Plastic gel settleability prevention total synthesis water-based grinding fluid and preparation method thereof
By using a fully synthetic water-based grinding fluid with composite sedimentants and anti-gel dispersants in the grinding fluid, the problems of overheating and debris settlement during the grinding process of plastic workpieces are solved, and high-precision processing and long-life liquid are achieved. Ensure safety and environmental protection.
Patent Information
- Application Number
- CN202410892978.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-01
AI Technical Summary
During the grinding process, plastic workpieces are partially overheated, surface quality and accuracy are damaged, and plastic debris in the grinding fluid are difficult to settle, resulting in clogging of the filter net, affecting processing accuracy and safety.
A fully synthesized water-based grinding fluid using composite sedimentation agent and anti-gel dispersant is used to achieve rapid settlement and stable dispersion of plastic powder through electrostatic adsorption and molecular chains, avoiding gel formation, and the formula does not contain heavy metals. , secondary amines, nitrites and other harmful substances.
It effectively reduces the risk of overheating of plastic workpieces, ensures processing accuracy and finish, extends the service life of grinding fluid, ensures safe operation, and is environmentally friendly and corrosion-free.
Smart Images

Figure BDA0004928144870000021 
Figure BDA0004928144870000071 
Figure FDA0004928144860000011
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water-based grinding fluid, in particular to an anti-plastic gel sedimentable fully synthetic water-based grinding fluid and a preparation method thereof. Background Art
[0002] Plastic workpieces are generally produced by direct molding methods, but some plastic workpieces are difficult to mold directly or have high precision requirements, so grinding is necessary. The grinding of plastic workpieces generally uses equipment for processing metals. Since the performance of plastics is quite different from that of metals, and there are many types of plastics, the performance of different types also varies greatly, so the grinding of plastic workpieces has its own characteristics.
[0003] First, the thermal conductivity of plastic is much lower than that of metal. Its thermal conductivity is only less than 0.3% of that of metal, and its thermal expansion coefficient is large (1.5 to 20 times larger than that of metal). Therefore, the heat generated by friction during the grinding process is mainly transferred to the tool. Even if a small amount of heat is transferred to the plastic workpiece, it is difficult to transfer to the inside of the plastic workpiece, which is very easy to cause local overheating, causing the plastic workpiece to change color or even deform, seriously affecting the surface quality and dimensional accuracy of the plastic workpiece. Compressed air is used to reduce the temperature during processing. Secondly, high-speed grinding makes the ground plastic debris in a molten state, which hardens when it is cold. During the processing, the debris is very easy to adhere to the tool, thereby changing the angle of the tool, increasing the grinding depth, and affecting the processing accuracy of the plastic workpiece. In addition, the debris dust generated during the grinding process of the plastic workpiece seriously affects the safety of the operator.
[0004] When processing plastic workpieces with grinding fluid, the plastic debris and powder generated by high-speed grinding will be suspended in the grinding fluid and cannot be effectively discharged. On the one hand, they will remain and accumulate on the surface of plastic products as the equipment circulates, affecting the processing accuracy. On the other hand, long-term immersion in the grinding fluid will cause the plastic debris powder to swell and condense into a colloid (jelly-like), blocking the circulation filter and making the grinding fluid unable to be recycled.
[0005] In some public patents, only some studies have been conducted on the sedimentation of metal or glass chips, some of which are limited to single sedimentation and some to multiple sedimentation. However, the premise of these sedimentations is that metal and glass will not produce swelling and gelling problems due to immersion in the grinding fluid, and only the sedimentation properties need to be considered. Plastics not only have sedimentation problems, but also swelling and gelling problems. A large amount of swelling and gelling phenomena cause the filter screen to be blocked, which is particularly important in the recycling of grinding fluids. The anti-plastic gel sedimentation fully synthetic water-based grinding fluid developed by the present invention not only has the use of plastic sedimentation, but also can prevent the plastic from forming a colloidal jelly after sedimentation, thereby ensuring the entire circulation service life of the grinding fluid. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a fully synthetic water-based grinding fluid with anti-plastic gel sedimentation properties and a preparation method thereof. The grinding fluid is optimized through formula screening and does not contain harmful substances such as heavy metals, secondary amines, nitrites, etc., and has good sedimentation and anti-gel properties for plastics during long-term use, thereby ensuring the surface processing accuracy and smoothness of the workpiece and extending the service life of the grinding fluid.
[0007] The technical solution adopted by the present invention to solve the technical problem is:
[0008] A fully synthetic water-based grinding fluid with anti-plastic gel sedimentation properties, the components and weight proportions of which are:
[0009]
[0010] Moreover, the composite sedimentation agent is a composite of a main sedimentation agent and an auxiliary sedimentation agent. The main sedimentation agent is a short-chain hyperbranched gemini quaternary ammonium salt, and the auxiliary sedimentation agent is one or a mixture of two or more of diaminourea polymer, dodecyl dimethyl benzyl ammonium bromide, and polydichloroethyl ether tetramethylethylenediamine.
[0011] Moreover, the anti-gel dispersant is one or a mixture of two or more of succinic acid, methylene succinic acid, 2-hydroxysuccinic acid, and 3-hydroxy-3-carboxyglutaric acid.
[0012] Moreover, the rust inhibitor is one or a mixture of two or more of monocarboxylic acid, dicarboxylic acid, tricarboxylic acid, sodium carbonate, benzotriazole, and methylbenzotriazole.
[0013] Moreover, the base value reserve agent is one or a mixture of two or more of monoethanolamine, triethanolamine, isopropanolamine, methyldiethanolamine, dimethylethanolamine and diglycolamine.
[0014] Moreover, the complexing agent is one or a mixture of two or more of ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate, tetrasodium ethylenediaminetetraacetate, and polyacrylic acid.
[0015] Moreover, the lubricant is one or a mixture of two or more of ethylene glycol, glycerol, trans-block polyether, water-soluble polymer ester, and boric acid ester.
[0016] Moreover, the bactericide is one or a mixture of two or more of hydroxyethyl hexahydro-s-triazine, morpholine derivatives, sodium pyrithione and benzisothiazolinone.
[0017] Moreover, the conductivity of the deionized water is less than 10 us / cm.
[0018] The method for preparing the above-mentioned anti-plastic gel sedimentable fully synthetic water-based grinding fluid comprises the following steps:
[0019] S1: Weigh the composite sedimentation agent, anti-gelling agent dispersant, rust inhibitor, alkalinity reserve agent, complexing agent, lubricant, bactericide and deionized water according to the mass ratio;
[0020] S2: Add deionized water to the reactor, then add the rust inhibitor and the alkalinity reserve agent in sequence, start stirring, heat the reactor to 60-80°C, until the mixed liquid is completely dissolved into a clear and transparent liquid, and stop heating;
[0021] S3: Add the composite sedimentation agent, anti-gelling agent, complexing agent, lubricant and bactericide into the reactor, stir for 30 to 60 minutes, and completely dissolve them into a uniform liquid to obtain an anti-plastic gel sedimentable fully synthetic water-based grinding fluid.
[0022] The advantages and positive effects achieved by the present invention are:
[0023] 1. The present invention uses a composite sedimentation agent, a short-chain hyperbranched gemini quaternary ammonium salt, which is a weak cation and is conducive to reducing the surface tension of the solution. It can wet the plastic powder and gather around it by electrostatic adsorption. Since the charge itself is relatively weak, the particles can achieve a certain sedimentation effect before forming larger particles. In addition, a sedimentation agent such as diamino urea polymer, dodecyl dimethyl benzyl ammonium bromide, and polydichloroethyl ether tetramethylethylenediamine are used as auxiliary agents. The sedimentation effect of the plastic powder is achieved quickly and lastingly through a bridging effect, that is, the small particle size is ensured to settle quickly, and the particles are not allowed to accumulate into large particles to form a gel risk.
[0024] 2. Plastics will swell and even gel when soaked in weak alkaline grinding fluid for a long time. The small particle size and large surface area of powder will increase the occurrence of gel. The anti-gel dispersant selected in the present invention can prevent the flocculation of solid particles through the water molecule film formed by the molecular chain to make the dispersion stable. After the plastic debris powder settles to the bottom, it will not gel after long-term soaking and will not clog the filter.
[0025] 3. Excellent cleanliness. In plastic processing, tool grinding generates heat, causing plastic thermal adsorption and static adsorption on the tool. In the past, compressed air was used to cool and clean the tool and the surface of the plastic workpiece, but compressed air cannot quickly and evenly cool the tool and clean the plastic debris on the tool. The present invention uses anti-plastic gel sedimentable fully synthetic water-based grinding fluid to cool the tool and the plastic workpiece. While taking into account the characteristics of rapid cooling of the tool, no corrosion, good plastic processing surface quality, high precision, etc., the debris powder generated during the grinding process is quickly washed away by the grinding fluid.
[0026] 4. The present invention does not use harmful substances such as heavy metals, secondary amines, and nitrites when designing the formula, which is green and environmentally friendly and safer and more reliable for personnel. DETAILED DESCRIPTION
[0027] The embodiments of the present invention are described in detail below. It should be noted that the embodiments are descriptive rather than restrictive and cannot be used to limit the protection scope of the present invention.
[0028] The raw materials used in the present invention, unless otherwise specified, are conventional commercial products; the methods used in the present invention, unless otherwise specified, are conventional methods in the art; and the concentrations of the various substances used in the present invention are all commonly used concentrations.
[0029] Example 1
[0030] A fully synthetic water-based grinding fluid with anti-plastic gel sedimentation property, the components and the mass percentage of each component are as follows:
[0031] Short chain hyperbranched gemini quaternary ammonium salt 1.5%, diamino urea polymer 0.5%, succinic acid 3.5%, tricarboxylic acid 10%, monocarboxylic acid 2%, benzotriazole 0.5%, monoethanolamine 8%, triethanolamine 4%, methyldiethanolamine 3%, disodium ethylenediaminetetraacetate 1%, trans-block polyether 4%, hydroxyethyl hexahydro-s-triazine 1%, morpholine derivative 1%, deionized water 60%.
[0032] The preparation method of the above-mentioned anti-plastic gel sedimentable fully synthetic water-based grinding fluid comprises the following steps:
[0033] S1: Add deionized water to a reactor, then add tricarboxylic acid, monocarboxylic acid, benzotriazole, monoethanolamine, triethanolamine, and methyldiethanolamine in sequence, start stirring, heat the reactor to 60-80° C., until the mixed solution is completely dissolved into a clear and transparent liquid, and stop heating;
[0034] S2: Then, disodium ethylenediaminetetraacetic acid, trans-block polyether, short-chain hyperbranched gemini quaternary ammonium salt, diamino urea polymer, succinic acid, hydroxyethyl hexahydrotriazine and morpholine derivative are added to the reaction kettle in sequence, and stirred for 30 to 60 minutes until they are completely dissolved into a uniform liquid, thereby obtaining a fully synthetic water-based grinding fluid with anti-plastic gel sedimentation properties.
[0035] Example 2
[0036] A fully synthetic water-based grinding fluid with anti-plastic gel sedimentation property, the components and the mass percentage of each component are as follows:
[0037] Short chain hyperbranched gemini quaternary ammonium salt 1.8%, polydichloroethyl ether tetramethylethylenediamine 0.6%, succinic acid 4%, tricarboxylic acid 7%, dicarboxylic acid 4%, benzotriazole 0.5%, monoethanolamine 6%, isopropanolamine 3%, diglycolamine 2%, ethylenediaminetetraacetic acid 0.5%, trans-block polyether 3%, borate 1.5%, hydroxyethyl hexahydro-s-triazine 0.5%, morpholine derivative 1.5%, deionized water 64.1%.
[0038] The preparation method of the above-mentioned anti-plastic gel sedimentable fully synthetic water-based grinding fluid comprises the following steps:
[0039] S1: Add deionized water to a reactor, then add tricarboxylic acid, dicarboxylic acid, benzotriazole, monoethanolamine, isopropanolamine, and diglycolamine in sequence, start stirring, heat the reactor to 60-80° C., until the mixed solution is completely dissolved into a clear and transparent liquid, and stop heating;
[0040] S2: Then, ethylenediaminetetraacetic acid, trans-block polyether, borate, short-chain hyperbranched gemini quaternary ammonium salt, polydichloroethyl ether tetramethylethylenediamine, succinic acid, hydroxyethyl hexahydrotriazine, and morpholine derivative are added to the reaction kettle in sequence, and stirred for 30 to 60 minutes until they are completely dissolved into a uniform liquid, thereby obtaining a fully synthetic water-based grinding fluid with anti-plastic gel sedimentation properties.
[0041] Example 3
[0042] A fully synthetic water-based grinding fluid with anti-plastic gel sedimentation property, the components and the mass percentage of each component are as follows:
[0043] 1.5% short-chain hyperbranched gemini quaternary ammonium salt, 0.5% dodecyl dimethyl benzyl ammonium bromide, 3.5% 2-hydroxysuccinic acid, 5% tricarboxylic acid, 6% dicarboxylic acid, 2% monocarboxylic acid, 0.5% benzotriazole, 10% monoethanolamine, 2% triethanolamine, 2% diglycolamine, 1% disodium ethylenediaminetetraacetic acid, 3% trans-block polyether, 0.5% water-soluble polymer ester, 1% sodium pyrithione, 1% morpholine derivative, and 60.5% deionized water.
[0044] The preparation method of the above-mentioned anti-plastic gel sedimentable fully synthetic water-based grinding fluid comprises the following steps:
[0045] S1: Add deionized water to a reactor, and then add tricarboxylic acid, dicarboxylic acid, monocarboxylic acid, benzotriazole, monoethanolamine, triethanolamine, and diglycolamine in sequence, start stirring, heat the reactor to 60-80° C., until the mixed solution is completely dissolved into a clear and transparent liquid, and stop heating;
[0046] S2: Then, disodium ethylenediaminetetraacetate, trans-block polyether, water-soluble polymer ester, short-chain hyperbranched gemini quaternary ammonium salt, dodecyldimethylbenzylammonium bromide, 2-hydroxysuccinic acid, sodium pyrithione and morpholine derivative are added to the reaction kettle in sequence, and stirred for 30 to 60 minutes until they are completely dissolved into a uniform liquid, thereby obtaining a fully synthetic water-based grinding fluid with anti-plastic gel sedimentation properties.
[0047] Example 4
[0048] A fully synthetic water-based grinding fluid with anti-plastic gel sedimentation property, the components and the mass percentage of each component are as follows:
[0049] Short chain hyperbranched gemini quaternary ammonium salt 2%, diamino urea polymer 0.5%, methylene succinic acid 4.2%, tricarboxylic acid 10%, sodium carbonate 2%, methylbenzotriazole 0.8%, monoethanolamine 9%, triethanolamine 2%, methyldiethanolamine 2%, disodium ethylenediaminetetraacetic acid 1%, trans-block polyether 5%, sodium pyrithione 1%, morpholine derivative 1%, deionized water 59.5%.
[0050] The preparation method of the above-mentioned anti-plastic gel sedimentable fully synthetic water-based grinding fluid comprises the following steps:
[0051] S1: Add deionized water to a reactor, then add tricarboxylic acid, sodium carbonate, methylbenzotriazole, monoethanolamine, triethanolamine, and methyldiethanolamine in sequence, start stirring, heat the reactor to 60-80° C., until the mixed solution is completely dissolved into a clear and transparent liquid, and stop heating;
[0052] S2: Then, disodium ethylenediaminetetraacetic acid, trans-block polyether, short-chain hyperbranched gemini quaternary ammonium salt, diamino urea polymer, methylene succinic acid, sodium pyrithione and morpholine derivative are added to the reaction kettle in sequence, and stirred for 30 to 60 minutes until they are completely dissolved into a uniform liquid, thereby obtaining a fully synthetic water-based grinding fluid with anti-plastic gel sedimentation properties.
[0053] Example 5
[0054] A fully synthetic water-based grinding fluid with anti-plastic gel sedimentation property, the components and the mass percentage of each component are as follows:
[0055] Short chain hyperbranched gemini quaternary ammonium salt 1.8%, diamino urea polymer 0.5%, 3-hydroxy-3-carboxyglutaric acid 4%, tricarboxylic acid 8%, dicarboxylic acid 2%, sodium carbonate 2%, methylbenzotriazole 0.5%, monoethanolamine 7%, triethanolamine 4%, methyldiethanolamine 3%, ethylenediaminetetraacetic acid 0.5%, trans-block polyether 5%, sodium pyrithione 1.5%, benzisothiazolinone 0.5%, deionized water 59.7%.
[0056] The preparation method of the above-mentioned anti-plastic gel sedimentable fully synthetic water-based grinding fluid comprises the following steps:
[0057] S1: Add deionized water to a reactor, and then add tricarboxylic acid, dicarboxylic acid, sodium carbonate, methylbenzotriazole, monoethanolamine, triethanolamine, and methyldiethanolamine in sequence, start stirring, heat the reactor to 60-80° C., until the mixed solution is completely dissolved into a clear and transparent liquid, and stop heating;
[0058] S2: Then, ethylenediaminetetraacetic acid, trans-block polyether, short-chain hyperbranched gemini quaternary ammonium salt, diamino urea polymer, 3-hydroxy-3-carboxyglutaric acid, sodium pyrithione and benzisothiazolinone are added to the reaction kettle in sequence, and stirred for 30 to 60 minutes until they are completely dissolved into a uniform liquid, thereby obtaining a fully synthetic water-based grinding fluid with anti-plastic gel sedimentation properties.
[0059] Example 6
[0060] A fully synthetic water-based grinding fluid with anti-plastic gel sedimentation property, the components and the mass percentage of each component are as follows:
[0061] Short chain hyperbranched gemini quaternary ammonium salt 2.2%, diamino urea polymer 0.6%, succinic acid 3.8%, tricarboxylic acid 10%, monocarboxylic acid 2%, sodium carbonate 1%, methylbenzotriazole 0.5%, isopropanolamine 9%, triethanolamine 4%, methyldiethanolamine 3%, ethylenediaminetetraacetic acid 0.5%, trans-block polyether 4.8%, morpholine derivative 1.5%, benzisothiazolinone 0.5%, deionized water 56.6%.
[0062] The preparation method of the above-mentioned anti-plastic gel sedimentable fully synthetic water-based grinding fluid comprises the following steps:
[0063] S1: Add deionized water to a reactor, then add tricarboxylic acid, monocarboxylic acid, sodium carbonate, methylbenzotriazole, isopropanolamine, triethanolamine, and methyldiethanolamine in sequence, start stirring, heat the reactor to 60-80° C., until the mixed solution is completely dissolved into a clear and transparent liquid, and stop heating;
[0064] S2: Then, ethylenediaminetetraacetic acid, trans-block polyether, short-chain hyperbranched gemini quaternary ammonium salt, diamino urea polymer, succinic acid, morpholine derivative, and benzisothiazolinone are added to the reactor in sequence, and stirred for 30 to 60 minutes until they are completely dissolved into a uniform liquid, thereby obtaining a fully synthetic water-based grinding fluid with anti-plastic gel sedimentation properties.
[0065] Comparative Example 1
[0066] A certain brand of water-based fully synthetic grinding fluid is available on the market.
[0067] Comparative Example 2
[0068] A certain brand of water-based fully synthetic grinding fluid is available on the market.
[0069] Plastic powder sedimentation test
[0070] 1. Prepare 100 ml of 5% dilution with tap water, mix well, and pour 50 ml into a 50 ml stoppered measuring cylinder;
[0071] 2. Weigh 2g of plastic powder, add it into a 50ml stoppered measuring cylinder, shake it gently to immerse all the powder below the liquid surface, cover it with the stopper and tighten it;
[0072] 3. Shake the stoppered measuring cylinder up and down with the same force for 1 minute to completely disperse the plastic powder in the diluent;
[0073] 4. Place the stoppered measuring cylinder on the table and let it stand to observe the powder settling.
[0074] 5. Each set of tests needs to be repeated 3 times and the average value is taken.
[0075] Settlement evaluation criteria
[0076] When standing for 5 minutes, the larger the powder sedimentation volume (supernatant liquid) of the dilution in the stoppered measuring cylinder, the better the sedimentation property.
[0077] Plastic powder immersion gel evaluation criteria:
[0078] After the sedimentation test, the sample was tightly covered and left at room temperature for 1 month to observe the state of the dilution liquid. It was good if the upper layer was clear and the lower layer was free of colloid. The more colloid, the worse the anti-gel property. The test results are shown in Table 1.
[0079] Table 1 Sedimentation and anti-gel test results
[0080]
[0081] It can be seen from the experimental results that the present invention maintains the sedimentation of the grinding fluid on the plastic debris powder and effectively ensures that the plastic powder will not produce gelation during immersion by using additives in a reasonable manner.
[0082] The above-mentioned reference embodiments provide a detailed description of the anti-plastic gel sedimentable fully synthetic water-based grinding fluid and its preparation method, which is illustrative rather than restrictive. Several embodiments can be cited according to the limited scope. Therefore, changes and modifications without departing from the overall concept of the present invention should be within the scope of protection of the present invention.
Claims
1. A fully synthetic water-based grinding fluid with anti-plastic gel sedimentation property, characterized in that: Its components and weight parts are:
2. The anti-plastic gel sedimentable fully synthetic water-based grinding fluid according to claim 1, characterized in that: The composite sedimentation agent is a composite of a main sedimentation agent and an auxiliary sedimentation agent. The main sedimentation agent is a short-chain hyperbranched gemini quaternary ammonium salt, and the auxiliary sedimentation agent is one or a mixture of two or more of diaminourea polymer, dodecyl dimethyl benzyl ammonium bromide, and polydichloroethyl ether tetramethylethylenediamine.
3. The anti-plastic gel sedimentable fully synthetic water-based grinding fluid according to claim 1, characterized in that: The anti-gel dispersant is one or a mixture of two or more of succinic acid, methylene succinic acid, 2-hydroxysuccinic acid, and 3-hydroxy-3-carboxyglutaric acid.
4. The anti-plastic gel sedimentable fully synthetic water-based grinding fluid according to claim 1, characterized in that: The rust inhibitor is one or a mixture of two or more of monocarboxylic acid, dicarboxylic acid, tricarboxylic acid, sodium carbonate, benzotriazole, and methylbenzotriazole.
5. The anti-plastic gel sedimentable fully synthetic water-based grinding fluid according to claim 1, characterized in that: The base value reserve agent is one or a mixture of two or more of monoethanolamine, triethanolamine, isopropanolamine, methyldiethanolamine, dimethylethanolamine and diglycolamine.
6. The anti-plastic gel sedimentable fully synthetic water-based grinding fluid according to claim 1, characterized in that: The complexing agent is one or a mixture of two or more of ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate, tetrasodium ethylenediaminetetraacetate, and polyacrylic acid.
7. The fully synthetic water-based grinding fluid for preventing plastic gel cutting and continuous sedimentation as claimed in claim 1, characterized in that: The lubricant is one or a mixture of two or more of ethylene glycol, glycerol, trans-block polyether, water-soluble polymer ester and boric acid ester.
8. The anti-plastic gel sedimentable fully synthetic water-based grinding fluid according to claim 1, characterized in that: The bactericide is one or a mixture of two or more of hydroxyethyl hexahydro-s-triazine, morpholine derivatives, sodium pyrithione and benzisothiazolinone.
9. The anti-plastic gel sedimentable fully synthetic water-based grinding fluid according to claim 1, characterized in that: The deionized water has an electrical conductivity of less than 10 us / cm.
10. The method for preparing the anti-plastic gel sedimentable fully synthetic water-based grinding fluid according to any one of claims 1 to 9, characterized in that: Here are the steps: S1: Weigh the composite sedimentation agent, anti-gelling agent, rust inhibitor, alkalinity reserve agent, complexing agent, lubricant, bactericide and deionized water according to the mass ratio; S2: Add deionized water to the reactor, then add the rust inhibitor and the alkalinity reserve agent in sequence, start stirring, heat the reactor to 60-80°C, until the mixed liquid is completely dissolved into a clear and transparent liquid, and stop heating; S3: Add the composite sedimentation agent, anti-gelling agent, complexing agent, lubricant and bactericide into the reactor, stir for 30 to 60 minutes, and completely dissolve them into a uniform liquid to obtain an anti-plastic gel sedimentable fully synthetic water-based grinding fluid.