Two-component polyurethane heat-conducting structural adhesive and preparation method thereof

By adjusting the dosage and molecular weight of double-ended hydroxy polyether modified silicone oil, polydiol and hyperbranched polyester polyol, and adjusting the crosslinking point structure of polyurethane structural glue, the large elastic modulus of polyurethane thermal conductivity structural glue in the prior art is solved. , the problem of low displacement ductility achieves the effect of improving elongation of break without deteriorating heat conductivity and bonding properties.

CN118879262APending Publication Date: 2024-11-01COLLTECH DONGGUAN BONDING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410979046.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing polyurethane thermally conductive structural adhesives have large elastic modulus and low displacement ductility when subjected to vibration loads, resulting in low reliability of the battery module and it is difficult to improve the elongation of break without deteriorating the thermal conductivity and bonding properties.

Method used

Using double-ended hydroxy polyether modified silicone oil, polydiol and hyperbranched polyester polyol as raw materials, the crosslinking point structure type and crosslinking degree of polyurethane structural glue is adjusted by adjusting the dosage and molecular weight, reducing the elastic modulus and improving the Tensile elongation at break.

Benefits of technology

On the basis of maintaining thermal conductivity and bonding properties, the elastic modulus is significantly reduced, the elongation of break is improved, and the energy absorption capacity of structural glue and the reliability of the battery module are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004955477500000031
    Figure BDA0004955477500000031
  • Figure BDA0004955477500000051
    Figure BDA0004955477500000051
  • Figure BDA0004955477500000061
    Figure BDA0004955477500000061
Patent Text Reader

Abstract

The invention provides a two-component polyurethane heat-conducting structural adhesive and a preparation method thereof, the two-component polyurethane heat-conducting structural adhesive comprises a component A and a component B, and the mass ratio of the component A to the component B is 1: (1-1.5); the component A is prepared from the following raw materials in parts by weight: 20 to 30 parts of dihydroxyl-terminated polyether modified silicone oil, 8 to 10 parts of polydihydric alcohol, 5 to 8 parts of hyperbranched polyester polyol, 50 to 70 parts of heat-conducting filler, 0.5 to 1.5 parts of silane coupling agent, 0.5 to 1 part of thixotropic agent, 1 to 2 parts of molecular sieve and 0.05 to 0.3 part of catalyst; the component B is prepared from the following raw materials in parts by weight: 15 to 25 parts of isocyanate, 5 to 10 parts of polydihydric alcohol, 50 to 70 parts of heat-conducting filler, 0.5 to 1.5 parts of silane coupling agent, 0.5 to 1 part of thixotropic agent and 1 to 2 parts of molecular sieve; the hydroxyl value of the hyperbranched polyester polyol is 600 to 700 mg KOH / g. The two-component polyurethane heat-conducting structural adhesive disclosed by the invention can achieve the purposes of reducing the elastic modulus and improving the tensile elongation at break on the premise of not reducing the existing heat-conducting and adhesive properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyurethane thermal conductive structural adhesives, and in particular relates to a two-component polyurethane thermal conductive structural adhesive and a preparation method thereof. Background Art

[0002] As one of the most critical components of new energy vehicles, power batteries provide a source of power for them, directly affecting the performance of new energy vehicles such as cruising range, safety, service life, charging time and temperature adaptability. Two-component polyurethane thermal conductive structural adhesive has the characteristics of light weight, strong bonding, high toughness, good insulation and high thermal conductivity. It has been widely used in the assembly and installation of power batteries, replacing traditional mechanical connection methods such as rivets, bolts and even welding, to achieve structural bonding, sealing, heat dissipation of power batteries and lightweighting of vehicles.

[0003] For example, the high temperature resistant heat conductive polyurethane structural adhesive and its preparation method disclosed in patent CN115785887B, in terms of mass percentage, component A: 5.0% to 15.0% polyether polyol, 3.0% to 7.0% chain extender, 3.5% to 16.0% modified castor oil, 0 to 5.0% diluent, 65.0% to 80.0% thermal conductive filler, 0.1% to 2.0% thixotropic agent, 0.5% to 1.0% silane coupling agent, 0.5% to 4.0% first water absorbent, 0.01% to 0.3% catalyst; component B: 12.0% to 25.0% isocyanate, 5.0% to 12.0% polyester polyol, 0.1% to 0.3% second water absorbent, 65.0% to 80.0% thermal conductive filler, 0.1% to 2.0% thixotropic agent, and 0.5% to 1.0% silane coupling agent. Patent CN115558457B discloses a two-component polyurethane structural adhesive and a preparation method and application thereof, comprising component A and component B, wherein component A comprises the following components in parts by weight: 10 to 40 parts of NCO-terminated polyurethane prepolymer; 0 to 30 parts of polymethylene polyphenyl polyisocyanate; 50 to 80 parts of thermal conductive filler A; and 1 to 4 parts of dewatering agent A; and component B comprises the following components in parts by weight: 5 to 30 parts of castor oil polyol; 2 to 20 parts of aromatic polyether polyol; 1 to 10 parts of non-halogenated phosphorus polyol; 1 to 8 parts of aldehyde-ketone resin; 50 to 80 parts of thermal conductive filler B; and 1 to 3 parts of dewatering agent B.

[0004] The car vibrates during driving. During long driving, the battery module will be stretched or torn due to vibration load, resulting in damage or failure. As a component that bears greater stress, the structural adhesive needs to have a higher elongation at break to ensure sufficient deformation space before damage, that is, it can gradually deform and ductile fracture when bearing load, rather than suddenly fracture, so as to improve the energy absorption capacity of the structural adhesive and reduce the risk of damage to the battery module. Although the above polyurethane thermal conductive structural adhesive has good bonding properties, thermal conductivity, and insulation properties, and meets the requirements of power batteries for bonding, rapid heat dissipation, etc., it has a large elastic modulus and a relatively small displacement ductility, and the reliability of the battery module is low.

[0005] Therefore, there is an urgent need for a polyurethane thermally conductive structural adhesive that has a lower elastic modulus and a higher elongation at break without reducing the existing strength and bonding properties of the polyurethane thermally conductive structural adhesive. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a two-component polyurethane thermal conductive structural adhesive and a preparation method thereof. The present invention uses double-terminal hydroxyl polyether modified silicone oil and polyglycol as raw material polyhydroxy compounds, and hyperbranched polyester polyol as a cross-linking agent. By changing the dosage and size of the three, the cross-linking point structure type, cross-linking degree, and flexibility of the molecular chain between the cross-linking points of the polyurethane structural adhesive are adjusted to achieve the purpose of reducing the elastic modulus and improving the tensile elongation at break without reducing the existing thermal conductivity and bonding properties.

[0007] To achieve the above object, the present invention adopts the following technical solutions:

[0008] A two-component polyurethane thermal conductive structural adhesive, comprising components A and B, wherein the mass ratio of components A to B is 1:1-1.5;

[0009] Component A comprises the following raw materials in parts by weight: 20-30 parts of double-terminal hydroxyl polyether modified silicone oil, 8-10 parts of polyglycol, 5-8 parts of hyperbranched polyester polyol, 50-70 parts of thermal conductive filler, 0.5-1.5 parts of silane coupling agent, 0.5-1 parts of thixotropic agent, 1-2 parts of molecular sieve, and 0.05-0.3 parts of catalyst;

[0010] Component B includes the following raw materials in parts by weight: 15-25 parts of isocyanate, 5-10 parts of polyglycol, 50-70 parts of thermal conductive filler, 0.5-1.5 parts of silane coupling agent, 0.5-1 parts of thixotropic agent, and 1-2 parts of molecular sieve;

[0011] The hyperbranched polyester polyol has a hydroxyl value of 600-700 mg KOH / g.

[0012] Furthermore, the weight average molecular weight of the hyperbranched polyester polyol is 500-1200 g / mol, and is specifically selected from one or a combination of two or more of HyPer101 and HyPer102; preferably HyPer102.

[0013] The double-terminated hydroxyl polyether modified silicone oil has a weight average molecular weight of 1000-4000 g / mol, and is specifically selected from one or a combination of two or more of SF 8427, BY16-201, and OFX-3667 from Dow Corning.

[0014] The weight average molecular weight of the polyglycol is 500-1000 g / mol; it is specifically selected from polyester diol and polyether diol or a combination of both.

[0015] The isocyanate is selected from one or a combination of two or more of 4,4'-diphenylmethane diisocyanate and toluene diisocyanate.

[0016] The thermal conductive filler is selected from one or a combination of two or more of aluminum oxide, magnesium oxide, aluminum hydroxide, boron nitride and aluminum nitride.

[0017] The silane coupling agent is selected from one or a combination of two or more of γ-aminopropyl triethoxysilane, γ-(2,3-epoxypropyloxy)propyl trimethoxysilane, γ-methacryloxypropyl trimethoxysilane, 3-glycidyloxypropyl triethoxysilane, N-β-(aminoethyl)-γ-aminopropyl trimethoxysilane, γ-mercaptopropyl triethoxysilane, γ-mercaptopropyl trimethoxysilane, N-β-(aminoethyl)-γ-aminopropyl methyldimethoxysilane, γ-isocyanatepropyl triethoxysilane, 1,3,5-tris(trimethoxysilylpropyl)isocyanurate, and γ-aminoethylaminopropyl trimethoxysilane.

[0018] The catalyst is selected from one or a combination of two or more of an organic tin catalyst, an organic bismuth catalyst, an organic zinc catalyst, and an organic zirconium catalyst.

[0019] The thixotropic agent is selected from one or a combination of two or more of fumed silica, organic bentonite and hydrogenated castor oil.

[0020] The molecular sieve has an average particle size of 1-10 μm and is selected from one of 3A molecular sieve, 4A molecular sieve, 5A molecular sieve, and 13X molecular sieve, or a combination of two or more thereof.

[0021] The present invention also provides a method for preparing the above-mentioned two-component polyurethane thermal conductive structural adhesive, comprising the following steps:

[0022] 1) Preparation of component A: mixing double-terminated hydroxyl polyether modified silicone oil, polyglycol, hyperbranched polyester polyol, thermal conductive filler, thixotropic agent and molecular sieve, heating, dehydrating, cooling, adding silane coupling agent and catalyst, mixing, degassing to obtain component A;

[0023] 2) Preparation of component B: heating the polyglycol, dehydrating it, cooling it, adding isocyanate to react, adding thermal conductive filler, silane coupling agent, thixotropic agent, and molecular sieve to mix, thus obtaining component B;

[0024] 3) Component A and component B are mixed evenly according to the mass ratio to obtain a two-component polyurethane thermal conductive structural adhesive.

[0025] In step 1), the temperature is raised to 110-130° C., the dehydration is carried out at -0.085 MPa to -0.1 MPa for 2-3 h, the temperature is lowered to 20-50° C., and the degassing is carried out at -0.085 MPa to -0.1 MPa for 0.5-2 h.

[0026] Step 2) The temperature is raised to 110-130°C, the dehydration is carried out at -0.085MPa to -0.1MPa for 1-3h, the temperature is lowered to 80-90°C, and the reaction time is 2-3h.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The present invention uses the above-mentioned double-terminal hydroxyl polyether modified silicone oil and polymer diol as the raw material polyhydroxy compounds of polyurethane, and uses hyperbranched polyester polyol as the raw material cross-linking agent of polyurethane. By changing the dosage and size of the three, the cross-linking point structure type, cross-linking degree, and the flexibility of the molecular chain between the cross-linking points of the polyurethane structural adhesive are adjusted, so as to achieve the purpose of reducing the elastic modulus and improving the tensile elongation at break without reducing the existing thermal conductivity and bonding properties. DETAILED DESCRIPTION

[0029] The present invention will be further described below in conjunction with specific embodiments, but is not limited to the contents of the specification. Unless otherwise specified, the "parts" described in the embodiments of the present invention are all parts by weight. The reagents used are all commercially available reagents in the art.

[0030] Double-terminated hydroxyl polyether modified silicone oil: Dow Corning SF8427; Dow Corning BY16-201.

[0031] Polyoxypropylene glycol was purchased from Shanghai Chuangsai Technology Co., Ltd. with weight average molecular weights of 1000 g / mol, 500 g / mol, 3000 g / mol, and 100 g / mol.

[0032] Hyperbranched polyester polyols were purchased from Wuhan Hyperbranched Resin Technology Co., Ltd. The performance indicators of the HyPer H10 series are as follows:

[0033]

[0034] Fumed silica was purchased from Evonik Chemical Co., Ltd., brand XH-202.

[0035] 4A molecular sieve was purchased from Pingxiang Jianghua Environmental Protection Equipment Filler Co., Ltd. with an average particle size of 2.5 μm.

[0036] The thermal conductive filler spherical alumina, DAM-07, was purchased from DENKA Corporation.

[0037] Example 1

[0038] 1) Preparation of component A: 20 parts of Dow Corning SF8427, 10 parts of polyoxypropylene glycol with a weight average molecular weight of 1000 g / mol, 5 parts of hyperbranched polyester polyol HyPerH102, 70 parts of spherical alumina DAM-07, 1 part of fumed silica XH-202, and 1 part of 4A molecular sieve were mixed, heated to 120° C., dehydrated at -0.085 MPa for 2 h, cooled, and then 1 part of γ-aminopropyltriethoxysilane and 0.2 parts of dibutyltin dilaurate were added and mixed, and degassed to obtain component A;

[0039] 2) Preparation of component B: 10 parts of polyoxypropylene glycol with a weight average molecular weight of 1000 g / mol were heated to 120° C., dehydrated at -0.085 MPa for 2 h, cooled to 80° C., 25 parts of 4,4'-diphenylmethane diisocyanate were added to react for 3 h, 70 parts of spherical alumina DAM-07, 1 part of γ-aminopropyltriethoxysilane, 1 part of fumed silica XH-202, and 1 part of 4A molecular sieve were added and mixed to obtain component B;

[0040] 3) The above-mentioned component A and component B are mixed evenly in a mass ratio of 1:1 to obtain a two-component polyurethane thermal conductive structural adhesive.

[0041] Example 2

[0042] The rest is the same as Example 1, except that HyPer H102 is replaced by HyPer H101 of equal mass.

[0043] Example 3

[0044] The rest is the same as Example 1, except that the amount of the hyperbranched polyester polyol HyPer H102 used is 10 parts.

[0045] Example 4

[0046] The rest is the same as Example 1, except that the weight average molecular weight of polyoxypropylene glycol is 500 g / mol.

[0047] Example 5

[0048] The rest is the same as Example 1, except that the weight average molecular weight of polyoxypropylene glycol is 100 g / mol.

[0049] Example 6

[0050] The rest is the same as Example 1, except that the weight average molecular weight of polyoxypropylene glycol is 3000 g / mol.

[0051] Example 7

[0052] The rest is the same as Example 1, except that Dow Corning BY16-201 of equal mass is used to replace Dow Corning SF8427.

[0053] Example 8

[0054] The rest is the same as Example 1, except that the amount of Dow Corning SF 8427 is 30 parts.

[0055] Example 9

[0056] 1) Preparation of component A: 30 parts of Dow Corning SF 8427, 8 parts of polyoxypropylene glycol with a weight average molecular weight of 1000 g / mol, 10 parts of hyperbranched polyester polyol HyPer H102, 70 parts of spherical alumina DAM-07, 1 part of fumed silica XH-202, and 1 part of 4A molecular sieve were mixed, heated to 120° C., dehydrated at -0.085 MPa for 2 h, cooled, and then 1 part of γ-aminopropyltriethoxysilane and 0.2 parts of dibutyltin dilaurate were added and mixed, and degassed to obtain component A;

[0057] 2) Preparation of component B: 8 parts of polyoxypropylene glycol with a weight average molecular weight of 1000 g / mol were heated to 120° C., dehydrated at -0.085 MPa for 2 h, cooled to 80° C., added with 20 parts of 4,4'-diphenylmethane diisocyanate for reaction for 3 h, and then 70 parts of spherical alumina DAM-07, 1 part of γ-aminopropyltriethoxysilane, 1 part of fumed silica XH-202, and 1 part of 4A molecular sieve were added and mixed to obtain component B;

[0058] 3) The above-mentioned component A and component B are mixed evenly in a mass ratio of 1:1.5 to obtain a two-component polyurethane thermal conductive structural adhesive.

[0059] Comparative Example 1

[0060] The rest is the same as Example 1, except that Dow Corning SF 8427 is replaced by an equal amount of polyoxypropylene glycol having a weight average molecular weight of 3000 g / mol.

[0061] Comparative Example 2

[0062] The rest is the same as Example 1, except that HyPer H102 is replaced by HyPer H103 of equal mass.

[0063] Comparative Example 3

[0064] The rest is the same as Example 1, except that an equal mass of trimethylolpropane is used to replace HyPer H102.

[0065] Comparative Example 4

[0066] The rest is the same as Example 1, except that the amount of Dow Corning SF 8427 is 35 parts.

[0067] Comparative Example 5

[0068] The rest is the same as Example 1, except that the amount of Dow Corning SF 8427 is 15 parts.

[0069] The structural adhesives prepared in the above examples and comparative examples were subjected to the following performance tests:

[0070] Modulus: DMA8000 dynamic thermomechanical analyzer was used, the tensile method was adopted, the frequency was 500 Hz, the heating rate was 20-200°C, and the modulus data at 25°C were obtained by analyzing the curve.

[0071] Elongation at break: Elongation at break was tested according to ASTM D412.

[0072] Adhesion performance: Referring to the standard GB / T 7124-2008 Determination of tensile shear strength of adhesives (rigid material to rigid material), the single lap tensile shear strength of 30003 aluminum alloy and 30003 aluminum alloy was tested, the tensile speed was 2mm / min, the number of specimens was 5, and the maximum shear failure load was recorded as the failure load. The test results were expressed as the arithmetic mean of the tensile shear strength, and the tensile shear strength was calculated by dividing the failure load by the shear area.

[0073] Fatigue performance: GB / T 27595-2011 Adhesive structural adhesive tensile shear fatigue performance test method, adhesive layer thickness 0.2mm, frequency 60Hz, amplitude τa 0.3MPa, cycle 10 6 The above bonding properties were retested and the tensile shear strength retention rate was calculated.

[0074] Table 1 Performance test results

[0075]

[0076]

[0077] Since the molecular weight of hyperbranched polyester polyols of different generations is quite different, it has a direct impact on the number, structure and degree of crosslinking points. Changing the dosage or the hyperbranched polyester polyols of different hydroxyl values ​​significantly changes the tensile properties and tensile shear strength of the structural adhesive. The performance test results of Example 1, Example 2 and Comparative Example 2 can confirm that the structural adhesive using HyPer H103 with a hydroxyl value of 560 mgKOH / g and a large weight-average molecular weight can significantly reduce the number of crosslinking points, resulting in a significant decrease in the elastic modulus and cohesion, and an imbalance in the elastic modulus, elongation and bonding strength.

[0078] Polyoxypropylene glycol and double-terminated hydroxyl polyether modified silicone oils of different molecular weights have a great influence on the molecular weight and intermolecular interaction between crosslinking points. Changing the dosage or molecular weight has a direct impact on the elongation, modulus and strength of the structural adhesive, which can be confirmed by the performance test results of Example 1, Example 4-5 and Example 7.

[0079] It can be seen from the above embodiments and comparative examples that only by using double-terminal hydroxyl polyether modified silicone oil and polymer diol as the raw material polyhydroxy compounds of polyurethane and hyperbranched polyester polyol as the raw material cross-linking agent of polyurethane, and by changing the dosage and size of the three to adjust the cross-linking point structure type, cross-linking degree, and the flexibility of the molecular chain between the cross-linking points of the polyurethane structural adhesive, can the purpose of reducing the elastic modulus and improving the tensile elongation at break be achieved without reducing the existing thermal conductivity and bonding properties.

[0080] The above detailed description is a specific description of one feasible embodiment of the present invention. The embodiment is not intended to limit the patent scope of the present invention. Any equivalent implementation or modification that does not deviate from the present invention should be included in the scope of the technical solution of the present invention.

Claims

1. A two-component polyurethane thermal conductive structural adhesive, characterized in that: It includes components A and B, and the mass ratio of components A to B is 1:1-1.5; Component A comprises the following raw materials in parts by weight: 20-30 parts of double-terminal hydroxyl polyether modified silicone oil, 8-10 parts of polyglycol, 5-8 parts of hyperbranched polyester polyol, 50-70 parts of thermal conductive filler, 0.5-1.5 parts of silane coupling agent, 0.5-1 parts of thixotropic agent, 1-2 parts of molecular sieve, and 0.05-0.3 parts of catalyst; Component B includes the following raw materials in parts by weight: 15-25 parts of isocyanate, 5-10 parts of polyglycol, 50-70 parts of thermal conductive filler, 0.5-1.5 parts of silane coupling agent, 0.5-1 parts of thixotropic agent, and 1-2 parts of molecular sieve; The hyperbranched polyester polyol has a hydroxyl value of 600-700 mg KOH / g.

2. The two-component polyurethane thermal conductive structural adhesive according to claim 1, characterized in that: The weight average molecular weight of the hyperbranched polyester polyol is 500-1200 g / mol, and is specifically selected from one or a combination of two or more of HyPer101 and HyPer102; preferably HyPer102.

3. The two-component polyurethane thermal conductive structural adhesive according to claim 1, characterized in that: The double-terminated hydroxyl polyether modified silicone oil has a weight average molecular weight of 1000-4000 g / mol, and is specifically selected from one or a combination of two or more of SF 8427, BY16-201, and OFX-3667 from Dow Corning.

4. The two-component polyurethane thermal conductive structural adhesive according to claim 1, characterized in that: The weight average molecular weight of the polyglycol is 500-1000 g / mol; it is specifically selected from polyester diol and polyether diol or a combination of both.

5. The two-component polyurethane thermal conductive structural adhesive according to claim 1, characterized in that: The isocyanate is selected from one or a combination of two or more of 4,4'-diphenylmethane diisocyanate and toluene diisocyanate.

6. The two-component polyurethane thermal conductive structural adhesive according to claim 1, characterized in that: The thermal conductive filler is selected from one or a combination of two or more of aluminum oxide, magnesium oxide, aluminum hydroxide, boron nitride and aluminum nitride.

7. The two-component polyurethane thermal conductive structural adhesive according to claim 1, characterized in that: The catalyst is selected from one or a combination of two or more of an organic tin catalyst, an organic bismuth catalyst, an organic zinc catalyst, and an organic zirconium catalyst.

8. The two-component polyurethane thermal conductive structural adhesive according to claim 1, characterized in that: The molecular sieve has an average particle size of 1-10 μm and is selected from one of 3A molecular sieve, 4A molecular sieve, 5A molecular sieve, and 13X molecular sieve, or a combination of two or more thereof.

9. The method for preparing the two-component polyurethane thermal conductive structural adhesive according to any one of claims 1 to 8, characterized in that: The steps include: 1) Preparation of component A: mixing double-terminated hydroxyl polyether modified silicone oil, polyglycol, hyperbranched polyester polyol, thermal conductive filler, thixotropic agent and molecular sieve, heating, dehydrating, cooling, adding silane coupling agent and catalyst, mixing, degassing to obtain component A; 2) Preparation of component B: heating the polyglycol, dehydrating it, cooling it, adding isocyanate to react, adding thermal conductive filler, silane coupling agent, thixotropic agent, and molecular sieve to mix, thus obtaining component B; 3) Component A and component B are mixed evenly according to the mass ratio to obtain a two-component polyurethane thermal conductive structural adhesive.

10. The method for preparing the two-component polyurethane thermal conductive structural adhesive according to claim 9, characterized in that: In step 1), the temperature is raised to 110-130°C, the dehydration is carried out at -0.085MPa to -0.1MPa for 2-3h, the temperature is lowered to 20-50°C, and the degassing is carried out at -0.085MPa to -0.1MPa for 0.5-2h; in step 2), the temperature is raised to 110-130°C, the dehydration is carried out at -0.085MPa to -0.1MPa for 1-3h, the temperature is lowered to 80-90°C, and the reaction time is 2-3h.