, it should be understood that there are a large number of variations. It should also be understood that one or more exemplary embodiments are merely examples and are not intended to limit the scope, applicability, or configuration of the described embodiments in any way. On the contrary, the foregoing detailed description will provide a convenient roadmap for those skilled in the art to implement one or more exemplary embodiments. It should be understood that various changes may be made to the functions and arrangements of the elements without departing from the scope defined by the appended claims and their equivalents.

Claims

1. A method of applying an adhesive to a substrate, comprising: Mixing together the ingredients of a two-component formulation of component A and component B, wherein component A comprises: component A methacrylate monomer, high flash point (meth)acrylate monomer, free radical polymerization inhibitor, component A impact modifier, and component B comprises: component B impact modifier and polymerization accelerator; The two components are combined together to form an adhesive mixture, wherein a free radical polymerization initiator, a polymerization accelerator and a toughening agent are present in the mixture of the component A and the component B or are added thereto as additional ingredients; applying the adhesive mixture to the substrate; as well as The adhesive mixture was allowed to cure into an adhesive that maintained a bake temperature of 205°C for one hour without adversely affecting adhesion to the substrate.

2. The method according to claim 1, wherein the volume ratio of the adhesive component A to the activator component B is 10-1:1±0.10% or 4:1±0.10%.

3. The method of claim 1 further comprising contacting a second substrate with the mixture during curing to create a bond between the substrate and the second substrate.

4. The method of claim 1 further comprising securing the substrate and the second substrate in a fixture in a joint position and in contact with the mixture simultaneously for a period of 5 to 180 minutes during free radical curing, and subsequently releasing the substrate and the second substrate from the fixture.

5. A two-component adhesive formulation comprising: Adhesive component A, the adhesive component A comprising: component A methacrylate monomer, high flash point (meth)acrylate monomer, component A impact modifier, component A toughening agent; and The activator component B comprises: a component B anti-impact modifier, a component B toughening agent, a component B monomer, a free radical polymerization initiator and a polymerization accelerator.

6. The formulation of claim 5, further comprising methacrylate phosphate monomers or oligomers.

7. The formulation of claim 6, wherein the methacrylate phosphate monomer or oligomer is at least one of glycerol monomethacrylate phosphate, glycerol dimethacrylate phosphate, hydroxy methacrylate phosphate, bis-(methacryloyloxyethyl) phosphate, methacryloyloxypropyl phosphate, bis-(methacryloyloxypropyl) phosphate, bis-(methacryloyloxy)propoxy phosphate, methacryloyloxyhexyl phosphate, bis-(methacryloyloxyhexyl) phosphate, methacryloyloxyoctyl phosphate, bis-(methacryloyloxyoctyl) phosphate, methacryloyloxydecyl phosphate, bis-(methacryloyloxydecyl) phosphate, caprolactone methacrylate phosphate, polymethacrylic acid polycarboxylic acid polyphosphonic acid, polymethacrylic acid polychlorophosphate, or any combination thereof.

8. The formulation of claim 6, wherein the methacrylate phosphate monomer or oligomer is present in an amount of 0.3 to 5 weight percent after the component A and the component B are mixed.

9. The formulation according to claim 6, wherein the component A monomer or the component B monomer is each independently at least one of the following: a (meth)acrylic acid monomer, an acrylic acid monomer, a methacrylic acid monomer, an acrylate or methacrylate monomer, a C 1-16 Amino acrylate, C 1-16 Secondary amine acrylate, C 1-16 Alkyl acrylic acid, epoxy C 1-16 Acrylates and combinations thereof.

10. The formulation of claim 6, wherein the Part A monomer reactant is the same as the Part B monomer reactant.

11. The formulation of claim 6, wherein the formulation does not include methyl methacrylate monomer.

12. The formulation of claim 6, wherein the high flash point (meth)acrylate monomer has a flash point of at least 90°C.

13. The formulation according to claim 6, further comprising a high flash point (meth)acrylate monomer in component B.

14. The formulation of claim 6, wherein the high flash point (meth)acrylate monomer is present in an amount of 15 to 35 weight percent after the component A and the component B are mixed.

15. The formulation of claim 6, wherein the impact modifier is present in an amount of 10 to 30 weight percent after the component A and the component B are mixed.

16. The formulation of claim 6, wherein the toughening agent is present in the fully formulated adhesive at 8 to 25 weight percent after the component A is mixed with the component B.

17. The formulation according to claim 6, further comprising a hydroxylated methacrylate monomer in component A.

18. The formulation of claim 6, wherein the adhesion promoter is present in the fully formulated adhesive at 0.5 to 5 weight percent after the component A and the component B are mixed.

19. The formulation of claim 6, wherein the toughening agent is ultra high molecular weight polyethylene (UHMW-PE).

20. A bonding structure comprising: first base; Second base; as well as An adhesive formed by curing the formulation of claim 6 between the first substrate and the second substrate.