Production process of 9SiCr cold-rolled wide-width plate coil

By adopting annealing, pickling and spherical annealing processes in the production of 9SiCr cold rolled steel, combined with wide-width plate rolling and roll rolling technology, the problems of high pickling difficulty and low production efficiency are solved, and high efficiency and low cost are achieved Wide-width plate roll production.

CN118879990AActive Publication Date: 2024-11-01HUNAN VALIN LIANYUAN IRON & STEEL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410975703.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-01
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

9SiCr cold-rolled steel has problems such as pickling difficulty and low production efficiency in the cold rolling production process, especially due to its high strength and poor plate shape, the pull-through rate of the traditional narrow-band production method is low, resulting in Cold rolling production efficiency is low and steel curling is greatly reduced.

Method used

Using a process flow including first annealing, pickling, spherical annealing and second annealing, soften the steel coil by low-temperature annealing, reduce the reduction of oxides, improve the pickling efficiency, and in the production of wide-width plate coils Use wide-plate single-frame cold rolling mill and rolling in rolling mode to improve production efficiency and cost-effectiveness.

Benefits of technology

It realizes efficient pickling and high-quality wide-width plate coil production of 9SiCr cold-rolled steel, which improves production efficiency, reduces costs, and ensures the thickness accuracy and surface quality of the steel coil.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879990A_ABST
    Figure CN118879990A_ABST
Patent Text Reader

Abstract

The invention provides a production technology of a 9SiCr cold-rolled wide-width plate coil. The technology comprises the following steps that the 9SiCr hot-rolled plate coil is subjected to first-time annealing, acid pickling, spheroidizing annealing, rolling and second-time annealing; the first-time annealing comprises first-section heating, second-section heating, first-section heat preservation, third-section heating, second-section heat preservation, first-time cooling and second-time cooling; the temperature of first-stage heat preservation in the first annealing process is 380-420 DEG C; and the width of the 9SiCr cold-rolled wide-width plate coil is more than 900 mm. A 9SiCr hot-rolled plate coil is subjected to first-time annealing, softening and destressing, acid pickling and spheroidizing annealing, the annealed steel coil is rolled, and finally the annealed steel coil is subjected to second-time annealing to form a cold-rolled finished product coil. According to the method, the high-quality cold-rolled 9SiCr cold-rolled plate coil is produced through the wide plate coil, and the method has the beneficial effects of being high in production efficiency, low in production cost and stable in process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of steel smelting, and in particular to a production process of a 9SiCr cold-rolled wide-width coil. Background Art

[0002] 9SiCr is a low alloy steel for cutting tools, and also belongs to low carbon and high hardness steel. It is composed of elements such as iron, carbon, silicon and chromium, and is obtained through a special heat treatment process. This steel has the characteristics of high hardness, good toughness, strong wear resistance, high impact strength and good thermal fatigue resistance. 9SiCr steel also has excellent cutting performance and wear resistance, which can greatly improve the service life of cutting tools and molds. Due to its high hardenability and hardenability, as well as high tempering stability, 9SiCr is suitable for step quenching or isothermal quenching.

[0003] 9SiCr steel has a long history of application, mainly used to manufacture machine tool accessories and cold working dies, such as printing dies, gear rolling dies, thread rolling plates, cold punching dies, etc. In recent years, 9SiCr is gradually being applied to dies with larger loads, and is partially used to replace Cr12 steel.

[0004] There are two major difficulties in the cold rolling production process of this material:

[0005] One is that pickling is difficult, and the iron oxide scale is relatively easy to remove when the hot-rolled coil is directly pickled in the pickling process of this steel grade. However, due to the high strength and poor plate shape of the steel coil, it is easy to break and scratch the coil when unwinding, and it is very difficult to pickle and thread the strip. The pickling speed is 10m / min~30m / min, and the pickling efficiency is low. Pickling after annealing and spheroidization can reduce the strength of the steel coil, and the difficulty of threading is relatively low. However, the surface iron oxide scale is reduced to iron scale by hydrogen in the bell furnace, and the pickling needs to be strictly controlled to low-speed pickling. Moreover, it is difficult to wash off the reduced iron scale covering the surface during pickling, and the residual oxide under the iron scale is easy to cause oxide pressure in the subsequent cold rolling. Even in an environment where inert gas protection is used for high-temperature annealing, the oxygen elements in the iron oxide scale will diffuse into the matrix and react with the carbon in the matrix, causing the iron oxide scale to be reduced to iron scale that is difficult to pickle. In addition, the migrated and diffused oxygen elements further oxidize the surface of the matrix, causing surface grain boundary oxidation and producing a surface decarburization layer. The pickling methods currently used in the industry all have disadvantages, so the 9SiCr pickling process path needs to be optimized.

[0006] Secondly, the traditional production process of 9SiCr tool steel cold-rolled coils is produced through a single frame + narrow strip (width ≤ 500mm), and there is no single frame + wide plate coil (width > 900mm) mode. The reduction rate of narrow strip plus single frame mode is generally less than 25%. When the reduction rate increases, the strip is very easy to break. At present, there are problems such as low cold rolling production efficiency, difficult to control the difference between steel coils and plates, and large edge drop.

[0007] Application Contents

[0008] The present application is made in view of the above-mentioned problems, and its purpose is to provide a production process of 9SiCr cold-rolled wide-width coils, which can

[0009] Specifically, the present application provides a production process for 9SiCr cold-rolled wide-width coils, comprising the following steps:

[0010] The 9SiCr hot-rolled coil is subjected to first annealing, pickling, spheroidizing annealing, rolling and second annealing;

[0011] The first annealing includes a first stage of heating, a second stage of heating, a first stage of heat preservation, a third stage of heating, a second stage of heat preservation, a first stage of cooling and a second stage of cooling;

[0012] The temperature of the first insulation stage during the first annealing process is 380°C to 420°C;

[0013] The width of the 9SiCr cold-rolled wide-width coil is above 900 mm.

[0014] According to one of the technical solutions of this application, at least the following beneficial effects are achieved:

[0015] In this application, the 9SiCr hot-rolled coil is first annealed to soften and relieve stress, then pickled, and then spheroidized annealed. The annealed steel coil is rolled and finally annealed for the second time to become a cold-rolled finished coil. This application uses wide-width coils to produce high-quality cold-rolled 9SiCr cold-rolled coils, which has the characteristics of high production efficiency, low production cost, and stable process.

[0016] According to some embodiments of the present application, the rate of the first heating stage during the first annealing process is 350° C. / h-450° C. / h.

[0017] According to some embodiments of the present application, the time of the first heating stage during the first annealing process is 0.4 h to 0.6 h.

[0018] According to some embodiments of the present application, the final temperature of the first stage of heating during the first annealing process is 190°C to 210°C.

[0019] According to some embodiments of the present application, the rate of heating in the second stage during the first annealing process is 60° C. / h to 80° C. / h.

[0020] According to some embodiments of the present application, the final temperature of the second stage of heating during the first annealing process is 380°C to 420°C.

[0021] According to some embodiments of the present application, the first insulation time during the first annealing process is 3 hours to 5 hours.

[0022] According to some embodiments of the present application, the heating rate of the third stage during the first annealing process is 60° C. / h to 80° C. / h.

[0023] According to some embodiments of the present application, the final temperature of the third stage of heating during the first annealing process is 500°C to 660°C.

[0024] According to some embodiments of the present application, the temperature of the second insulation stage during the first annealing process is 500°C to 660°C.

[0025] According to some embodiments of the present application, the second insulation time during the first annealing process is 10 hours to 20 hours.

[0026] According to some embodiments of the present application, the final temperature of the first cooling during the first annealing process is 380°C to 420°C.

[0027] According to some embodiments of the present application, the first cooling method during the first annealing process is air cooling.

[0028] According to some embodiments of the present application, the final temperature of the second cooling during the first annealing process is 90° C. to 100° C.

[0029] According to some embodiments of the present application, the second cooling method in the first annealing process is water cooling.

[0030] According to some embodiments of the present application, the pickling solution is hydrochloric acid.

[0031] According to some embodiments of the present application, the mass fraction of the hydrochloric acid is 12% to 18%.

[0032] According to some embodiments of the present application, the temperature of the pickling solution is 70°C to 90°C.

[0033] According to some embodiments of the present application, the pickling rate is 30 m / min to 160 m / min.

[0034] According to some embodiments of the present application, the acid washing also includes water washing.

[0035] According to some embodiments of the present application, the water washing temperature is 60°C to 80°C.

[0036] According to some embodiments of the present application, the washing is followed by drying.

[0037] According to some embodiments of the present application, the drying is hot air drying.

[0038] According to some embodiments of the present application, the temperature of the hot air is 100°C to 140°C.

[0039] According to some embodiments of the present application, the spheroidizing annealing includes a first stage of heating, a second stage of heating, a first stage of heat preservation, a third stage of heating, a second stage of heat preservation, a first stage of cooling, a second stage of cooling and a third stage of cooling.

[0040] According to some embodiments of the present application, the heating rate of the first stage during the spheroidizing annealing process is 350° C. / h-450° C. / h.

[0041] According to some embodiments of the present application, the time of the first heating stage during the spheroidizing annealing process is 0.4 h to 0.6 h.

[0042] According to some embodiments of the present application, the final temperature of the first stage of heating during the spheroidizing annealing process is 190°C to 210°C.

[0043] According to some embodiments of the present application, the heating rate of the second stage during the spheroidizing annealing process is 60° C. / h to 80° C. / h.

[0044] According to some embodiments of the present application, the final temperature of the second stage of heating during the spheroidizing annealing process is 380°C to 420°C.

[0045] According to some embodiments of the present application, the temperature of the first insulation stage during the spheroidizing annealing process is 380°C to 420°C.

[0046] According to some embodiments of the present application, the first insulation time during the spheroidizing annealing process is 3 hours to 5 hours.

[0047] According to some embodiments of the present application, the heating rate of the third stage during the spheroidizing annealing process is 60° C. / h to 80° C. / h.

[0048] According to some embodiments of the present application, the final temperature of the third stage of heating during the spheroidizing annealing process is 700°C to 800°C.

[0049] According to some embodiments of the present application, the temperature of the second insulation stage during the spheroidizing annealing process is 700° C. to 800° C.

[0050] According to some embodiments of the present application, the second insulation time during the spheroidizing annealing process is 10 hours to 20 hours.

[0051] According to some embodiments of the present application, the final temperature of the first cooling during the spheroidizing annealing process is 580°C to 620°C.

[0052] According to some embodiments of the present application, the final temperature of the second cooling during the spheroidizing annealing process is 380°C to 420°C.

[0053] According to some embodiments of the present application, the second cooling method during the spheroidizing annealing process is air cooling.

[0054] According to some embodiments of the present application, the final temperature of the third cooling during the spheroidizing annealing process is 90°C to 100°C.

[0055] According to some embodiments of the present application, the third cooling method during the spheroidizing annealing process is water cooling.

[0056] According to some embodiments of the present application, the rolling is produced by a wide plate single-stand cold rolling mill.

[0057] According to some embodiments of the present application, the cold rolling force is set to 800 TON to 1000 TON.

[0058] According to some embodiments of the present application, the tension of the cold rolling mill is 150KN to 240KN.

[0059] According to some embodiments of the present application, the cold rolling working rolls are rolled using rough rolls.

[0060] According to some embodiments of the present application, the cold rolling reduction is 30% to 40%.

[0061] According to some embodiments of the present application, the rolling rate is 200 m / min to 300 m / min.

[0062] According to some embodiments of the present application, the rolling adopts shifting roll mode rolling.

[0063] According to some embodiments of the present application, the roller shifting value is 30 mm to 90 mm.

[0064] According to some embodiments of the present application, the second annealing includes a first stage of heating, a second stage of heating, a first stage of heat preservation, a third stage of heating, a second stage of heat preservation, a first stage of cooling, a second stage of cooling and a third stage of cooling.

[0065] According to some embodiments of the present application, the heating rate of the first stage during the second annealing process is 350° C. / h to 450° C. / h.

[0066] According to some embodiments of the present application, the time of the first heating stage during the second annealing process is 0.4 h to 0.6 h.

[0067] According to some embodiments of the present application, the final temperature of the first stage of heating during the second annealing process is 190°C to 210°C.

[0068] According to some embodiments of the present application, the rate of the second heating stage during the second annealing process is 40° C. / h to 80° C. / h.

[0069] According to some embodiments of the present application, the final temperature of the second stage of heating during the second annealing process is 380°C to 420°C.

[0070] According to some embodiments of the present application, the temperature of the first insulation stage during the second annealing process is 380° C. to 420° C.

[0071] According to some embodiments of the present application, the first insulation time during the second annealing process is 3 hours to 5 hours.

[0072] According to some embodiments of the present application, the heating rate of the third stage during the second annealing process is 40° C. / h to 80° C. / h.

[0073] According to some embodiments of the present application, the final temperature of the third stage of heating during the second annealing process is 700°C to 800°C.

[0074] According to some embodiments of the present application, the temperature of the second insulation stage during the second annealing process is 700° C. to 800° C.

[0075] According to some embodiments of the present application, the second insulation time during the second annealing process is 10 hours to 20 hours.

[0076] According to some embodiments of the present application, the final temperature of the first cooling during the second annealing process is 580°C to 620°C.

[0077] According to some embodiments of the present application, the final temperature of the second cooling during the second annealing process is 380°C to 420°C.

[0078] According to some embodiments of the present application, the second cooling method during the second annealing process is air cooling.

[0079] According to some embodiments of the present application, the final temperature of the third cooling during the second annealing process is 90° C. to 100° C.

[0080] According to some embodiments of the present application, the third cooling method during the second annealing process is water cooling.

[0081] According to some embodiments of the present application, the 9SiCr cold-rolled wide-width coil is composed of the following elements in mass fraction:

[0082] C 0.9% to 0.95%, Si 1.3% to 1.5%, Mn 0.4% to 0.6%, Cr 1.0% to 1.2%, and the balance is Fe and indispensable residual or impurity elements.

[0083] According to some embodiments of the present application, the thickness of the 9SiCr hot-rolled coil is 2.5 mm to 3.5 mm.

[0084] According to some embodiments of the present application, the width of the 9SiCr hot-rolled coil is 900 mm to 1500 mm.

[0085] According to some embodiments of the present application, the thickness of the 9SiCr cold-rolled wide-width coil is 1.5 mm to 1.8 mm;

[0086] According to some embodiments of the present application, the width of the 9SiCr cold-rolled wide-width coil is 900 mm to 1500 mm.

[0087] According to some embodiments of the present application, the thickness accuracy of the 9SiCr cold-rolled wide-width coil is -10 μm to 10 μm.

[0088] According to some embodiments of the present application, the convexity C40 of the 9SiCr cold-rolled wide-width coil is within 6 μm. BRIEF DESCRIPTION OF THE DRAWINGS

[0089] In order to more clearly illustrate the embodiments of the present drawings or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present drawings. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.

[0090] Figure 1 This is a cross-sectional view after high temperature annealing in Comparative Example 1 (scale is 10 μm).

[0091] Figure 2 This is a cross-sectional view after the first annealing in Example 1 of the present application (scale is 10 μm).

[0092] Figure 3 This is a surface defect diagram after pickling in the embodiment of this application.

[0093] Figure 4 This is a surface defect diagram after cold rolling of an embodiment of the present application.

[0094] Figure 5 This is the surface defect diagram of the steel after cold rolling in Comparative Example 1.

[0095] The purpose, features and advantages of this figure will be further described in conjunction with the embodiments with reference to the accompanying drawings. DETAILED DESCRIPTION

[0096] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is described and illustrated below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments provided in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.

[0097] Obviously, the following descriptions are only some examples or embodiments of the present application. For ordinary technicians in this field, the present application can also be applied to other similar scenarios without creative work. In addition, it can also be understood that although the efforts made in this development process may be complicated and lengthy, for ordinary technicians in the field related to the content disclosed in this application, some changes in design, manufacturing or production based on the technical content disclosed in this application are just conventional technical means, and should not be understood as insufficient content disclosed in this application.

[0098] However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially the same structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the following description is provided for those skilled in the art to fully understand the present application and is not intended to limit the subject matter described in the claims.

[0099] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0100] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0101] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0102] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0103] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0104] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0105] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0106] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0107] The production process of 9SiCr wide coil in this application includes the following steps:

[0108] The 9SiCr hot-rolled coil is subjected to first annealing, pickling, spheroidizing annealing, rolling and second annealing;

[0109] According to some embodiments of the present application, the process parameters of the first annealing are as follows:

[0110] The steel coil is heated freely from room temperature (20℃~25℃) to 200℃; then heated to 400℃ at a heating rate of 60℃ / h~80℃ / h and kept warm for 4h;

[0111] Then heat to 500℃~660℃ at 60℃ / h~80℃ / h and keep warm for 10h~20h; after the insulation, cool to 400℃ with air; cool to 100℃ with water and take out of the furnace.

[0112] This method can solve the problems of difficulty in pickling and threading, poor pickling effect, etc.

[0113] 9SiCr tool steel is difficult to pickle: this steel has high carbon and silicon content, high material strength and brittleness, large hot rolling load, and extremely thick oxide on the surface of the steel coil. Conventional pickling at a much lower pickling speed than other high carbon steels also requires two to three picklings to be clean. When the speed is faster or the number of times is less, the pickling surface is not clean and has residual pitting.

[0114] There are two conventional material pickling process paths, one is pickling after hot coil annealing, and the other is direct pickling of hot coil.

[0115] The former can reduce the strength of the steel coil, but the surface oxide scale is reduced to iron scale by hydrogen in the bell furnace, which is difficult to remove during pickling, and the residual oxide under the iron scale is easy to cause oxide pressure in the subsequent cold rolling; the latter oxide scale is relatively easy to remove, but the steel coil has high strength and poor plate shape, and it is easy to break and scratch the coil during unwinding. Pickling and threading are very difficult, and the production preparation for pickling and threading is too long and inefficient. Therefore, the appropriate process path for pickling raw coils of this type of steel is to use a lower temperature softening annealing (i.e., the first annealing) to inhibit the reduction of oxides.

[0116] According to some embodiments of the present application, the process parameters of the pickling process are as follows:

[0117] After using low temperature annealing to reduce the tensile strength of the steel coil from 1400MPa to 900MPa, the steel coil can be threaded smoothly. Under the current conditions of using regenerated acid with reduced acid concentration and lower water temperature, normal pickling can be achieved, ensuring quality while also saving pickling costs.

[0118] High temperature annealing (parameters see comparative example 1) cross section see Figure 1 The surface oxide is reduced to sponge iron by hydrogen, which is difficult to remove by pickling (see Figure 1 The cross-sectional results after the first annealing (Example 1) of this application are shown in Figure 2 The surface oxide is basically not reduced and can be easily removed by pickling.

[0119] Hydrochloric acid pickling, the mass fraction of hydrochloric acid is 12% to 18%, the temperature of hydrochloric acid is 70℃ to 90℃, and the pickling rate is 30m / min to 160m / min;

[0120] After washing with hydrochloric acid, rinse with water at a temperature of 60°C to 80°C;

[0121] The strip after rinsing is dried by hot air at a temperature of 110°C to 120°C.

[0122] According to some embodiments of the present application, the process parameters of the spheroidizing annealing process are as follows:

[0123] The steel coil is heated freely from room temperature (20℃~25℃) to 200℃; then heated to 400℃ at a heating rate of 60℃ / h and kept warm for 4h;

[0124] Then heat to 700℃~800℃ at 60℃ / h and keep warm for 10h~20h;

[0125] After the insulation is completed, it is cooled to about 600℃ with the furnace; then it is cooled to 400℃ by air; then it is cooled to 100℃ by water before being taken out of the furnace.

[0126] According to some embodiments of the present application, the rolling process parameters are as follows:

[0127] The process parameters are set according to the basic yield strength of 700-800MPa during rolling. The rolling force and tension of the material are stable during the rolling process, and the plate shape is well controlled. The finished product has uniform thickness distribution, small thickness fluctuation, thickness accuracy of ±10μm, and convexity C40 within 6μm.

[0128] The rolling is cold rolling;

[0129] The cold rolling is produced by a wide plate single-stand cold rolling unit, with a cold rolling force of 800TON to 1000TON; a tension of 150KN to 240KN; the cold rolling working rolls are rolled with rough rolls; the cold rolling reduction is 30% to 40%; the rolling rate is set at 200 to 300m / min, and the rolling is carried out in a shifting roll mode, with a shifting roll value of 30 to 90mm.

[0130] The production of coils with high dimensional accuracy is ensured by roller shifting.

[0131] According to some embodiments of the present application, the second annealing is bell furnace annealing.

[0132] According to some embodiments of the present application, the process parameters of the second annealing are as follows:

[0133] This process can ensure that the material accurately meets the terminal performance requirements, improve the material's spheroidization level and hardness performance. At the same time, it prevents excessive precipitation, migration and growth of carbides, resulting in carbon deficiency on the surface, ensuring that the material optimizes its mechanical processing performance.

[0134] The steel coil is heated freely from room temperature (20℃~25℃) to 200℃; then heated to 400℃ at a heating rate of 40℃ / h~80℃ / h and kept warm for 4 hours;

[0135] Then heat to 700℃~800℃ at 40℃ / h~80℃ / h and keep warm for 10h~20h;

[0136] After the insulation is completed, slowly cool it to about 600℃; change to air cooling to 400℃; change to water cooling to 100℃ and take it out of the furnace.

[0137] The technical effect of this application is to solve the industry problem of difficult pickling of 9SiCr, and to produce cold-rolled products with a large reduction rate in the form of wide coils rather than narrow strips or wide coils in strips after hood annealing, with high production efficiency and low cost. Moreover, in the production of wide plate single-stand cold rolling units, the equipment has high precision and the ability to shift the working rolls, which can produce high-quality cold-rolled wide-width coils with high efficiency and low cost. Compared with the current traditional cold-rolled high-quality steel enterprises at home and abroad, this technology is used to produce high-end products such as cold-rolled 9SiCr, which can bring significant economic benefits.

[0138] Example 1

[0139] This embodiment is a production process for a 1.8 mm thick 9SiCr wide coil, which consists of the following steps:

[0140] The 9SiCr hot-rolled coil is subjected to first annealing, pickling, spheroidizing annealing, rolling and second annealing;

[0141] Hot-rolled steel coils with the steel grade of 9SiCr are selected as raw materials. The raw material specifications are 3.0mm×1250mm, and the chemical composition is C0.91%, Si 1.4%, Mn 0.5%, Cr 1.1%. The rest are Fe and indispensable residual or impurity elements. After cold rolling, the finished product specifications are 1.8mm×1250mm.

[0142] The first annealing is low temperature stress relief annealing, and the parameters are as follows:

[0143] The steel coil is heated freely from room temperature (25℃) to 200℃ in half an hour; then heated to 400℃ at a heating rate of 40℃ / h and kept warm for 2h; then heated to 650℃ at 70℃ / h and kept warm for 18h; after the insulation, it is cooled to 400℃ by air; then cooled to 100℃ by water and taken out of the furnace, and pickled after being taken out of the furnace.

[0144] The pickling is carried out by hydrochloric acid pickling, the mass concentration of hydrochloric acid is 15%, and the acid solution temperature is 82°C; the water rinse is carried out, and the rinsing temperature is 70°C; the strip steel after rinsing is dried by hot air, and the hot air temperature is 110°C; the pickling rate is 120m / min.

[0145] After pickling, the steel coil is spheroidized annealed. The parameters of spheroidized annealing are as follows:

[0146] The temperature is freely raised from room temperature (25℃) to 200℃ in half an hour; then heated to 400℃ at a heating rate of 60℃ / h and kept warm for 4h; then heated to 790℃ at 60℃ / h and kept warm for 10h; after the insulation, it is slowly cooled to 600℃; cooled to 400℃ by air; cooled to 100℃ by water and rolled after being taken out of the furnace.

[0147] The rolling process is cold rolling, and the process parameters are as follows:

[0148] The cold rolling is produced by a wide plate single-stand cold rolling unit. The rolling forces of the three cold rolling passes are 800TON, 950TON, and 900TON respectively; the front tensions are 150KN, 180KN, and 240KN respectively, and the rear tensions are 200KN, 240KN, and 280KN; the cold rolling working rolls are rolled with rough rolls; the cold rolling reduction is 40%; the rolling rate is 260m / min, and the rolling is carried out in a shifting roll mode, with the shifting roll values ​​being 30mm, 30mm, and 0mm respectively.

[0149] After cold rolling, the steel coil is annealed in a bell furnace (i.e., the second annealing). The process parameters are as follows:

[0150] The steel coil is heated freely from room temperature (25℃) to 200℃ in half an hour; then heated to 400℃ at a heating rate of 60℃ / h and kept warm for 4h; then heated to 750℃ at 60℃ / h and kept warm for 10h; after the insulation, it is slowly cooled to 600℃; cooled to 400℃ by air; cooled to 100℃ by water before being taken out of the furnace.

[0151] After annealing, a 9SiCr cold-rolled finished coil with a specification of 1.8 mm × 1250 mm (width) was produced, with a thickness accuracy of ±10 μm, a convexity C40 within 6 μm, no oxide residue on the surface of the steel coil, and a 5-level spheroidized pearlite structure. The results of the first annealing, pickling and cold rolling in Example 1 are shown in Figures 2 to 4 ,from Figure 4 It is known that the surface of this embodiment is smooth and has no residue after cold rolling.

[0152] Example 2

[0153] This embodiment is a production process for a 1.5 mm thick 9SiCr wide coil, which consists of the following steps:

[0154] The 9SiCr hot-rolled coil is subjected to first annealing, pickling, spheroidizing annealing, rolling and second annealing;

[0155] Hot-rolled steel coils with the steel grade of 9SiCr are selected as raw materials, with the raw material specifications of 2.5mm×1250mm, the chemical composition of C0.90%, Si 1.3%, Mn 0.4%, Cr 1.2%, and the rest are Fe and indispensable residual or impurity elements. After cold rolling, the finished product specifications are 1.5mm×1250mm.

[0156] The first annealing is low temperature stress relief annealing, and the parameters are as follows:

[0157] The steel coil is heated freely from room temperature (25℃) to 200℃ in half an hour; then heated to 400℃ at a heating rate of 40℃ / h and kept warm for 2h; then heated to 650℃ at 70℃ / h and kept warm for 18h; after the insulation, it is cooled to 400℃ by air; then cooled to 100℃ by water and taken out of the furnace, and pickled after being taken out of the furnace.

[0158] The pickling is carried out by hydrochloric acid pickling, the mass concentration of hydrochloric acid is 15%, and the acid solution temperature is 82°C; the water rinse is carried out, and the rinsing temperature is 70°C; the strip steel after rinsing is dried by hot air, and the hot air temperature is 110°C; the pickling rate is 120m / min.

[0159] After pickling, the steel coil is spheroidized annealed. The parameters of spheroidized annealing are as follows:

[0160] The temperature is freely raised from room temperature (25℃) to 200℃ in half an hour; then heated to 400℃ at a heating rate of 60℃ / h and kept warm for 4h; then heated to 760℃ at 60℃ / h and kept warm for 10h; after the insulation, it is slowly cooled to 600℃; cooled to 400℃ by air; cooled to 100℃ by water and rolled after being taken out of the furnace.

[0161] The rolling process is cold rolling, and the process parameters are as follows:

[0162] The cold rolling is produced by a wide plate single-stand cold rolling unit. The rolling forces of the three cold rolling passes are 800TON, 950TON, and 900TON respectively; the front tensions are 150KN, 180KN, and 240KN respectively, and the rear tensions are 200KN, 240KN, and 280KN; the cold rolling working rolls are rolled with rough rolls; the cold rolling reduction is 40%; the rolling rate is 260m / min, and the rolling is carried out in a shifting roll mode, with the shifting roll values ​​being 30mm, 30mm, and 0mm respectively.

[0163] After cold rolling, the steel coil is annealed in a bell furnace (i.e., the second annealing). The process parameters are as follows:

[0164] The steel coil is heated freely from room temperature (25℃) to 200℃; then heated to 400℃ at a heating rate of 60℃ / h and kept warm for 4h; then heated to 750℃ at 60℃ / h and kept warm for 10h; after the insulation, it is slowly cooled to 600℃; cooled to 400℃ by air; cooled to 100℃ by water before being taken out of the furnace.

[0165] After annealing, the 9SiCr cold-rolled finished coil with a specification of 1.5mm×1250mm (width) is produced, with a thickness accuracy of ±7μm and a convexity C40 within 6μm. There is no oxide residue on the surface of the steel coil, and the structure is a 5-level spheroidized pearlite structure.

[0166] Comparative Example 1

[0167] This comparative example is a production process of a 1.8 mm thick 9SiCr wide coil, and the only difference from Example 1 is that the first annealing is replaced by a high temperature annealing, and the parameters of the high temperature annealing are as follows:

[0168] It takes half an hour to heat freely from room temperature (25℃) to 200℃; then heat to 400℃ at a heating rate of 60℃ / h and keep warm for 4h; then heat to 800℃ at 60℃ / h and keep warm for 10h; after the insulation, slowly cool to 600℃; cool to 400℃ with air; cool to 100℃ with water and pickle after taking out of the furnace.

[0169] High temperature annealing of steel coil (parameters see comparative example 1) cross section Figure 1 The surface oxide is reduced to sponge iron by hydrogen, which is difficult to remove during pickling.

[0170] After annealing, the cold-rolled 9SiCr finished coil with a specification of 1.8mm×1250mm (width) is produced, with a thickness accuracy of ±10μm and a convexity C40 within 6μm. There are more oxide residues on the surface of the steel coil (see Figure 5 ), the organization is spheroidized pearlite organization of level 5. The board surface quality cannot meet the relevant quality standards.

[0171] In summary, the production process of the present application is different from the cold-rolled 9SiCr produced by the existing single-frame cold-rolled narrow strip mill, which has a more complicated process flow, large edge wire loss, low production efficiency and high production cost; in the present application, the 9SiCr hot-rolled coil is first annealed to soften and relieve stress, then pickled, and then spheroidized annealed, the annealed steel coil is rolled, and finally annealed for the second time to become a cold-rolled finished coil. The present application uses wide-width coils to produce high-quality cold-rolled 9SiCr cold-rolled coils, which has the characteristics of high production efficiency, low production cost and stable process.

[0172] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A production process for 9SiCr cold-rolled wide coils, It is characterized in that The following steps are involved: The 9SiCr hot-rolled coil is subjected to first annealing, pickling, spheroidizing annealing, rolling and second annealing; The first annealing includes a first stage of heating, a second stage of heating, a first stage of heat preservation, a third stage of heating, a second stage of heat preservation, a first stage of cooling and a second stage of cooling; The temperature of the first insulation stage during the first annealing process is 380°C to 420°C; The width of the 9SiCr cold-rolled wide-width coil is above 900 mm.

2. The production process according to claim 1, It is characterized in that The first heating rate in the first annealing process is 350°C / h-450°C / h; And / or, the first heating period in the first annealing process is 0.4h to 0.6h; And / or, the final temperature of the first stage of heating in the first annealing process is 190° C. to 210° C.; And / or, the heating rate of the second stage during the first annealing process is 60° C. / h to 80° C. / h; And / or, the final temperature of the second stage of heating in the first annealing process is 380° C. to 420° C.; And / or, the first insulation time in the first annealing process is 3h to 5h; And / or, the heating rate of the third stage during the first annealing process is 60° C. / h to 80° C. / h; And / or, the final temperature of the third stage of heating in the first annealing process is 500° C. to 660° C.; And / or, the temperature of the second insulation stage during the first annealing process is 500° C. to 660° C.; And / or, the second insulation time in the first annealing process is 10h to 20h; And / or, the final temperature of the first cooling during the first annealing process is 380° C. to 420° C.; And / or, the first cooling method in the first annealing process is air cooling; And / or, the final temperature of the second cooling during the first annealing process is 90° C. to 100° C.; And / or, the second cooling method in the first annealing process is water cooling.

3. The production process according to claim 1, It is characterized in that The pickling solution of the pickling is hydrochloric acid; And / or, the mass fraction of the hydrochloric acid is 12% to 18%; and / or, the temperature of the pickling solution is 70° C. to 90° C.; And / or, the pickling rate is 30m / min to 160m / min; And / or, the pickling further comprises water washing; And / or, the water washing temperature is 60°C to 80°C; and / or, the washing is followed by drying; And / or, the drying is hot air drying; And / or, the temperature of the hot air is 100°C to 140°C.

4. The production process according to claim 1, It is characterized in that The spheroidizing annealing includes a first stage of heating, a second stage of heating, a first stage of heat preservation, a third stage of heating, a second stage of heat preservation, a first stage of cooling, a second stage of cooling and a third stage of cooling; And / or, the heating rate of the first stage during the spheroidizing annealing process is 350°C / h-450°C / h; And / or, the first stage of heating time during the spheroidizing annealing process is 0.4h to 0.6h; And / or, the final temperature of the first stage of heating during the spheroidizing annealing process is 190° C. to 210° C.; And / or, the heating rate of the second stage during the spheroidizing annealing process is 60°C / h to 80°C / h; And / or, the final temperature of the second stage of heating during the spheroidizing annealing process is 380°C to 420°C; And / or, the temperature of the first stage of the spheroidizing annealing process is 380° C. to 420° C.; And / or, the first holding time during the spheroidizing annealing process is 3h to 5h; And / or, the heating rate of the third stage during the spheroidizing annealing process is 60°C / h to 80°C / h; And / or, the final temperature of the third stage of heating during the spheroidizing annealing process is 700° C. to 800° C.; And / or, the temperature of the second stage of the spheroidizing annealing process is 700° C. to 800° C.; And / or, the second holding time during the spheroidizing annealing process is 10 h to 20 h; And / or, the final temperature of the first cooling during the spheroidizing annealing process is 580° C. to 620° C.; And / or, the final temperature of the second cooling during the spheroidizing annealing process is 380° C. to 420° C.; And / or, the second cooling method during the spheroidizing annealing process is air cooling; And / or, the final temperature of the third cooling during the spheroidizing annealing process is 90° C. to 100° C.; And / or, the third cooling method during the spheroidizing annealing process is water cooling.

5. The production process according to claim 1, It is characterized in that The rolling is produced by a wide plate single-stand cold rolling mill; And / or, the cold rolling force is set to 800TON to 1000TON; And / or, the tension of the cold rolling mill is 150KN to 240KN; And / or, the cold rolling working rolls are rolled using rough rolls; and / or, cold rolling reduction of 30% to 40%; And / or, the rolling rate is 200m / min to 300m / min; And / or, the rolling is carried out in a roll shifting mode; And / or, the roller shifting value is 30 mm to 90 mm.

6. The production process according to claim 1, It is characterized in that The second annealing includes a first stage of heating, a second stage of heating, a first stage of heat preservation, a third stage of heating, a second stage of heat preservation, a first stage of cooling, a second stage of cooling and a third stage of cooling; And / or, the heating rate of the first stage during the second annealing process is 350° C. / h-450° C. / h; And / or, the first heating period in the second annealing process is 0.4h to 0.6h; And / or, the final temperature of the first stage of heating in the second annealing process is 190° C. to 210° C.; And / or, the rate of the second heating stage in the second annealing process is 40°C / h to 80°C / h; And / or, the final temperature of the second stage of heating in the second annealing process is 380° C. to 420° C.; And / or, the temperature of the first insulation stage during the second annealing process is 380° C. to 420° C.; And / or, the first insulation time during the second annealing process is 3h to 5h; And / or, the heating rate of the third stage during the second annealing process is 40°C / h to 80°C / h; And / or, the final temperature of the third stage of heating in the second annealing process is 700° C. to 800° C.; And / or, the temperature of the second insulation stage during the second annealing process is 700° C. to 800° C.; And / or, the second insulation time during the second annealing process is 10h to 20h; And / or, the final temperature of the first cooling during the second annealing process is 580° C. to 620° C.; And / or, the final temperature of the second cooling during the second annealing process is 380° C. to 420° C.; And / or, the second cooling method in the second annealing process is air cooling; And / or, the final temperature of the third cooling during the second annealing process is 90° C. to 100° C.; And / or, the third cooling method during the second annealing process is water cooling.

7. The production process according to claim 1, It is characterized in that The 9SiCr cold-rolled wide coil is composed of the following elements by mass fraction: C 0.9% to 0.95%, Si 1.3% to 1.5%, Mn 0.4% to 0.6%, Cr 1.0% to 1.2%, and the balance is Fe and indispensable residual or impurity elements.

8. The production process according to claim 1, It is characterized in that The thickness of the 9SiCr hot-rolled coil is 2.5 mm to 3.5 mm; And / or, the width of the 9SiCr hot-rolled coil is 900 mm to 1500 mm.

9. The production process according to claim 1, It is characterized in that The thickness of the 9SiCr cold-rolled wide coil is 1.5 mm to 1.8 mm; And / or, the width of the 9SiCr cold-rolled wide-width coil is 900 mm to 1500 mm.

10. The production process according to claim 1, It is characterized in that The thickness accuracy of the 9SiCr cold-rolled wide coil is -10μm to 10μm; And / or, the convexity C40 of the 9SiCr cold-rolled wide coil is within 6 μm.

Citation Information

Patent Citations

  • Heat treatment technology of 9SiCr steel

    CN105986091A

  • Manufacturing method of cold-rolled medium-high carbon structural steel

    CN106119495A

  • SK85 carbon tool steel

    CN113621773A

  • Production process of high-carbon tool steel cold-rolled coil plate

    CN114525391A

  • Production of steel plate as cold-roll excellent in flatness of punched parts