Phase change polyurethane material and preparation method thereof

By using puffed vanadium trioxide and chromium ion modified dopamine polyurethane in phase change polyurethane materials, the problem of separation and layering of the material during circulation is solved, and the thermal cycling and conductive properties are improved, satisfying various applications need.

CN118879283AInactive Publication Date: 2024-11-01SICHUAN KAIGAN CARBON NANOTECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411113773.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the repeated cycle of heat absorption/exothermic process of existing vanadium dioxide modified polyurethane phase change materials, they are prone to separation and separation, resulting in uneven functional structures, weakening of thermal cycling performance, and it is difficult to maintain the initial phase change performance.

Method used

Use puffed vanadium trioxide as aggregate and fill it with chromium ion modified dopamine polyurethane. Through the high-density corundum configuration and capillary adsorption, the modified polyurethane filler is stably distributed to maintain the uniform and stable phase change material during the circulation process. sex.

Benefits of technology

The thermal cycling performance stability and conductivity of phase change materials are improved, meeting the needs of more application scenarios, while maintaining high thermal insulation performance and thermal conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004993054920000151
    Figure BDA0004993054920000151
Patent Text Reader

Abstract

The invention relates to the technical field of polyurethane, and discloses a phase-change polyurethane material and a preparation method thereof in order to solve the problem that an existing polyurethane phase-change material is difficult to meet the use requirements in multiple aspects at the same time, and the phase-change polyurethane material comprises vanadium trioxide aggregate and modified polyurethane filler filled in the vanadium trioxide aggregate; the modified polyurethane filler is formed by polymerizing Cr < (at) dopamine and isocyanate, and the Cr < (at) dopamine is modified dopamine doped with divalent chromium ions. Expanded vanadium trioxide is adopted as aggregate, dopamine polyurethane combined with chromium ions is filled, through a high-density corundum configuration structure, a material frame with a stable form is provided for a polyurethane base material, the phase change base material is kept uniform and stable in the cyclic heat absorption and release process, meanwhile, the volume change of the material before and after phase change is reduced, and the phase change performance of the material is improved. Meanwhile, the material is endowed with good heat insulation performance and conductivity, and the use requirements of low-temperature application scenes and other application scenes can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polyurethane, and in particular to a phase change polyurethane material and a preparation method thereof. Background Art

[0002] Phase Change Material (PCM) is a material with unique functions, that is, a material that changes its state within a specific temperature range and can provide latent heat. The process of changing physical properties is called a phase change process. At this time, the phase change material can absorb or release a large amount of latent heat to achieve temperature regulation and energy conversion. Common phase change materials basically use polymer materials such as polyurethane as the matrix, and use their good plasticity and processability to make phase change materials that can be applied to different scenarios or different specific requirements.

[0003] For example, the patent with publication number CN112500697A provides a polydopamine-coated tungsten-doped vanadium dioxide modified polyurethane solid-solid phase change material and a preparation method thereof. Polydopamine-coated tungsten-doped vanadium dioxide nanoparticles are added to the polyurethane material system to react to form a polydopamine-coated tungsten-doped vanadium dioxide modified polyurethane solid-solid phase change material, which can not only improve the thermal responsiveness of the material, but also improve its photothermal conversion efficiency. Combined with the good energy storage and temperature regulation properties of the polyurethane solid-solid phase change material, it is applied to fabrics to further improve the energy storage and temperature regulation effects of the fabrics.

[0004] However, the currently proposed method of improving the polyurethane material system with vanadium dioxide to prepare phase change materials can improve the thermal conductivity of the phase change materials, etc. However, the thermal insulation and electrical conductivity of the existing polyurethane materials obtained by vanadium dioxide modification are difficult to meet higher usage requirements, and the material performance stability is relatively weak. Summary of the invention

[0005] The technical problems to be solved by the present invention are:

[0006] Existing polyurethane phase change materials are difficult to take into account multiple performance effects at the same time. For example, vanadium dioxide modified polyurethane phase change materials have poor electrical conductivity and other problems, which make it difficult to meet the needs of different application scenarios. The existing treatment methods for improving thermal insulation and electrical conductivity can easily lead to the gradual separation and stratification of the phase change material from a uniform composite system during the repeated cycle of heat absorption / exothermic process, and the functional structural units tend to transform into an inhomogeneous form, which leads to the weakening of the thermal cycle performance of the phase change material, making it difficult to maintain the phase change performance in the initial stage.

[0007] The technical solution adopted by the present invention is:

[0008] The invention provides a phase change polyurethane material, comprising vanadium trioxide aggregate and modified polyurethane filler filled in the vanadium trioxide aggregate; the modified polyurethane filler is formed by polymerization of Cr@dopamine and isocyanate, and the Cr@dopamine is modified dopamine doped with divalent chromium ions.

[0009] Preferably, the preparation method of Cr@dopamine comprises the following steps: placing dopamine hydrochloride in a solvent, mixing, adding chromium salt and a catalyst, stirring and reacting at 20-25° C. to obtain the Cr@dopamine.

[0010] Preferably, before adding the chromium salt and the catalyst, the pH value is adjusted to 5-6 using hydrochloric acid.

[0011] Preferably, based on molar weight, the ratio of dopamine hydrochloride to chromium ions in the chromium salt is 1-1.2:0.8-1.35.

[0012] Preferably, the preparation method of the modified polyurethane filler comprises the following steps: mixing Cr@dopamine and isocyanate, adding a catalyst, stirring and reacting for 20-50 hours to obtain the modified polyurethane filler.

[0013] Preferably, the molecular ratio of Cr@dopamine to isocyanate is 0.95-1.35:0.4-1.

[0014] Preferably, the volume ratio of the modified polyurethane filler to the vanadium trioxide aggregate is 0.75-1:0.8-1.2.

[0015] The present invention also provides a method for preparing the phase change polyurethane material, comprising the following steps:

[0016] (1) mixing vanadium trioxide aggregate with fiber xylan, a compatibilizer, and a dispersant, adding the mixture to a solvent, and performing ultrasonic dispersion to obtain a dispersed liquid;

[0017] (2) adding modified polyurethane filler to the dispersion liquid, heating for reaction, ultrasonic dispersion, and curing and forming to obtain the phase change polyurethane material.

[0018] Preferably, in step (1), the method for preparing vanadium trioxide aggregate comprises the following steps: taking ammonium vanadate or ammonium metavanadate, first heating it to 400-450°C for roasting, then cooling it to 80-100°C, adding oxalic acid solution, and stirring for reaction; after the reaction is completed, removing the solvent, performing an expansion treatment at 500-800°C in an inert gas atmosphere, and cooling to obtain the vanadium trioxide aggregate.

[0019] Preferably, in step (1), the vanadium trioxide aggregate accounts for 40-65wt% of the total mass of the dispersed liquid.

[0020] The beneficial effects of the present invention are as follows:

[0021] The present invention adopts expanded vanadium trioxide as aggregate and fills dopamine polyurethane combined with chromium ions. Through the high-density corundum configuration structure, a material framework with stable shape is provided for the polyurethane base material. Through the capillary adsorption effect, the modified polyurethane filler can be stably distributed in the aggregate cavity, which can not only maintain the uniformity and stability of the phase change base material in the cyclic heat absorption and release process, but also reduce the volume change of the material before and after the phase change, thereby maintaining the stability of the use performance of the phase change material; in addition, through the vanadium trioxide aggregate and the used Cr@dopamine polyurethane polymerization monomer, the phase change polyurethane material can have good thermal insulation and electrical conductivity, which can meet the use requirements of more application scenarios. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0023] The invention provides a phase change polyurethane material, comprising vanadium trioxide aggregate and modified polyurethane filler filled in the vanadium trioxide aggregate; the modified polyurethane filler is formed by polymerization of Cr@dopamine and isocyanate, and the Cr@dopamine is modified dopamine doped with divalent chromium ions.

[0024] The present invention adopts expanded vanadium trioxide as aggregate and fills dopamine polyurethane combined with chromium ions. Through the high-density corundum configuration structure, a material framework with stable shape is provided for the polyurethane base material. Through capillary adsorption, the modified polyurethane filler can be stably distributed in the aggregate cavity, which can not only keep the phase change base material uniform and stable during the cyclic heat absorption and release process, but also reduce the volume change of the material before and after the phase change, thereby maintaining the stable performance of the phase change material.

[0025] The preparation method of the phase change polyurethane material of the present invention comprises the following steps:

[0026] (1) Preparation of dispersion liquid

[0027] Take ammonium vanadate or ammonium metavanadate, heat it to 400-450°C for roasting, then cool it to 80-100°C, add oxalic acid solution, and stir to react; after the reaction is completed, evaporate and dry, remove the solvent, and heat it to 500-800°C under the protection of inert gas, expand it for 0.5-4h, and cool it to obtain expanded vanadium trioxide with high-density corundum configuration, which is used as vanadium trioxide aggregate;

[0028] Take fiber xylan, compatibilizer and dispersant respectively, add them into solvent and mix well; then add expanded vanadium trioxide, and control the vanadium trioxide aggregate to account for 10-65wt% of the total mass of dispersed liquid, and perform ultrasonic dispersion for 2-5h to obtain dispersed liquid.

[0029] (2) Preparation of modified polyurethane filler

[0030] Place dopamine hydrochloride in a solvent, stir to mix evenly, adjust the pH value to acidic, preferably pH=5-6, add chromium salt and catalyst, control the molar mass ratio of dopamine hydrochloride to chromium ion in chromium salt to be 1-1.2:0.8-1.35, stir and react at room temperature of 20-25°C for 25-30h to obtain Cr@dopamine;

[0031] In a low temperature environment of 3-7°C, Cr@dopamine and isocyanate are mixed and stirred, the molecular ratio of Cr@dopamine to isocyanate is controlled to be 0.95-1.35:0.4-1, a catalyst is added, and the temperature is restored to room temperature, and the reaction is continued by stirring at a low speed for 20-50 hours to obtain a modified polyurethane filler.

[0032] Among them, chromium salts can be chromous acetate, sodium dichromate, etc. When reacting in an acidic environment, chromium is a divalent ion and can be connected to dopamine to form Cr 2+ The doped dopamine material, through the vanadium trioxide aggregate and the used Cr@dopamine polyurethane polymerization monomer, can enable the phase change polyurethane material to exert a good thermal conductivity; the catalyst can be hydrogen peroxide, sodium hypochlorite, etc.

[0033] (3) Preparation of phase change polyurethane materials

[0034] The modified polyurethane filler is placed in a dispersion liquid, wherein the volume ratio of the modified polyurethane filler to the vanadium trioxide aggregate in the dispersion liquid is 0.75-1:0.8-1.2, heated to 30-45°C, ultrasonically dispersed for 10-15 hours, and then cured and formed by injection molding, calendering, etc. to obtain a phase change polyurethane material.

[0035] Example 1

[0036] Take 10 mol of ammonium metavanadate, place it in a reactor, heat it to 420±5°C, roast it for 6.5h, then cool it to 85±2°C, add 15 mol of oxalic acid and 2.5L of deionized water, stir it continuously at 600r / min, and keep it warm for reaction; after the reaction is completed, filter it, rinse it with deionized water three times, and then remove the residual solvent by evaporation and drying; then place it in a reactor filled with nitrogen, heat it to 780°C, and perform an expansion treatment for 0.75h, then take it out and cool it to obtain expanded vanadium trioxide, which is placed in a nitrogen atmosphere for storage for later use.

[0037] Take another 10g of dopamine hydrochloride, put it into 1L of deionized water, stir at 750r / min to mix, and adjust the pH value to 5.5±0.1 with 0.5M hydrochloric acid; add 8.5g of sodium dichromate and 0.1g of hydrogen peroxide, place it at about 22°C, continue stirring and react for 26.5h to obtain Cr@dopamine, which is stored for later use.

[0038] In a low temperature environment of about 5°C, take equal molar masses of Cr@dopamine and diphenylmethane diisocyanate, mix them, add 0.5wt% triethylamine, and then return to room temperature. During this period, stir and react at 200r / min for 35h to obtain a modified polyurethane filler, which is stored for later use.

[0039] Take fiber xylan, maleic anhydride and sodium dodecylbenzene sulfonate separately, fiber xylan is a hemicellulose polysaccharide extracted from corn bran, add them to tetrahydrofuran, stir and mix; then add expanded vanadium trioxide, and the expanded vanadium trioxide accounts for 55wt% of the total mass of the materials in this step, ultrasonically disperse for 4.5h to obtain a dispersed liquid; then add modified polyurethane filler to the dispersed liquid, and the volume ratio of the modified polyurethane filler to the expanded vanadium trioxide in the dispersed liquid needs to be controlled to be 0.75:1, mix well, heat to 35°C, ultrasonically disperse for 12h, add a curing agent for injection molding, and obtain a phase change polyurethane material.

[0040] Example 2

[0041] Take 10 mol of ammonium metavanadate, place it in a reactor, heat it to 420±5°C, roast it for 6.5h, then cool it to 85±2°C, add 15 mol of oxalic acid and 2.5L of deionized water, stir it continuously at 600r / min, and keep it warm for reaction; after the reaction is completed, filter it, rinse it with deionized water three times, and then remove the residual solvent by evaporation and drying; then place it in a reactor filled with nitrogen, heat it to 780°C, and perform an expansion treatment for 0.75h, then take it out and cool it to obtain expanded vanadium trioxide, which is placed in a nitrogen atmosphere for storage for later use.

[0042] Take another 10g of dopamine hydrochloride, put it into 1L of deionized water, stir at 750r / min to mix, and adjust the pH value to 5.5±0.1 with 0.5M hydrochloric acid; add 2.5g of sodium dichromate and 0.1g of hydrogen peroxide, place it at about 22°C, continue stirring and react for 26.5h to obtain Cr@dopamine, which is stored for later use.

[0043] In a low temperature environment of about 5°C, take equal molar masses of Cr@dopamine and diphenylmethane diisocyanate, mix them, add 0.5wt% triethylamine, and then return to room temperature. During this period, stir and react at 200r / min for 35h to obtain a modified polyurethane filler, which is stored for later use.

[0044] Take fiber xylan, maleic anhydride and sodium dodecylbenzene sulfonate separately, fiber xylan is a hemicellulose polysaccharide extracted from corn bran, add them to tetrahydrofuran, stir and mix; then add expanded vanadium trioxide, and the expanded vanadium trioxide accounts for 55wt% of the total mass of the materials in this step, ultrasonically disperse for 4.5h to obtain a dispersed liquid; then add modified polyurethane filler to the dispersed liquid, and the volume ratio of the modified polyurethane filler to the expanded vanadium trioxide in the dispersed liquid needs to be controlled to be 0.75:1, mix well, heat to 35°C, ultrasonically disperse for 12h, add a curing agent for injection molding, and obtain a phase change polyurethane material.

[0045] Example 3

[0046] Take 10 mol of ammonium metavanadate, place it in a reactor, heat it to 420±5°C, roast it for 6.5h, then cool it to 85±2°C, add 15 mol of oxalic acid and 2.5L of deionized water, stir it continuously at 600r / min, and keep it warm for reaction; after the reaction is completed, filter it, rinse it with deionized water three times, and then remove the residual solvent by evaporation and drying; then place it in a reactor filled with nitrogen, heat it to 780°C, and perform an expansion treatment for 0.75h, then take it out and cool it to obtain expanded vanadium trioxide, which is placed in a nitrogen atmosphere for storage for later use.

[0047] Take another 10g of dopamine hydrochloride, put it into 1L of deionized water, stir at 750r / min to mix, and adjust the pH value to 5.5±0.1 with 0.5M hydrochloric acid; add 12g of sodium dichromate and 0.1g of hydrogen peroxide, place it at about 22°C, continue stirring and react for 26.5h to obtain Cr@dopamine, which is stored for later use.

[0048] In a low temperature environment of about 5°C, take equal molar masses of Cr@dopamine and diphenylmethane diisocyanate, mix them, add 0.5wt% triethylamine, and then return to room temperature. During this period, stir and react at 200r / min for 35h to obtain a modified polyurethane filler, which is stored for later use.

[0049] Take fiber xylan, maleic anhydride and sodium dodecylbenzene sulfonate separately, fiber xylan is a hemicellulose polysaccharide extracted from corn bran, add them to tetrahydrofuran, stir and mix; then add expanded vanadium trioxide, and the expanded vanadium trioxide accounts for 55wt% of the total mass of the materials in this step, ultrasonically disperse for 4.5h to obtain a dispersed liquid; then add modified polyurethane filler to the dispersed liquid, and the volume ratio of the modified polyurethane filler to the expanded vanadium trioxide in the dispersed liquid needs to be controlled to be 0.75:1, mix well, heat to 35°C, ultrasonically disperse for 12h, add a curing agent for injection molding, and obtain a phase change polyurethane material.

[0050] Example 4

[0051] Take 10 mol of ammonium metavanadate, place it in a reactor, heat it to 420±5°C, roast it for 6.5h, then cool it to 85±2°C, add 15 mol of oxalic acid and 2.5L of deionized water, stir it continuously at 600r / min, and keep it warm for reaction; after the reaction is completed, filter it, rinse it with deionized water three times, and then remove the residual solvent by evaporation and drying; then place it in a reactor filled with nitrogen, heat it to 780°C, and perform an expansion treatment for 0.75h, then take it out and cool it to obtain expanded vanadium trioxide, which is placed in a nitrogen atmosphere for storage for later use.

[0052] Take another 10g of dopamine hydrochloride, put it into 1L of deionized water, stir at 750r / min to mix, and adjust the pH value to 5.5±0.1 with 0.5M hydrochloric acid; add 8.5g of sodium dichromate and 0.1g of hydrogen peroxide, place it at about 22°C, continue stirring and react for 26.5h to obtain Cr@dopamine, which is stored for later use.

[0053] In a low temperature environment of about 5°C, Cr@dopamine and diphenylmethane diisocyanate were taken at a molar mass ratio of 0.5:1.2, mixed, 0.5wt% triethylamine was added, and then returned to room temperature. During this period, stirring was continued at 200r / min for 35h to obtain a modified polyurethane filler, which was stored for later use.

[0054] Take fiber xylan, maleic anhydride and sodium dodecylbenzene sulfonate separately, fiber xylan is a hemicellulose polysaccharide extracted from corn bran, add them to tetrahydrofuran, stir and mix; then add expanded vanadium trioxide, and the expanded vanadium trioxide accounts for 55wt% of the total mass of the materials in this step, ultrasonically disperse for 4.5h to obtain a dispersed liquid; then add modified polyurethane filler to the dispersed liquid, and the volume ratio of the modified polyurethane filler to the expanded vanadium trioxide in the dispersed liquid needs to be controlled to be 0.75:1, mix well, heat to 35°C, ultrasonically disperse for 12h, add a curing agent for injection molding, and obtain a phase change polyurethane material.

[0055] Example 5

[0056] Take 10 mol of ammonium metavanadate, place it in a reactor, heat it to 420±5°C, roast it for 6.5h, then cool it to 85±2°C, add 15 mol of oxalic acid and 2.5L of deionized water, stir it continuously at 600r / min, and keep it warm for reaction; after the reaction is completed, filter it, rinse it with deionized water three times, and then remove the residual solvent by evaporation and drying; then place it in a reactor filled with nitrogen, heat it to 780°C, and perform an expansion treatment for 0.75h, then take it out and cool it to obtain expanded vanadium trioxide, which is placed in a nitrogen atmosphere for storage for later use.

[0057] Take another 10g of dopamine hydrochloride, put it into 1L of deionized water, stir at 750r / min to mix, and adjust the pH value to 5.5±0.1 with 0.5M hydrochloric acid; add 8.5g of sodium dichromate and 0.1g of hydrogen peroxide, place it at about 22°C, continue stirring and react for 26.5h to obtain Cr@dopamine, which is stored for later use.

[0058] In a low temperature environment of about 5°C, Cr@dopamine and diphenylmethane diisocyanate were taken at a molar mass ratio of 1:0.6, mixed, 0.5wt% triethylamine was added, and then returned to room temperature. During this period, stirring was continued at 200r / min for 35h to obtain a modified polyurethane filler, which was stored for later use.

[0059] Take fiber xylan, maleic anhydride and sodium dodecylbenzene sulfonate separately, fiber xylan is a hemicellulose polysaccharide extracted from corn bran, add them to tetrahydrofuran, stir and mix; then add expanded vanadium trioxide, and the expanded vanadium trioxide accounts for 55wt% of the total mass of the materials in this step, ultrasonically disperse for 4.5h to obtain a dispersed liquid; then add modified polyurethane filler to the dispersed liquid, and the volume ratio of the modified polyurethane filler to the expanded vanadium trioxide in the dispersed liquid needs to be controlled to be 0.75:1, mix well, heat to 35°C, ultrasonically disperse for 12h, add a curing agent for injection molding, and obtain a phase change polyurethane material.

[0060] Example 6

[0061] Take 10 mol of ammonium metavanadate, place it in a reactor, heat it to 420±5°C, roast it for 6.5h, then cool it to 85±2°C, add 15 mol of oxalic acid and 2.5L of deionized water, stir it continuously at 600r / min, and keep it warm for reaction; after the reaction is completed, filter it, rinse it with deionized water three times, and then remove the residual solvent by evaporation and drying; then place it in a reactor filled with nitrogen, heat it to 780°C, and perform an expansion treatment for 0.75h, then take it out and cool it to obtain expanded vanadium trioxide, which is placed in a nitrogen atmosphere for storage for later use.

[0062] Take another 10g of dopamine hydrochloride, put it into 1L of deionized water, stir at 750r / min to mix, and adjust the pH value to 5.5±0.1 with 0.5M hydrochloric acid; add 8.5g of sodium dichromate and 0.1g of hydrogen peroxide, place it at about 22°C, continue stirring and react for 26.5h to obtain Cr@dopamine, which is stored for later use.

[0063] In a low temperature environment of about 5°C, take equal molar masses of Cr@dopamine and diphenylmethane diisocyanate, mix them, add 0.5wt% triethylamine, and then return to room temperature. During this period, stir and react at 200r / min for 35h to obtain a modified polyurethane filler, which is stored for later use.

[0064] Take fiber xylan, maleic anhydride and sodium dodecylbenzene sulfonate separately, fiber xylan is a hemicellulose polysaccharide extracted from corn bran, add them to tetrahydrofuran, stir and mix; then add expanded vanadium trioxide, and the expanded vanadium trioxide accounts for 55wt% of the total mass of the materials in this step, ultrasonically disperse for 4.5h to obtain a dispersed liquid; then add modified polyurethane filler to the dispersed liquid, and the volume ratio of the modified polyurethane filler to the expanded vanadium trioxide in the dispersed liquid needs to be controlled to be 0.55:1, mix well, heat to 35°C, ultrasonically disperse for 12h, add a curing agent for injection molding, and obtain a phase change polyurethane material.

[0065] Example 7

[0066] Take 10 mol of ammonium metavanadate, place it in a reactor, heat it to 420±5°C, roast it for 6.5h, then cool it to 85±2°C, add 15 mol of oxalic acid and 2.5L of deionized water, stir it continuously at 600r / min, and keep it warm for reaction; after the reaction is completed, filter it, rinse it with deionized water three times, and then remove the residual solvent by evaporation and drying; then place it in a reactor filled with nitrogen, heat it to 780°C, and perform an expansion treatment for 0.25h, then take it out and cool it to obtain expanded vanadium trioxide, which is placed in a nitrogen atmosphere for storage for later use.

[0067] Take another 10g of dopamine hydrochloride, put it into 1L of deionized water, stir at 750r / min to mix, and adjust the pH value to 5.5±0.1 with 0.5M hydrochloric acid; add 8.5g of sodium dichromate and 0.1g of hydrogen peroxide, place it at about 22°C, continue stirring and react for 26.5h to obtain Cr@dopamine, which is stored for later use.

[0068] In a low temperature environment of about 5°C, take equal molar masses of Cr@dopamine and diphenylmethane diisocyanate, mix them, add 0.5wt% triethylamine, and then return to room temperature. During this period, stir and react at 200r / min for 35h to obtain a modified polyurethane filler, which is stored for later use.

[0069] Take fiber xylan, maleic anhydride and sodium dodecylbenzene sulfonate separately, fiber xylan is a hemicellulose polysaccharide extracted from corn bran, add them to tetrahydrofuran, stir and mix; then add expanded vanadium trioxide, and the expanded vanadium trioxide accounts for 35wt% of the total mass of the materials in this step, ultrasonically disperse for 4.5h to obtain a dispersed liquid; then add modified polyurethane filler to the dispersed liquid, and the volume ratio of the modified polyurethane filler to the expanded vanadium trioxide in the dispersed liquid needs to be controlled to be 0.75:1, mix well, heat to 35°C, ultrasonically disperse for 12h, add a curing agent for injection molding, and obtain a phase change polyurethane material.

[0070] Example 8

[0071] Take 10 mol of ammonium metavanadate, place it in a reactor, heat it to 420±5°C, roast it for 6.5h, then cool it to 85±2°C, add 15 mol of oxalic acid and 2.5L of deionized water, stir it continuously at 600r / min, and keep it warm for reaction; after the reaction is completed, filter it, rinse it with deionized water three times, and then remove the residual solvent by evaporation and drying; then place it in a reactor filled with nitrogen, heat it to 780°C, and perform an expansion treatment for 0.75h, then take it out and cool it to obtain expanded vanadium trioxide, which is placed in a nitrogen atmosphere for storage for later use.

[0072] Take another 10g of dopamine hydrochloride, put it into 1L of deionized water, stir at 750r / min to mix, and adjust the pH value to 5.5±0.1 with 0.5M hydrochloric acid; add 6g of sodium dichromate and 0.1g of hydrogen peroxide, place it at about 22°C, continue stirring and react for 26.5h to obtain Cr@dopamine, which is stored for later use.

[0073] In a low temperature environment of about 5°C, take equal molar masses of Cr@dopamine and diphenylmethane diisocyanate, mix them, add 0.5wt% triethylamine, and then return to room temperature. During this period, stir and react at 200r / min for 35h to obtain a modified polyurethane filler, which is stored for later use.

[0074] Take fiber xylan, maleic anhydride and sodium dodecylbenzene sulfonate separately, fiber xylan is a hemicellulose polysaccharide extracted from corn bran, add them to tetrahydrofuran, stir and mix; then add expanded vanadium trioxide, and the expanded vanadium trioxide accounts for 55wt% of the total mass of the materials in this step, ultrasonically disperse for 4.5h to obtain a dispersed liquid; then add modified polyurethane filler to the dispersed liquid, and the volume ratio of the modified polyurethane filler to the expanded vanadium trioxide in the dispersed liquid needs to be controlled to be 0.63:1, mix well, heat to 35°C, ultrasonically disperse for 12h, add a curing agent for injection molding, and obtain a phase change polyurethane material.

[0075] Comparative Example 1

[0076] Take 10 mol of ammonium metavanadate, place it in a reactor, heat it to 420±5°C, roast it for 6.5h, then cool it to 85±2°C, add 15 mol of oxalic acid and 2.5L of deionized water, stir it continuously at 600r / min, and keep it warm for reaction; after the reaction is completed, filter it, rinse it with deionized water three times, and then remove the residual solvent by evaporation and drying; then place it in a reactor filled with nitrogen, heat it to 780°C, and perform an expansion treatment for 0.75h, then take it out and cool it to obtain expanded vanadium trioxide, which is placed in a nitrogen atmosphere for storage for later use.

[0077] In a low temperature environment of about 5°C, take equal molar masses of dopamine and diphenylmethane diisocyanate, mix them, add 0.5wt% triethylamine, and then return to room temperature. During this period, stir and react at 200r / min for 35h to obtain a polyurethane filler, which is stored for later use.

[0078] Take fiber xylan, maleic anhydride and sodium dodecylbenzene sulfonate separately, fiber xylan is a hemicellulose polysaccharide extracted from corn bran, add them to tetrahydrofuran, stir and mix; then add expanded vanadium trioxide, and the expanded vanadium trioxide accounts for 55wt% of the total mass of the materials in this step, ultrasonically disperse for 4.5h to obtain a dispersed liquid; then add modified polyurethane to the dispersed liquid, and control the volume ratio of the modified polyurethane to the expanded vanadium trioxide in the dispersed liquid to be 0.75:1, mix well, heat to 35°C, ultrasonically disperse for 12h, add a curing agent for injection molding, and obtain a phase change polyurethane material.

[0079] Comparative Example 2

[0080] Take 10 mol of ammonium metavanadate, place it in a reactor, heat it to 420±5°C, roast it for 6.5h, then cool it to 85±2°C, add 15 mol of oxalic acid and 2.5L of deionized water, stir it continuously at 600r / min, and keep it warm for reaction; after the reaction is completed, filter it, rinse it with deionized water three times, and then remove the residual solvent by evaporation and drying; then place it in a reactor filled with nitrogen, heat it to 780°C, and perform an expansion treatment for 0.75h, then take it out and cool it to obtain expanded vanadium trioxide, which is placed in a nitrogen atmosphere for storage for later use.

[0081] Take polyethylene glycol and diphenylmethane diisocyanate of equal molar mass, mix them evenly, add 0.5 wt % triethylamine, and then return to room temperature. During this period, stir and react at 200 r / min for 35 hours to obtain polyurethane, which is stored for later use.

[0082] Take fiber xylan, maleic anhydride and sodium dodecylbenzene sulfonate separately, fiber xylan is a hemicellulose polysaccharide extracted from corn bran, add them to tetrahydrofuran, stir and mix; then add expanded vanadium trioxide, and the expanded vanadium trioxide accounts for 55wt% of the total mass of the materials in this step, ultrasonically disperse for 4.5h to obtain a dispersed liquid; then add polyurethane to the dispersed liquid, and control the volume ratio of polyurethane to expanded vanadium trioxide in the dispersed liquid to be 0.75:1, mix well, heat to 35°C, ultrasonically disperse for 12h, add a curing agent and injection mold, to obtain a phase change polyurethane material.

[0083] Comparative Example 3

[0084] Take 10g of dopamine hydrochloride, put it in 1L of deionized water, stir at 750r / min to mix, and adjust the pH value to 5.5±0.1 with 0.5M hydrochloric acid; add 8.5g of sodium dichromate and 0.1g of hydrogen peroxide, place it in an environment of about 22℃, continue stirring and react for 26.5h to obtain Cr@dopamine, which is stored for later use.

[0085] In a low temperature environment of about 5°C, take equal molar masses of Cr@dopamine and diphenylmethane diisocyanate, mix them, add 0.5wt% triethylamine, and then return to room temperature. During this period, stir and react at 200r / min for 35h to obtain a modified polyurethane filler, which is stored for later use.

[0086] Take fiber xylan, maleic anhydride and sodium dodecylbenzene sulfonate separately, fiber xylan is a hemicellulose polysaccharide extracted from corn bran, add them to tetrahydrofuran, and stir to mix; then add vanadium dioxide, and the vanadium dioxide accounts for 55wt% of the total mass of the materials in this step, ultrasonically disperse for 4.5h to obtain a dispersed liquid; then add modified polyurethane filler to the dispersed liquid, and control the volume ratio of the modified polyurethane filler to the vanadium dioxide in the dispersed liquid to be 0.75:1, mix well, heat to 35°C, ultrasonically disperse for 12h, add a curing agent for injection molding, and obtain a phase change polyurethane material.

[0087] Comparative Example 4

[0088] Take 10 mol of ammonium metavanadate, place it in a reactor, heat it to 420±5°C, roast it for 6.5 hours, then cool it to 85±2°C, add 15 mol of oxalic acid and 2.5 L of deionized water, stir it continuously at 600 r / min, and keep it warm for reaction; after the reaction is completed, filter it, rinse it with deionized water three times, and then evaporate it to remove the residual solvent to obtain vanadium trioxide, which is stored for later use.

[0089] In a low temperature environment of about 5°C, take equimolar masses of dopamine hydrochloride and diphenylmethane diisocyanate, mix them, add 0.5wt% triethylamine, and then return to room temperature. During this period, stir and react at 200r / min for 35h to obtain a polyurethane base material, which is stored for later use.

[0090] Take fiber xylan, maleic anhydride, and sodium dodecylbenzene sulfonate separately. Fiber xylan is a hemicellulose polysaccharide extracted from corn bran, add them to tetrahydrofuran, and stir to mix; then add vanadium trioxide, and the vanadium trioxide accounts for 55wt% of the total mass of the materials in this step, and ultrasonically disperse for 4.5 hours to obtain a dispersed liquid; take sodium dichromate and a polyurethane base material in a mass ratio of 2.5:6.4, add them to the dispersed liquid, and control the volume ratio of the modified polyurethane filler to the expanded vanadium trioxide in the dispersed liquid to be 0.75:1, mix well, heat to 35°C, ultrasonically disperse for 12 hours, add a curing agent for injection molding, and obtain a phase change polyurethane material.

[0091] Test example

[0092] Samples: Examples 1-8, Comparative Examples 1-4

[0093] The phase change polyurethane materials prepared in the above Examples 1-8 and Comparative Examples 1-4 were sampled as test samples, and the material properties of the samples in the initial state and after 200 cycles of the phase change process were tested. The cyclic stability of different samples was tested by comparing the material properties before and after. The test results are summarized in Table 1 below:

[0094] Table 1 Performance test results of different phase change polyurethane materials

[0095]

[0096] Among them, the maximum thermal conductivity refers to the highest thermal conductivity that the phase change polyurethane material sample can achieve during the phase change process of the test.

[0097] It can be seen from Table 1 above:

[0098] ① The phase change enthalpy of the phase change polyurethane material samples in Examples 1 to 8 is slightly higher than that of the phase change polyurethane material samples in Comparative Examples 1 to 4 in the initial stage, but after multiple cycles of phase change process, the phase change enthalpy of the phase change polyurethane material samples in Examples 1 to 8 is significantly higher than that of the phase change polyurethane material samples in Comparative Examples 1 to 4, indicating that the phase change polyurethane material in the present invention can still absorb or release more energy in the phase change process after multiple cycles of phase change, has higher heat capacity and better thermal stability.

[0099] ② Compared with the initial state, the thermal conductivity of the phase change polyurethane material samples in Examples 1 to 8 remains the same or only slightly decreases after several cycles of phase change, while the thermal conductivity of the phase change polyurethane material samples in Comparative Examples 1 to 4 decreases significantly after several cycles of phase change, and at the same initial state, the thermal conductivity of the phase change polyurethane material samples in Examples 1 to 8 is generally higher than the thermal conductivity of the phase change polyurethane material samples in Comparative Examples 1 to 4, indicating that the phase change polyurethane material in the present invention not only has better thermal conductivity, but also can maintain a relatively stable thermal conductivity after cyclic phase change, that is, its thermal stability is stronger.

[0100] In summary, the phase change polyurethane material and preparation method thereof proposed in the present invention can simultaneously achieve more outstanding phase change latent heat, thermal conductivity, thermal stability and other performance effects.

[0101] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A phase change polyurethane material, characterized in that: The invention comprises vanadium trioxide aggregate and modified polyurethane filler filled in the vanadium trioxide aggregate; The modified polyurethane filler is prepared by polymerization of Cr@dopamine and isocyanate, and the Cr@dopamine is modified dopamine doped with divalent chromium ions.

2. The phase change polyurethane material according to claim 1, characterized in that: The preparation method of Cr@dopamine comprises the following steps: Dopamine hydrochloride is placed in a solvent, mixed evenly, and a chromium salt and a catalyst are added, and stirred for reaction at 20-25° C. to obtain the Cr@dopamine.

3. The phase change polyurethane material according to claim 2, characterized in that: Before adding chromium salt and catalyst, adjust pH value to 5-6 with hydrochloric acid.

4. The phase change polyurethane material according to claim 2, characterized in that: Based on the molar weight, the dosage ratio of dopamine hydrochloride to the chromium ion in the chromium salt is 1-1.2:0.8-1.

35.

5. The phase change polyurethane material according to claim 1, characterized in that: The preparation method of the modified polyurethane filler comprises the following steps: The Cr@dopamine and isocyanate are mixed evenly, a catalyst is added, and the mixture is stirred and reacted for 20-50 hours to obtain the modified polyurethane filler.

6. The phase change polyurethane material according to claim 5, characterized in that: The molecular ratio of Cr@dopamine to isocyanate is 0.95-1.35:0.4-1.

7. The phase change polyurethane material according to any one of claims 1 to 6, characterized in that: The volume ratio of the modified polyurethane filler to the vanadium trioxide aggregate is 0.75-1:0.8-1.

2.

8. A method for preparing the phase change polyurethane material according to any one of claims 1 to 7, characterized in that: The steps include: (1) mixing vanadium trioxide aggregate with fiber xylan, a compatibilizer, and a dispersant, adding the mixture to a solvent, and performing ultrasonic dispersion to obtain a dispersed liquid; (2) adding modified polyurethane filler to the dispersion liquid, heating for reaction, ultrasonic dispersion, and curing and forming to obtain the phase change polyurethane material.

9. The method for preparing a phase change polyurethane material according to claim 8, characterized in that: In step (1), the method for preparing vanadium trioxide aggregate comprises the following steps: Take ammonium vanadate or ammonium metavanadate, heat it to 400-450°C for roasting, then cool it to 80-100°C, add oxalic acid solution, and stir to react; after the reaction, remove the solvent, perform expansion treatment at 500-800°C in an inert gas atmosphere, and cool to obtain the vanadium trioxide aggregate.

10. The method for preparing a phase change polyurethane material according to claim 8 or 9, characterized in that: In step (1), the vanadium trioxide aggregate accounts for 10-65wt% of the total mass of the dispersed liquid.