Combined fluorine and chlorine removal method for secondary zinc oxide soot
Through the activation of zinc oxide ash and sodium carbonate ball milling and step-by-step alkali washing and high-temperature roasting, the problem of difficult removal of high fluorine-chlorochlorine impurities in zinc oxide ash is solved, efficient and economical fluorine-chlorochlorine removal is achieved, and zinc smelting is improved. The impurity control and valuable metal recovery rate in the process meet the impurity requirements for large-scale zinc smelting, and have good environmental protection and economic benefits.
Patent Information
- Application Number
- CN202410946051.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art is difficult to efficiently and economically remove high fluorine-chloro-impacts from zinc oxide soot, resulting in a high impurity content during zinc electrolysis, affecting zinc smelting efficiency and environmental safety.
After activation by mixing zinc oxide soot and sodium carbonate, the ball mill is washed in step by step and roasted at high temperature to generate soluble fluorochlorochloride salt and remove it. Through a multi-step process, efficient fluorochlorochloride removal is achieved and the loss of valuable metals is reduced.
The deep removal of fluorine-chlorochlorine in zinc oxide ash is achieved, the fluorine-chlorochlorine content in zinc electrolytic raw materials is reduced, the recovery rate and economic benefits of valuable metals are improved, and the impurity requirements for large-scale zinc smelting is met, and the process is provided. The advantages of reason, low cost and environmental protection.
Smart Images

Figure CN118880045A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy and chemical industry, and in particular to a combined defluorination and dechlorination method for zinc oxide ash. Background Art
[0002] During zinc electrolysis in the zinc hydrometallurgy process, high levels of impurity elements such as As, Sb, Pb, F, and Cl can lead to zinc electrolysis plate burning, increased zinc energy consumption, or reduced quality of precipitated zinc, and increased production costs for zinc smelting. For example, fluoride ions destroy the aluminum oxide film on the surface of the cathode aluminum plate, forming a zinc-aluminum solid solution that makes it difficult to peel off the zinc sheet, resulting in increased consumption of the cathode aluminum plate, which affects the company's production capacity and, in severe cases, leads to production stoppages. At the same time, F is a highly toxic substance, and high fluorine content will deteriorate the workshop working environment and affect the health of the company's employees. Chlorine mainly affects the anode lead plate during the electrolysis process, causing the quality of the precipitated zinc to deteriorate. With the advancement of science and technology, zinc electrolytic plates are becoming larger and larger, and zinc stripping is mechanized. Therefore, the requirements for impurities in the electrolytic process are more stringent. For example, the new liquid index control in the zinc hydrometallurgy process is: As≤0.0002g / L, Sb≤0.0002g / L, Cl≤0.3g / L, F≤0.03g / L, and the quality control of zinc oxide entering the hydrometallurgy is: Cl≤0.08%, F≤0.006%.
[0003] With the progress of zinc smelting and the expansion of zinc production, the supply of zinc sulfide concentrate is becoming increasingly exhausted, and secondary zinc oxide has become an important secondary zinc resource. There are 6 main types of secondary zinc oxide: 1. Zinc oxide dust produced by the volatilization of wet zinc smelting slag through a rotary kiln; 2. Hot-dip galvanizing ash; 3. Zinc oxide dust produced in the recycling process of galvanized steel scrap; 4. Zinc oxide dust produced by a lead fuming furnace; 5. Zinc oxide dust, a byproduct of brass smelting; 6. Zinc oxide dust produced by the reduction and volatilization of blast furnace dust from steelmaking. There are differences in the types and contents of valuable metals such as zinc, lead, indium, silver, cadmium, cobalt, and nickel in secondary zinc oxide dust from different sources, and the contents of impurities As, Sb, F, and Cl vary greatly. For high-fluorine and chlorine secondary zinc oxide, the contents of F and Cl exceed 0.45% and 8.5% respectively, and it is difficult to remove them cleanly in one method during the pretreatment and impurity removal process of the enterprise.
[0004] At present, there are three main methods for pretreatment and impurity removal of zinc oxide: roasting, alkali washing or roasting-alkali washing combined method: roasting is a method in which the fluoride and chloride in zinc oxide undergo physical and chemical changes in a multi-chamber furnace at a high temperature of about 700°C and a certain negative pressure in the furnace is maintained, so that the fluorine and chlorine compounds are desorbed and returned to the gas phase, the low-boiling point fluorine and chlorine compounds are volatilized, and the fluorine and chlorine compounds of lead and zinc are decomposed into gaseous state, which enter the flue gas system along with the furnace gas and zinc oxide smoke and are removed. However, the multi-chamber furnace equipment has high one-time investment and high energy consumption, and the equipment is easily damaged and has high maintenance costs. It is mainly used for zinc oxide raw materials with F and Cl contents below 0.2% and 1% respectively, and the removal rate of F and Cl is less than 85%. For zinc oxide smoke with high fluorine and chlorine content, the removal effect is poor.
[0005] The alkaline washing method utilizes the principle of double decomposition reaction, taking advantage of the fact that alkali metals and halogen compounds are easily soluble in water, while lead and zinc react with alkali or carbonate ions to form compounds that are insoluble in weak alkalis to achieve the purpose of separation from fluorine and chlorine. Alkaline washing for fluorine and chlorine removal has the advantages of simple equipment and operation, and low cost, but a single alkaline washing process is difficult to remove completely, and the amount of wastewater is large, and the zinc loss rate is high.
[0006] The roasting-alkali washing method mainly uses the roasting method to volatilize most of the fluorine-containing chlorine compounds first, and decompose a small amount of non-volatile fluorine and chloride compounds at the same time, and then use the alkali washing method to elute the fluorine and chlorine into the solution. Compared with the roasting method or wet method alone, the advantages of this method are strong applicability to raw material treatment and high fluorine and chlorine removal rate. The disadvantages are that the process is long and the energy consumption is still high. A large amount of valuable metals such as lead, indium, and cadmium enter the smoke dust with the flue gas. If they are to be recovered, another production line needs to be built, which increases the production cost.
[0007] For example, the invention patent CN 112538568A adopts a disguised roasting and alkali washing method, which has a low roasting temperature, thereby reducing energy consumption. However, a large amount of valuable metals such as lead, indium, and cadmium still enter the smoke dust in the form of chlorides or fluorides with the flue gas, causing the valuable metals such as lead, indium, and cadmium to be dispersed, reducing the recovery rate of lead, indium, and cadmium in the main system, and increasing production costs. At the same time, the removal rate of F and Cl is about 95%, which is still difficult to meet the impurity requirements of large-scale cathode plate electrolysis.
[0008] Therefore, how to find an efficient, environmentally friendly, low-cost one-time deep treatment method for zinc oxide powder with F and Cl contents reaching or even exceeding 0.50% and 9.50% respectively to meet the requirements of large-scale zinc cathode electrolytic zinc raw materials is an urgent problem that needs to be solved. Therefore, it is imperative to seek a more economical, environmentally friendly, energy-saving and efficient method for deep removal of arsenic, antimony, fluorine, chlorine and other impurities from zinc oxide. Summary of the invention
[0009] The purpose of the present invention is to provide an economical, reasonable, environmentally friendly, energy-saving and efficient combined defluorination and dechlorination method for zinc oxide fly ash, so as to solve the problem that F and Cl in zinc oxide fly ash with F and Cl contents reaching 0.50% and 9.50% respectively are difficult to be completely and effectively removed, so as to ensure that zinc oxide fly ash with F and Cl contents reaching or even exceeding 0.50% and 9.50% respectively can meet the requirements for large-scale zinc cathode electrolytic zinc raw materials in the zinc hydrometallurgy process after impurity removal treatment.
[0010] In order to solve the above technical problems, the present invention provides a combined defluorination and dechlorination method for zinc oxide ash, which is suitable for defluorination and dechlorination of zinc oxide ash with fluorine and chlorine contents of 0.50% and 9.50% respectively, and comprises the following steps:
[0011] The zinc oxide ash is mixed with sodium carbonate and then ball-milled with water for activation pretreatment to obtain zinc oxide particles;
[0012] The zinc oxide particles are subjected to a first-stage alkali washing with an alkali washing agent, and then filtered to obtain a first-stage alkali washing liquid and a first-stage alkali washing residue;
[0013] The first-stage alkali-washed residue is subjected to second-stage alkali-washing with an alkali-washing agent, and then filtered to obtain a second-stage alkali-washing liquid and a second-stage alkali-washed residue;
[0014] The second-stage alkali-washed slag is roasted and cooled to obtain roasted zinc oxide sand;
[0015] The zinc oxide roasted sand is ball-milled and then sent to the zinc hydrometallurgical system to recover valuable metals.
[0016] Furthermore, the molar amount of the sodium carbonate is 0.3 to 0.5 times the sum of the molar numbers of fluorine and chlorine in the secondary zinc oxide ash.
[0017] Furthermore, the liquid-to-solid weight ratio of the secondary zinc oxide ash to the sodium carbonate solid to the water is 1.5:1 to 3:1.
[0018] Furthermore, the temperature of the ball milling activation pretreatment is 30 to 65° C., and the time is 5 to 30 minutes.
[0019] Furthermore, the median particle size of the secondary zinc oxide particles is 410-450 meshes.
[0020] Furthermore, the liquid-to-solid weight ratio of the alkali cleaning agent to the secondary zinc oxide particles in the first alkali cleaning is 5:1 to 8:1, the temperature of the first alkali cleaning is 70 to 85° C., and the time is 90 to 120 minutes.
[0021] Furthermore, after the first alkali washing is completed, if the Cl in the first alkali washing liquid is ≥60g / L, the first alkali washing liquid is purified and evaporated to produce sodium chloride and / or potassium chloride products; if the Cl in the first alkali washing liquid is <60g / L, it is returned to pretreatment for reuse.
[0022] Furthermore, the liquid-to-solid weight ratio of the alkali washing agent of the second stage alkali washing to the first stage alkali washing slag is 3:1-5:1, the temperature of the second stage alkali washing is 55-65°C, the time is 30-90min, and the obtained second stage alkali washing liquid is returned to the pretreatment for reuse.
[0023] Furthermore, the alkaline cleaning agent is a saturated alkaline solution, the solute in the saturated alkaline solution is one or two of sodium carbonate, potassium carbonate, sodium hydroxide and potassium hydroxide, and the mass ratio of the carbonate to the alkali is 3:1 to 5:1.
[0024] Furthermore, the temperature of the second-stage alkali-washed slag roasting is 650-720° C. and the time is 1.5-3.5 hours.
[0025] Furthermore, the smoke containing F and Cl impurities generated by the second-stage alkali-washed slag roasting is discharged after the smoke is cooled and dust-collected and meets the standards.
[0026] Furthermore, the zinc oxide roasted sand is ball-milled to a size of D50=240-350 mesh.
[0027] The invention provides a combined defluorination and dechlorination method for zinc oxide ash, wherein the zinc oxide ash is mixed with sodium carbonate and water, and then ball milled for activation, so that the insoluble basic fluoride and basic chloride in the zinc oxide ash react with the sodium carbonate to generate soluble fluoride and chloride salts and insoluble zinc compounds. Then, the zinc oxide granules obtained by ball milling activation pretreatment are alkali washed in steps, so that the soluble fluoride and chloride salts in the zinc oxide granules can be fully dissolved in the alkali washing agent, so that more than 94% of the fluoride and chloride in the zinc oxide ash can be removed, so that the residual fluoride and chloride in the alkali washing residue obtained by final filtration only exist in the form of a small amount of low-boiling valuable metal fluoride salt or valuable metal chloride salt. Then, the alkali washing residue obtained by final filtration is roasted, so that a small amount of low-boiling valuable metal fluoride salt or valuable metal chloride salt in the alkali washing residue can enter the smoke. In this way, the fluorine and chlorine in the zinc oxide roasted sand obtained by roasting are removed to below 0.006wt% and 0.08wt%, respectively, which solves the problem that F and Cl in the secondary zinc oxide fly ash with F and Cl contents of 0.50% and 9.50% respectively are difficult to be completely and effectively removed, thereby ensuring that the secondary zinc oxide fly ash with F and Cl contents reaching or even exceeding 0.50% and 9.50% respectively can meet the requirements for large-scale zinc cathode electrolytic zinc raw materials in the zinc hydrometallurgy process after impurity removal treatment.
[0028] Moreover, only a small amount of the valuable metals in the zinc oxide roasted sand enters the smoke in the form of low-boiling-point valuable metal fluoride salts and valuable metal chloride salts, and most of the valuable metals in the secondary zinc oxide ash still remain in the zinc oxide roasted sand. After the zinc oxide roasted sand is ball-milled, it is sent to the zinc hydrometallurgy system to recover the valuable metals therein, so that the direct recovery rate of valuable metals such as zinc, indium, lead, cadmium, etc. in the secondary zinc oxide ash can exceed 98.5%.
[0029] Therefore, the combined defluorination and dechlorination method of zinc oxide ash provided by the present invention can not only efficiently remove fluorine and chlorine from the zinc oxide ash in depth, thereby ensuring the requirements for the fluorine and chlorine content in the zinc electrolysis raw materials in the subsequent zinc hydrometallurgy and zinc extraction, but also improve the direct recovery rate of valuable metals such as zinc, lead, indium, and cadmium, thereby improving the economic benefits.
[0030] At the same time, the combined defluorination and dechlorination method of zinc oxide ash provided by the present invention also has the advantages of reasonable process, low cost, energy saving and environmental protection, and has a very broad industrialization prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 A flow chart of a combined defluorination and dechlorination method for zinc oxide ash provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0032] See also Figure 1 The embodiment of the present invention provides a combined defluorination and dechlorination method for zinc oxide ash, which is most suitable for defluorination and dechlorination of zinc oxide ash with fluorine and chlorine contents of 0.50% and 9.50% respectively, and comprises the following steps:
[0033] Step 1) Pretreatment: zinc oxide ash is mixed with sodium carbonate, water is added, and then ball milling is performed for activation pretreatment to obtain zinc oxide particles.
[0034] The molar amount of sodium carbonate added to the zinc oxide ash is 0.3 to 0.5 times the sum of the molar numbers of fluorine and chlorine in the zinc oxide ash.
[0035] Sodium carbonate is added to zinc oxide ash and water is added to mix, wherein the liquid-solid weight ratio of the zinc oxide ash and sodium carbonate to the added water is 1.5:1-3:1.
[0036] The zinc oxide ash is mixed with sodium carbonate and water and then sent to a ball mill for ball milling activation pretreatment. During the ball milling activation pretreatment process, the insoluble basic fluoride and basic chloride in the zinc oxide ash react with sodium carbonate to generate soluble fluoride and chlorine salts and insoluble zinc compounds, and the generated soluble fluoride and chlorine salts and insoluble zinc compounds remain in the zinc oxide particles obtained by the ball milling activation pretreatment.
[0037] In order to quickly and fully activate the secondary zinc oxide ash and sodium carbonate, the temperature during ball milling activation pretreatment is set to 30-65°C and the activation time is 5-30 minutes.
[0038] The chemical reactions that occur during the ball milling activation pretreatment process are as follows:
[0039] Zn5(OH)8F2·H2O+5Na2CO3→2NaF+5ZnCO3↓+H2O+8NaOH
[0040] Zn5(OH)8Cl2·H2O+5Na2CO3→2NaCl+5ZnCO3↓+H2O+8NaOH
[0041] ZnF2+2NaOH→2NaF+Zn(OH)2↓
[0042] ZnCl2+2NaOH→2NaCl+Zn(OH)2↓
[0043] In order to facilitate the leaching of soluble fluoride and chlorine salts from the zinc oxide granules in the subsequent alkali washing step, the medium particle size of the zinc oxide granules is controlled to be 410-450 meshes.
[0044] Step 2) one-stage alkali washing: the zinc oxide particles are subjected to one-stage alkali washing with an alkali washing agent, and then filtered to obtain a first-stage alkali washing liquid and a first-stage alkali washing residue.
[0045] In order to leach out the soluble fluoride and chlorine salts in the zinc oxide particles, the zinc oxide particles obtained by ball milling activation pretreatment are added to an alkali cleaning agent for a stage of alkali cleaning, so that the soluble fluoride and chlorine salts in the zinc oxide particles are dissolved in the alkali cleaning agent.
[0046] Wherein, the alkaline cleaning agent is a saturated alkaline solution, and the solute in the saturated alkaline solution is one or two of sodium carbonate, potassium carbonate, sodium hydroxide and potassium hydroxide.
[0047] As a preferred embodiment of the present invention, the alkaline cleaning agent used in the first stage of alkaline cleaning is a saturated solution of carbonate and alkali.
[0048] Wherein, the mass ratio of carbonate to alkali is 3:1 to 5:1.
[0049] Among them, the carbonate is sodium carbonate or potassium carbonate, and the alkali is sodium hydroxide or potassium hydroxide.
[0050] In order to make the soluble fluorine and chlorine salts in the zinc oxide particles quickly and fully dissolve in the alkali cleaning agent, the liquid-solid weight ratio of the alkali cleaning agent to the zinc oxide particles in the first alkali cleaning is controlled at 5:1-8:1, the temperature of the first alkali cleaning is controlled at 70-85°C, and the alkali cleaning time is controlled at 90-120 minutes.
[0051] Furthermore, after a stage of alkali washing is completed, the filtered alkali washing liquid is tested for chlorine element. If the Cl in the alkali washing liquid is ≥60g / L, the alkali washing liquid has no recycling value. At this time, the alkali washing liquid is discharged in an open circuit and purified and evaporated to produce products such as sodium chloride and / or potassium chloride.
[0052] If the Cl in the first-stage alkaline washing liquid is less than 60 g / L, the first-stage alkaline washing liquid is returned to the pretreatment stage of step 1) for reuse so as to participate in the activation of the secondary zinc oxide soot.
[0053] Step 3) Second stage alkali washing: the first stage alkali washing residue is subjected to second stage alkali washing with an alkali washing agent, and then filtered to obtain a second stage alkali washing liquid and a second stage alkali washing residue.
[0054] In order to further leach the soluble fluoride and chloride salts remaining in the first-stage alkali washing residue, the first-stage alkali washing residue is added into the alkali washing liquid for the second-stage alkali washing.
[0055] Wherein, the alkaline cleaning agent is a saturated alkaline solution, and the solute in the saturated alkaline solution is one or two of sodium carbonate, potassium carbonate, sodium hydroxide and potassium hydroxide.
[0056] As a preferred embodiment of the present invention, the solute in the alkaline cleaning agent used in the second-stage alkaline cleaning is one of sodium carbonate, potassium carbonate, sodium hydroxide and potassium hydroxide.
[0057] In order to make the soluble fluorine and chloride salts remaining in the first-stage alkali washing slag dissolve quickly and fully in the alkali washing agent, the liquid-solid weight ratio of the alkali washing agent of the second-stage alkali washing to the first-stage alkali washing slag is controlled at 3:1-5:1, the temperature of the second-stage alkali washing is controlled at 55-65°C, and the alkali washing time is controlled at 30-90 minutes.
[0058] After the second stage alkali washing, the second stage alkali washing liquid and the second stage alkali washing residue are obtained by filtration. Since the chlorine content in the second stage alkali washing liquid obtained by the second stage alkali washing is already very low, the obtained second stage alkali washing liquid is directly returned to the pretreatment stage for reuse to participate in the activation of the secondary zinc oxide ash.
[0059] The zinc oxide particles obtained by ball milling activation pretreatment are subjected to the above two steps of alkali washing, so that the soluble fluoride and chlorine salts in the zinc oxide particles can be fully dissolved in the alkali washing agent, and more than 94% of the fluoride and chlorine in the zinc oxide ash can be removed, so that the residual fluoride and chlorine in the second-stage alkali washing residue obtained by final filtration exists only in a small amount of low-boiling point valuable metal fluoride salt or valuable metal chloride salt.
[0060] Step 4) high temperature roasting: roasting the second-stage alkali-washed slag and cooling it to obtain zinc oxide roasted sand.
[0061] The temperature of the second-stage alkali-washed slag roasting is 650-720°C and the time is 1.5-3.5h.
[0062] The roasting of the second-stage alkali-washed slag can make a small amount of low-boiling-point valuable metal fluoride salt or valuable metal chloride salt in the second-stage alkali-washed slag enter the smoke dust. In this way, the fluorine and chlorine in the roasted zinc oxide sand obtained by roasting are removed to below 0.006wt% and 0.08wt%, solving the problem that F and Cl in the secondary zinc oxide ash with F and Cl contents of 0.50% and 9.50% respectively are difficult to be completely and effectively removed, thereby ensuring that the secondary zinc oxide ash with F and Cl contents reaching or even exceeding 0.50% and 9.50% respectively can meet the requirements of large-scale zinc cathode electrolytic zinc raw materials in the zinc hydrometallurgy process after impurity removal treatment.
[0063] The equipment used for roasting the second-stage alkali-washed slag is a rotary kiln, a multi-chamber furnace or a fluidized bed furnace.
[0064] During the second-stage alkaline-washed slag roasting process, the smoke containing F and Cl impurities is discharged after the flue gas is cooled and dust collected and meets the standards.
[0065] Step 5) ball milling: The zinc oxide roasted sand is ball milled to D50 = 240-350 mesh and then sent to the zinc hydrometallurgical system to recover valuable metals such as zinc, indium, lead, and cadmium.
[0066] Since only a small amount of valuable metals in the zinc oxide roasted sand enters the smoke in the form of low-boiling point valuable metal fluoride salts and valuable metal chloride salts, most of the valuable metals in the secondary zinc oxide ash still remain in the zinc oxide roasted sand. After the zinc oxide roasted sand is ball-milled, it is sent to the zinc hydrometallurgy system to recover the valuable metals therein, so that the direct recovery rate of valuable metals such as zinc, indium, lead, cadmium, etc. in the secondary zinc oxide ash can exceed 98.5%.
[0067] The combined defluorination and dechlorination method of zinc oxide ash provided by the present invention can not only effectively remove fluorine and chlorine from zinc oxide ash in depth through the process of pretreatment, two-stage alkali washing, high-temperature roasting and ball milling, thereby ensuring the requirements for the fluorine and chlorine content in zinc electrolysis raw materials in subsequent zinc hydrometallurgy and zinc extraction, but also improve the direct recovery rate of valuable metals such as zinc, lead, indium and cadmium, thereby improving the economic benefits.
[0068] Moreover, the combined defluorination and dechlorination method of zinc oxide ash provided by the present invention also has the advantages of reasonable process, low cost, energy saving and environmental protection, and has a very broad industrialization prospect.
[0069] The combined defluorination and dechlorination method of zinc oxide ash provided by the present invention is specifically described and compared by way of examples and comparative examples.
[0070] Example 1
[0071] The combined defluorination and dechlorination of zinc oxide soot with the composition of Zn 53.47wt%, Fe 1.16wt%, Pb1.43wt%, Cd0.042wt%, In0.16wt%, F 0.57wt%, Cl 10.02wt% is as follows:
[0072] 1. Pretreatment: Add sodium carbonate 0.3 times the theoretical molar sum of F and Cl to the zinc oxide ash containing 0.57wt% F and 10.02wt% Cl, mix and add water, then perform ball milling activation. The liquid-solid weight ratio is 3:1, the temperature is 30°C, the time is 30min, and the zinc oxide D50 after ball milling activation is 450 mesh.
[0073] 2. One-stage alkali washing: add the zinc oxide activated by ball milling into a mixed alkali washing agent whose solute is sodium carbonate and sodium hydroxide, the liquid-solid weight ratio of the alkali washing agent to the zinc oxide is 5:1, carry out one-stage alkali washing at a temperature of 85°C for 120 minutes, and then filter to obtain the alkali washing liquid and alkali washing residue.
[0074] 3. Second stage alkali washing: the alkali washing residue is subjected to second stage alkali washing with an alkali washing agent whose solute is potassium carbonate, with a liquid-solid weight ratio of 5:1, a temperature of 55°C, and a time of 90 min, and the second stage alkali washing liquid and the second stage alkali washing residue are obtained by filtration.
[0075] 4. High-temperature roasting: The second-stage alkali-washed slag is transferred to a rotary kiln for roasting at 720°C for 1.5 hours. After cooling, zinc oxide roasted sand is obtained. The smoke containing impurities such as F and Cl is cooled and dust-collected along with the flue gas and then discharged after meeting the standards.
[0076] 5. Ball milling: The zinc oxide roasted sand is ball milled to D50=350 mesh and then fed to the zinc hydrometallurgical system to recover the valuable metals zinc, indium, lead, cadmium, etc.
[0077] Through the combined defluorination and dechlorination test of secondary zinc oxide ash, the direct recovery rate of zinc and indium reached 99.05%, the direct recovery rate of lead and cadmium was 98.85%, the content of F and Cl in the second-stage alkali washing slag was 0.036% and 0.28% respectively, the content of F and Cl in zinc oxide roasted sand was 0.0042% and 0.068% respectively, and the removal rate of fluorine and chlorine was 99.25% and 99.39% respectively. After leaching and purification of the original process in the wet smelting, the zinc oxide roasted sand obtained a new liquid with a content of Cl 0.24g / L and F 0.021g / L, which meets the requirements of large-scale zinc electrolytic plates for new liquid.
[0078] Example 2
[0079] The combined defluorination and chlorination is carried out using zinc oxide with a composition of Zn 53.47wt%, Fe 1.16wt%, Pb1.43wt%, Cd0.042wt%, In0.16wt%, F 0.57wt%, and Cl 10.02wt%, as follows:
[0080] 1. Pretreatment: Add sodium carbonate 0.5 times the theoretical molar sum of F and Cl to zinc oxide ash containing 0.57wt% F and 10.02wt% Cl, mix and add water, then perform ball milling activation. The liquid-solid weight ratio is 1.5:1, the temperature is 65°C, the time is 5 minutes, and the zinc oxide D50 after ball milling activation is 410 mesh.
[0081] 2. One-stage alkali washing: add the ball-milled activated zinc oxide into a mixed alkali washing agent whose solute is potassium carbonate and potassium hydroxide, the liquid-solid weight ratio of the alkali washing agent to the zinc oxide is 8:1, carry out one-stage alkali washing at a temperature of 70°C for 90 minutes, and filter to obtain the alkali washing liquid and alkali washing residue.
[0082] 3. Second stage alkali washing: the alkali washing residue is subjected to second stage alkali washing with an alkali washing agent whose solute is sodium carbonate, with a liquid-solid weight ratio of 3:1, a temperature of 65°C, and a time of 30 min, and the second stage alkali washing liquid and the second stage alkali washing residue are obtained by filtration.
[0083] 4. High-temperature roasting: The second-stage alkali-washed slag is transferred to a multi-chamber furnace and roasted at a temperature of 650°C for 3.5 hours. After cooling, zinc oxide roasted sand is obtained. The smoke containing impurities such as F and Cl is cooled and dust-collected along with the flue gas and then discharged after meeting the standards.
[0084] 5. Ball milling: The zinc oxide roasted sand is ball milled to D50 = 240 mesh and then fed to the zinc hydrometallurgical system to recover the valuable metals zinc, indium, lead, cadmium, etc.
[0085] Through the test of combined defluorination and dechlorination of secondary zinc oxide fly ash, it is calculated that the direct recovery rate of zinc and indium is 99.21%, the direct recovery rate of lead and cadmium is 98.92%, the contents of F and Cl in the second-stage alkali washing slag are 0.034% and 0.31% respectively, the contents of F and Cl in the zinc oxide roasted sand are 0.0051% and 0.072% respectively, and the removal rates of fluorine and chlorine are 99.19% and 99.35% respectively; the zinc oxide roasted sand is leached and purified by the original process in the wet smelting to obtain a new liquid with a content of Cl 0.26g / L and F 0.022g / L, which meets the requirements of large-scale zinc electrolytic plates for new liquid.
[0086] Example 3
[0087] The combined defluorination and dechlorination of zinc oxide soot with the composition of Zn 53.47wt%, Fe 1.16wt%, Pb1.43wt%, Cd0.042wt%, In0.16wt%, F 0.57wt%, Cl 10.02wt% is as follows:
[0088] 1. Pretreatment: Add sodium carbonate 0.4 times the theoretical molar sum of F and Cl to zinc oxide ash containing 0.57wt% F and 10.02wt% Cl, mix and add water, then perform ball milling activation. The liquid-solid weight ratio is 2:1, the temperature is 45°C, the time is 15min, and the zinc oxide D50 after ball milling activation is 425 mesh.
[0089] 2. One-stage alkali washing: add the ball-milled activated zinc oxide into a mixed alkali washing agent whose solute is potassium carbonate and sodium hydroxide, the liquid-solid weight ratio of the alkali washing agent to the zinc oxide is 7:1, carry out one-stage alkali washing at a temperature of 80°C for 110 minutes, and filter to obtain the alkali washing liquid and alkali washing residue.
[0090] 3. Second stage alkali washing: the alkali washing residue is subjected to second stage alkali washing with an alkali washing agent whose solute is sodium hydroxide, with a liquid-solid weight ratio of 4:1, a temperature of 60°C, and a time of 60 min, and the second stage alkali washing liquid and the second stage alkali washing residue are obtained by filtration.
[0091] 4. High-temperature roasting: The second-stage alkali-washed slag is transferred to a boiling furnace and roasted at a temperature of 690°C for 2.5 hours. After cooling, zinc oxide roasted sand is obtained. The smoke containing impurities such as F and Cl is cooled and dust collected along with the flue gas and then discharged after meeting the standards.
[0092] 5. Ball milling: The zinc oxide roasted sand is ball milled to D50 = 290 mesh and then fed to the zinc hydrometallurgical system to recover the valuable metals zinc, indium, lead, cadmium, etc.
[0093] Through the test of combined defluorination and dechlorination of secondary zinc oxide fly ash, it is calculated that the direct recovery rate of zinc and indium is 99.21%, the direct recovery rate of lead and cadmium is 98.92%, the contents of F and Cl in the second-stage alkali washing slag are 0.034% and 0.31% respectively, the contents of F and Cl in the zinc oxide roasted sand are 0.0051% and 0.072% respectively, and the removal rates of fluorine and chlorine are 99.19% and 99.35% respectively; the zinc oxide roasted sand is leached and purified by the original process in the wet smelting to obtain a new liquid with a content of Cl 0.26g / L and F 0.022g / L, which meets the requirements of large-scale zinc electrolytic plates for new liquid.
[0094] Comparative Example
[0095] The fluorine and chlorine are removed by roasting and alkali elution using zinc oxide soot with a composition of 53.47wt% Zn, 1.16wt% Fe, 1.43wt% Pb, 0.042wt% Cd, 0.16wt% In, 0.57wt% F and 10.02wt% Cl. The specific situation is as follows:
[0096] The secondary zinc oxide fly ash is roasted in a multi-hearth furnace to remove fluorine and chlorine to obtain zinc oxide roasted sand and fluorine-containing chlorine dust, and the removal rates of fluorine and chlorine are 75.63% and 81.29% respectively. The dust mainly contains zinc chloride, lead chloride, zinc fluoride and lead fluoride, and the direct recovery rate of zinc is 92.85%, and the direct recovery rate of lead is 38.62%. The alkali-washed slag obtained after alkali washing of zinc oxide roasted sand has F and Cl contents of 0.008wt% and 0.26wt% respectively.
[0097] Compared with Examples 1-3 of the present invention, the F and Cl contents in the raw materials entering the zinc hydrometallurgy system for zinc smelting in the control example are significantly higher than the enterprise standards of large-plate zinc electrolysis enterprises. During the zinc electrolysis process, large areas of plate burning will occur, the lead content in the precipitated zinc exceeds the standard, and the direct recovery rate of valuable metals zinc and lead is significantly low.
[0098] Therefore, compared with the comparative example, the combined defluorination and dechlorination method of zinc oxide ash provided in Examples 1-3 of the present invention, through the process of pretreatment, two-stage alkali washing, high-temperature roasting and ball milling, can not only efficiently remove fluorine and chlorine from zinc oxide ash in depth, thereby ensuring the requirements for the fluorine and chlorine content in the zinc electrolysis raw materials in the subsequent zinc hydrometallurgy for zinc extraction, but also can improve the direct recovery rate of valuable metals such as zinc, lead, indium, and cadmium, thereby improving the economic benefits.
[0099] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A combined defluorination and dechlorination method for zinc oxide fly ash, suitable for defluorination and dechlorination of zinc oxide fly ash with fluorine and chlorine contents of 0.50% and 9.50% respectively, characterized in that: The steps include: The zinc oxide ash is mixed with sodium carbonate, water is added, and then ball milling is performed for activation pretreatment to obtain zinc oxide particles; The zinc oxide particles are subjected to a first-stage alkali washing with an alkali washing agent, and then filtered to obtain a first-stage alkali washing liquid and a first-stage alkali washing residue; The first-stage alkali-washed residue is subjected to second-stage alkali-washing with an alkali-washing agent, and then filtered to obtain a second-stage alkali-washing liquid and a second-stage alkali-washed residue; The second-stage alkali-washed slag is roasted and cooled to obtain roasted zinc oxide sand; The zinc oxide roasted sand is ball-milled and then sent to the zinc hydrometallurgical system to recover valuable metals.
2. The combined defluorination and dechlorination method of zinc oxide ash according to claim 1, characterized in that: The molar amount of the sodium carbonate is 0.3 to 0.5 times the sum of the molar numbers of fluorine and chlorine in the zinc oxide ash, and the liquid-solid weight ratio of the zinc oxide ash to the sodium carbonate solid and water is 1.5:1 to 3:
1.
3. The combined defluorination and chlorination method of zinc oxide ash according to claim 2, characterized in that: The temperature of the ball milling activation pretreatment is 30-65° C., and the time is 5-30 minutes; the medium particle size of the secondary zinc oxide particles is 410-450 meshes.
4. The combined defluorination and dechlorination method of zinc oxide ash according to claim 1, characterized in that: The liquid-to-solid weight ratio of the alkali cleaning agent to the secondary zinc oxide particles in the first alkali cleaning is 5:1-8:1, the temperature of the first alkali cleaning is 70-85° C., and the time is 90-120 minutes.
5. The combined defluorination and dechlorination method of zinc oxide ash according to claim 4, characterized in that: After the first stage of alkali washing is completed, if the Cl in the first stage of alkali washing liquid is ≥60g / L, the first stage of alkali washing liquid is purified and evaporated to produce sodium chloride and / or potassium chloride products; if the Cl in the first stage of alkali washing liquid is <60g / L, it is returned to pretreatment for reuse.
6. The combined defluorination and dechlorination method of zinc oxide ash according to claim 1, characterized in that: The liquid-solid weight ratio of the alkali washing agent of the second stage alkali washing to the first stage alkali washing residue is 3:1-5:1, the temperature of the second stage alkali washing is 55-65°C, the time is 30-90 minutes, and the obtained second stage alkali washing liquid is returned to the pretreatment for reuse.
7. The combined defluorination and dechlorination method of zinc oxide ash according to claim 4 or 6, characterized in that: The alkaline cleaning agent is a saturated alkaline solution, the solute in the saturated alkaline solution is one or two of sodium carbonate, potassium carbonate, sodium hydroxide and potassium hydroxide, and the mass ratio of the carbonate to the alkali is 3:1 to 5:
1.
8. The combined defluorination and dechlorination method of zinc oxide ash according to claim 1, characterized in that: The temperature of the second-stage alkali-washed slag roasting is 650-720° C. and the time is 1.5-3.5 hours.
9. The combined defluorination and dechlorination method of zinc oxide ash according to claim 8, characterized in that: The smoke dust containing F and Cl impurities generated by the second-stage alkali-washed slag roasting is discharged after being cooled and dust-collected along with the smoke gas and meeting the standards.
10. The combined defluorination and dechlorination method of zinc oxide ash according to claim 1, characterized in that: The zinc oxide calcined sand is ball-milled to a size of D50=240-350 meshes.
Citation Information
Patent Citations
Method for removing fluorine and chlorine in zinc oxide powder by low-temperature roasting and water washing
CN112538568A
Cited By
Method for continuously removing fluorine and chlorine in fluorine-chlorine-containing zinc oxide waste by differential contact type countercurrent washing tower
CN119320876A