Wood-plastic material binder for building construction and preparation method thereof
The bonding strength and antibacteriality of the binder are improved by using maleicated chitosan, trimethylolpropane trimethacrylate and vinylsilane coupling agent grafting technology in wood plastic binders The performance solves the problems of low bond strength and fibers not resistant to mold in the prior art, and achieves the improvement of high strength and antibacterial properties.
Patent Information
- Application Number
- CN202411126378.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The bonding strength of existing wood plastic adhesives is low, and wood fibers or plant fibers are not resistant to mold, making it difficult to meet the needs of high strength and antibacterial properties.
Maleylated chitosan, trimethylolpropane trimethacrylate and vinylsilane coupling agent were grafted to the acrylic molecular chain to prepare a wood-plastic material binder for construction to improve bonding Compatibility and bond strength of the agent with the matrix material and enhance antibacterial properties.
The high-strength bonding effect between the adhesive and the matrix material and good antibacterial properties are achieved, and the overall performance of wood plastic materials is improved.
Smart Images

Figure BDA0004996539750000081 
Figure BDA0004996539750000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adhesives, and in particular relates to a wood-plastic material adhesive for building construction and a preparation method thereof. Background Art
[0002] Wood-plastic material refers to a new type of environmentally friendly composite material made by hot pressing, extrusion, injection and other molding processing methods by combining the advantages of wood and plastic. It is a green building material and environmentally friendly product. The composite of wood and plastic substrate can be achieved through an adhesive. At present, the adhesive for wood-plastic materials is mainly hot-melt adhesive, such as polyurethane, epoxy resin, etc., but the bonding strength still needs to be improved. In the prior art, polyolefin is used as the main resin, and polar groups are introduced on it to improve the bonding strength with wood, but the grafting rate of polar groups is low, so that the bonding strength of the adhesive is still low. In addition, wood fiber or other plant fibers account for about 35-75% of wood-plastic materials, and it is necessary to solve the problem that wood fiber or other plant fibers are not resistant to mold. Therefore, it is necessary to solve the above problems and provide a wood-plastic material adhesive with high bonding strength and good antibacterial properties. Summary of the invention
[0003] The purpose of the present invention is to provide a wood-plastic material binder for construction and a preparation method thereof. Maleated chitosan, trimethylolpropane trimethacrylate and a vinyl silane coupling agent are grafted onto an acrylic acid molecular chain to prepare a wood-plastic material binder for construction. The binder has good compatibility with a base material, good bonding effect, high strength and good antibacterial performance.
[0004] The technical problem to be solved by the present invention is that in the prior art, polyolefin is used as the main resin, and polar groups are introduced thereon to improve the bonding strength with wood, but the grafting rate of the polar groups is low, so that the bonding strength of the adhesive is still low. In addition, wood fiber or other plant fiber accounts for about 35-75% of the wood-plastic material, and the problem that wood fiber or other plant fiber is not resistant to mold needs to be solved.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A wood-plastic material adhesive for building construction comprises the following components in parts by weight: 80-100 parts of polypropylene, 5-10 parts of maleic anhydride, 10-18 parts of chitosan, 1-3 parts of trimethylolpropane trimethacrylate, 2-5 parts of vinyl silane coupling agent, 0.1-0.5 parts of initiator A, 0.05-0.1 parts of initiator B, 0.2-0.7 parts of antioxidant and 320-400 parts of solvent.
[0007] Furthermore, the vinyl silane coupling agent is at least one of vinyl trimethoxy silane, vinyl triethoxy silane, γ-methacryloxypropyl trimethoxy silane, and vinyl tri(2-methoxyethoxy) silane.
[0008] Furthermore, the initiator A is at least one of dicumyl peroxide, dibenzoyl peroxide, methyl ethyl ketone peroxide, and azobisisobutyronitrile.
[0009] Furthermore, the initiator B is at least one of dicumyl peroxide, dibenzoyl peroxide, methyl ethyl ketone peroxide, and azobisisobutyronitrile.
[0010] Further, initiator A and initiator B may be the same or different.
[0011] Furthermore, the antioxidant is at least one of tris(2,4-di-tert-butyl) phosphite, 3,5-dibutyl-4-hydroxy-phenylpropionic acid octadecyl ester, p-tert-butylphenol, and 2,4-dimethyl-6-tert-butylphenol.
[0012] Furthermore, the solvent is at least one of toluene and xylene.
[0013] A method for preparing a wood-plastic material adhesive for construction, comprising the following steps:
[0014] A1, dissolving chitosan in acetic acid solution to obtain chitosan solution; dissolving maleic anhydride in deionized water, adding the chitosan solution, stirring and reacting to obtain maleoylated chitosan;
[0015] In the above preparation process, chitosan is reacted with maleic anhydride to generate maleated chitosan, and maleic anhydride is ring-opened to generate maleated chitosan with carboxyl group and carbon-carbon double bond.
[0016] Furthermore, in step A1, the stirring reaction time is 6-9h.
[0017] Furthermore, in step A1, the concentration of the acetic acid solution is 2-3%.
[0018] Furthermore, in step A1, the ratio of chitosan to acetic acid solution is (3.5-5) g: (100-110) mL.
[0019] Furthermore, in step A1, the usage ratio of maleic anhydride to deionized water is 2 g: (10-20) mL.
[0020] A2, polypropylene, maleated chitosan and trimethylolpropane trimethacrylate are mixed, initiator A and antioxidant are added, and then introduced into a twin-screw extruder, extruded and granulated to obtain graft-modified polypropylene;
[0021] In the above preparation process, maleated chitosan and trimethylolpropane trimethacrylate are grafted onto the polypropylene molecular chain, so that the polarity of the grafted modified polypropylene is improved, thereby improving the compatibility of the binder with the substrate. The present invention utilizes the carbon-carbon double bond on maleated chitosan to react with polypropylene, and grafts chitosan onto the polypropylene molecular chain, so that the binder has antibacterial properties. At the same time, the maleated chitosan molecular structure contains polar groups such as amino, hydroxyl and carboxyl groups, which can interact with the wood surface to produce hydrogen bonds, thereby improving the bonding strength between the binder and the substrate. The present invention grafts trimethylolpropane trimethacrylate onto the polypropylene molecular chain, on the one hand, to increase the crosslinking density of the grafted modified polypropylene, thereby improving its strength; on the other hand, trimethylolpropane trimethacrylate contains three carbon-carbon double bonds, which is convenient for the subsequent grafted modified polypropylene to react with the vinyl silane coupling agent. The addition of the vinyl silane coupling agent can further improve the bonding strength between the binder and the wood-plastic material.
[0022] Furthermore, in step A2, the temperature of each barrel of the twin-screw extruder is 130-190°C.
[0023] Furthermore, in step A2, the main engine speed of the twin-screw extruder is 350-550 rpm.
[0024] A3. Add grafted modified polypropylene and vinyl silane coupling agent into solvent and mix evenly to obtain a mixed solution; add initiator B into the mixed solution and stir for 3-5 hours to obtain a wood-plastic material binder for construction.
[0025] Beneficial effects of the present invention:
[0026] (1) In the technical solution of the present invention, maleated chitosan, trimethylolpropane trimethacrylate and vinyl silane coupling agent are grafted onto acrylic acid molecular chains to prepare a wood-plastic material adhesive for construction. The adhesive has good compatibility with the base material, good bonding effect, high strength and good antibacterial performance.
[0027] (2) In the technical solution of the present invention, the maleylated chitosan contains polar groups such as amine, hydroxyl and carboxyl groups in its molecular structure, which can produce hydrogen bond interactions with the wood surface, thereby improving the bonding strength between the adhesive and the substrate, and at the same time making the adhesive have anti-mildew and antibacterial properties.
[0028] (3) In the technical solution of the present invention, trimethylolpropane trimethacrylate is grafted onto the polypropylene molecular chain. On the one hand, the crosslinking density of the grafted modified polypropylene can be increased, thereby improving its strength; on the other hand, trimethylolpropane trimethacrylate contains three carbon-carbon double bonds, which facilitates the reaction of the grafted modified polypropylene with the vinyl silane coupling agent. The addition of the vinyl silane coupling agent can further improve the bonding strength between the binder and the wood-plastic material. DETAILED DESCRIPTION
[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Example 1
[0031] A wood-plastic material adhesive for construction includes the following components in parts by weight: 80 parts of polypropylene, 5 parts of maleic anhydride, 10 parts of chitosan, 1 part of trimethylolpropane trimethacrylate, 2 parts of vinyl trimethoxysilane, 0.1 part of initiator A (dicumyl peroxide), 0.05 part of initiator B (dibenzoyl peroxide), 0.2 part of tris(2,4-di-tert-butyl) phosphite, and 320 parts of toluene.
[0032] The method for preparing the wood-plastic material binder for construction comprises the following steps:
[0033] A1. Weigh the above raw materials in parts by weight; dissolve chitosan in 2% acetic acid solution (the ratio of chitosan to acetic acid solution is 3.5 g: 100 mL) to obtain a chitosan solution; dissolve maleic anhydride in deionized water (the ratio of maleic anhydride to deionized water is 2 g: 10 mL), add the chitosan solution, stir and react for 6 hours to obtain maleoylated chitosan;
[0034] A2, polypropylene, maleoylated chitosan obtained in step A1 and trimethylolpropane trimethacrylate are mixed, initiator A and antioxidant tris(2,4-di-tert-butyl) phosphite are added, and then introduced into a twin-screw extruder for extrusion granulation, wherein the twin-screw extruder is provided with 10 temperature zones, and the temperatures in each temperature zone are 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 190°C, 190°C, and 190°C, respectively, and the main engine speed is 350rpm, to obtain graft modified polypropylene;
[0035] A3. Add grafted modified polypropylene and vinyl trimethoxysilane into solvent toluene and mix evenly to obtain a mixed solution; add initiator B into the mixed solution and stir for 3 hours to obtain a wood-plastic material binder for construction.
[0036] Example 2
[0037] A wood-plastic material adhesive for construction comprises the following components in parts by weight: 90 parts of polypropylene, 6 parts of maleic anhydride, 14 parts of chitosan, 1.8 parts of trimethylolpropane trimethacrylate, 3.9 parts of vinyl triethoxysilane, 0.3 parts of initiator A (dicumyl peroxide), 0.07 parts of initiator B (dicumyl peroxide), 0.35 parts of 3,5-dibutyl-4-hydroxy-phenylpropionic acid octadecyl ester, and 340 parts of toluene.
[0038] The method for preparing the wood-plastic material binder for construction comprises the following steps:
[0039] A1. Weigh the above raw materials in parts by weight; dissolve chitosan in 2% acetic acid solution (the ratio of chitosan to acetic acid solution is 4 g: 100 mL) to obtain a chitosan solution; dissolve maleic anhydride in deionized water (the ratio of maleic anhydride to deionized water is 2 g: 12 mL), add the chitosan solution, stir and react for 7 hours to obtain maleoylated chitosan;
[0040] A2, polypropylene, maleoylated chitosan obtained in step A1 and trimethylolpropane trimethacrylate are mixed, and then initiator A and 3,5-dibutyl-4-hydroxy-phenylpropionic acid octadecyl ester are added, and then introduced into a twin-screw extruder for extrusion granulation, the twin-screw extruder is provided with 10 temperature zones, and the temperatures in each temperature zone are 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 190°C, 190°C, 190°C, and the main engine speed is 400rpm, to obtain graft modified polypropylene;
[0041] A3. Add grafted modified polypropylene and vinyl triethoxysilane into solvent toluene and mix evenly to obtain a mixed solution; add initiator B into the mixed solution and stir for 3.5 hours to obtain a wood-plastic material binder for construction.
[0042] Example 3
[0043] A wood-plastic material adhesive for construction includes the following components in parts by weight: 95 parts of polypropylene, 8 parts of maleic anhydride, 17 parts of chitosan, 2.2 parts of trimethylolpropane trimethacrylate, 4.2 parts of vinyl triethoxysilane, 0.35 parts of initiator A (dibenzoyl peroxide), 0.09 parts of initiator B (diisopropyl peroxide), 0.54 parts of p-tert-butylphenol, and 355 parts of toluene.
[0044] The method for preparing the wood-plastic material binder for construction comprises the following steps:
[0045] A1. Weigh the above raw materials in parts by weight; dissolve chitosan in 2-3% acetic acid solution (the ratio of chitosan to acetic acid solution is 4.2 g: 105 mL) to obtain a chitosan solution; dissolve maleic anhydride in deionized water (the ratio of maleic anhydride to deionized water is 2 g: 14 mL), add the chitosan solution, stir and react for 8 hours to obtain maleoylated chitosan;
[0046] A2, polypropylene, maleoylated chitosan obtained in step A1 and trimethylolpropane trimethacrylate are mixed, initiator A and p-tert-butylphenol are added, and then introduced into a twin-screw extruder for extrusion granulation, wherein the twin-screw extruder is provided with 10 temperature zones, and the temperatures in each temperature zone are 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 190°C, 190°C, and 190°C, respectively, and the main engine speed is 450rpm, to obtain graft modified polypropylene;
[0047] A3. Add grafted modified polypropylene and vinyl triethoxysilane into solvent toluene and mix evenly to obtain a mixed solution; add initiator B into the mixed solution and stir for 4 hours to obtain a wood-plastic material binder for construction.
[0048] Example 4
[0049] A wood-plastic material adhesive for construction includes the following components in parts by weight: 100 parts of polypropylene, 8 parts of maleic anhydride, 18 parts of chitosan, 2.9 parts of trimethylolpropane trimethacrylate, 4.3 parts of gamma-methacryloxypropyl trimethoxysilane, 0.42 parts of initiator A (methyl ethyl ketone peroxide), 0.1 parts of initiator B (dibenzoyl peroxide), 0.58 parts of 2,4-dimethyl-6-tert-butylphenol, and 378 parts of xylene.
[0050] The method for preparing the wood-plastic material binder for construction comprises the following steps:
[0051] A1. Weigh the above raw materials in parts by weight; dissolve chitosan in 3% acetic acid solution (the ratio of chitosan to acetic acid solution is 5 g: 100 mL) to obtain a chitosan solution; dissolve maleic anhydride in deionized water (the ratio of maleic anhydride to deionized water is 2 g: 18 mL), add the chitosan solution, stir and react for 8 hours to obtain maleoylated chitosan;
[0052] A2, polypropylene, maleoylated chitosan obtained in step A1 and trimethylolpropane trimethacrylate are mixed, initiator A and 2,4-dimethyl-6-tert-butylphenol are added, and then introduced into a twin-screw extruder for extrusion granulation, wherein the twin-screw extruder is provided with 10 temperature zones, and the temperatures in each temperature zone are 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 190°C, 190°C, and 190°C, respectively, and the main engine speed is 500rpm, to obtain graft modified polypropylene;
[0053] A3. Add grafted modified polypropylene and γ-methacryloxypropyltrimethoxysilane into solvent xylene and mix evenly to obtain a mixed solution; add initiator B into the mixed solution and stir for 4.5 hours to obtain a wood-plastic material adhesive for construction.
[0054] Example 5
[0055] A wood-plastic material adhesive for construction includes the following components in parts by weight: 100 parts of polypropylene, 10 parts of maleic anhydride, 18 parts of chitosan, 3 parts of trimethylolpropane trimethacrylate, 5 parts of vinyl tris(2-methoxyethoxy)silane, 0.5 parts of initiator A (dicumyl peroxide), 0.1 parts of initiator B (azobisisobutyronitrile), 0.7 parts of tris(2,4-di-tert-butyl) phosphite, and 400 parts of xylene.
[0056] The method for preparing the wood-plastic material binder for construction comprises the following steps:
[0057] A1. Weigh the above raw materials in parts by weight; dissolve chitosan in 2-3% acetic acid solution (the ratio of chitosan to acetic acid solution is 5 g: 110 mL) to obtain a chitosan solution; dissolve maleic anhydride in deionized water (the ratio of maleic anhydride to deionized water is 2 g: 20 mL), add the chitosan solution, stir and react for 9 hours to obtain maleoylated chitosan;
[0058] A2, polypropylene, maleoylated chitosan obtained in step A1 and trimethylolpropane trimethacrylate are mixed, initiator A and tri(2,4-di-tert-butyl) phosphite are added, and then introduced into a twin-screw extruder for extrusion granulation, wherein the twin-screw extruder is provided with 10 temperature zones, and the temperatures in each temperature zone are 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 190°C, 190°C, and 190°C, respectively, and the main engine speed is 550rpm, to obtain graft modified polypropylene;
[0059] A3. Add grafted modified polypropylene and vinyl tri(2-methoxyethoxy)silane into solvent xylene and mix evenly to obtain a mixed solution; add initiator B into the mixed solution and stir for 5 hours to obtain a wood-plastic material adhesive for construction.
[0060] Comparative Example 1
[0061] Compared with Example 3, Comparative Example 1 does not contain chitosan, and other steps and raw materials are the same as those of Example 3.
[0062] Comparative Example 2
[0063] Compared with Example 3, Comparative Example 2 does not contain a vinyl silane coupling agent, and other steps and raw materials are the same as those of Example 3.
[0064] Comparative Example 3
[0065] Compared with Example 3, Comparative Example 3 does not contain trimethylolpropane trimethacrylate, and in step A2, polypropylene, maleated chitosan and vinyl silane coupling agent are mixed for reaction, and other steps and raw materials are the same as those in Example 3.
[0066] Performance Testing
[0067] According to GB / T 17657-2022, the bonding properties of the binders prepared in Examples 1-5 and Comparative Examples 1-3 on the polyethylene wood-plastic composites were measured, wherein the contents of polyethylene, wood powder and binder were 40%, 50% and 10%, respectively. The results are shown in Table 1.
[0068] Table 1
[0069]
[0070]
[0071] It can be seen from the data in Table 1 that the adhesive prepared by the present invention has high internal bonding strength and can effectively bond wood-plastic composite materials. It can be seen from the data of Comparative Example 3 and Comparative Example 1 that since chitosan contains hydroxyl and amino groups, and maleic anhydride and chitosan produce new carboxyl groups after reaction, the bonding strength between the adhesive and the wood substrate is improved. It can be seen from the data of Comparative Example 3 and Comparative Example 2 that the vinyl silane coupling agent can improve the bonding strength between the adhesive and the substrate. It can be seen from the data of Comparative Example 3 and Comparative Example 3 that the addition of trimethylolpropane trimethacrylate can improve the cohesion of the adhesive, thereby improving the bonding strength of the adhesive, and more vinyl silane coupling agents can be grafted to further improve the bonding strength.
[0072] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0073] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A wood-plastic material adhesive for construction, Features: The invention comprises the following components in parts by weight: 80-100 parts of polypropylene, 5-10 parts of maleic anhydride, 10-18 parts of chitosan, 1-3 parts of trimethylolpropane trimethacrylate, 2-5 parts of vinyl silane coupling agent, 0.1-0.5 parts of initiator A, 0.05-0.1 parts of initiator B, 0.2-0.7 parts of antioxidant and 320-400 parts of solvent.
2. A wood-plastic material adhesive for construction according to claim 1, Features: The vinyl silane coupling agent is at least one of vinyl trimethoxy silane, vinyl triethoxy silane, γ-methacryloxypropyl trimethoxy silane and vinyl tri(2-methoxyethoxy) silane.
3. A method for preparing a wood-plastic material binder for construction according to any one of claims 1 to 2, Features: The following steps are involved: A1, dissolving chitosan in acetic acid solution to obtain chitosan solution; dissolving maleic anhydride in deionized water, adding the chitosan solution, stirring and reacting to obtain maleoylated chitosan; A2, polypropylene, maleated chitosan and trimethylolpropane trimethacrylate are mixed, initiator A and antioxidant are added, and then introduced into a twin-screw extruder, extruded and granulated to obtain graft-modified polypropylene; A3. Add grafted modified polypropylene and vinyl silane coupling agent into solvent and mix evenly to obtain a mixed solution; add initiator B into the mixed solution and stir for 3-5 hours to obtain a wood-plastic material binder for construction.
4. A method for preparing a wood-plastic material adhesive for construction according to claim 3, Features: In the step A1, the stirring reaction time is 6-9 hours.
5. A method for preparing a wood-plastic material adhesive for construction according to claim 3, Features: In the step A1, the concentration of the acetic acid solution is 2-3%.
6. A method for preparing a wood-plastic material adhesive for construction according to claim 3, Features: In the step A1, the ratio of chitosan to acetic acid solution is (3.5-5) g: (100-110) mL.
7. A method for preparing a wood-plastic material adhesive for construction according to claim 3, Features: In the step A1, the usage ratio of maleic anhydride to deionized water is 2 g: (10-20) mL.
8. A method for preparing a wood-plastic material adhesive for construction according to claim 3, Features: In the step A2, the temperature of each barrel of the twin-screw extruder is 130-190°C.
9. The method for preparing a wood-plastic material adhesive for construction according to claim 3, Features: In the step A2, the main engine speed of the twin-screw extruder is 350-550 rpm.
10. The method for preparing a wood-plastic material adhesive for construction according to claim 3, Features: The initiator A and initiator B may be the same or different.
Citation Information
Cited By
Environment-friendly medicinal composite packaging film and preparation method thereof
CN120399302A