Alpha + beta double-phase high-toughness brass alloy material with harmonic structure
The harmonic structure α+β biphasic brass alloy material prepared by homogenization annealing-hot rolling-annealing process solves the problem of strength-plastic mismatch between brass alloy and achieves coordination between strength and plasticity. The process flow is simplified and suitable for industrial production.
Patent Information
- Application Number
- CN202410926975.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-01
AI Technical Summary
Brass alloy has problems with strength-plastic mismatch in terms of mechanical properties. The existing lifting methods are cumbersome, costly and difficult to take into account both strength and tough plasticity, which limits its application in the field of high-tech.
The homogenized annealing-hot rolling-annealing process is used to prepare α+β biphasic high-strength brass alloy material with harmonic structure. The α phase is formed as the core through specific ratios of copper, zinc, aluminum and iron and the process steps. , the structure of α+β phase as shell simplifies the process flow and is suitable for industrial production.
A perfect combination between strength and plasticity is achieved. The microstructure of the material is characterized by α phase as the core and α+β phase as the shell, the grain size is consistent, and the heterostructure is characterized by phase gradient, which simplifies the process and improves efficiency and cost. Benefits, suitable for industrial production.
Smart Images

Figure CN118880103A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal materials, and in particular relates to an α+β two-phase high-strength and toughness brass alloy material with a harmonic structure. Background Art
[0002] Brass alloy materials are widely used in the fields of electronics, power, aerospace, transportation, etc. due to their excellent electrical and thermal conductivity, ductility, corrosion resistance and low price. However, with the rapid development of science and technology, modern industry requires copper alloy materials to have better mechanical properties on the basis of their original properties to meet the requirements of various high-tech fields. Brass can be divided into α-phase brass, α+β-duplex brass and β-phase brass according to different microstructures. The α-phase is a solid solution of Zn atoms in copper with a face-centered cubic lattice; while the β-phase is a solid solution based on the electronic compound CuZn with a body-centered cubic lattice. At present, the most widely used are α-phase and α+β-duplex brass, which have good plasticity but relatively low strength. Although the β-phase brass has high strength, when the temperature drops to 456-468℃, the β-phase will undergo an ordered transformation from the β-phase to the β′ phase, and the ordered β′ phase has fewer slip systems and limited ability to resist deformation, which greatly deteriorates the plasticity of the alloy. In addition, the grain size of single β brass alloy is coarse, which easily produces polycrystalline brittleness and reduces the overall plasticity of the alloy. Therefore, the problem of strength-plasticity mismatch is common in brass alloy systems, which limits the further application of brass in high-tech fields.
[0003] At present, there are three main methods to improve the performance of brass alloys: large plastic deformation, heat treatment and microalloying. Although these methods can improve the mechanical properties of alloys, they inevitably have some defects: deformation heat treatment and large plastic deformation are cumbersome and expensive, which is not conducive to industrial production. In addition, large plastic deformation will lead to reduced plasticity of the alloy, and microalloying is also difficult to take into account the strength and toughness of the alloy. Therefore, a performance improvement strategy that satisfies the strength-plasticity match is urgently needed in brass alloys. Heterostructure materials have recently received widespread attention. They are a class of materials composed of heterogeneous regions with significantly different (>100%) mechanical properties or physical properties. Unlike traditional materials, the heterogeneous deformation-induced strengthening and heterogeneous deformation-induced strain hardening generated by the interactive coupling between different property regions of heterostructure materials during deformation make the material have excellent strength-plasticity adaptability, which subverts people's previous predictions of material properties.
[0004] As a kind of heterogeneous structural material, harmonic structural material (also known as core-shell structural material) was first proposed by scholars Ameyama et al., and has gradually attracted people's interest due to its unique microstructure. The main feature of the harmonic structure is that coarse grains are embedded in a three-dimensional grid structure composed of ultrafine grains. At present, harmonic materials are mainly manufactured by powder metallurgy with severe plastic deformation. The powder is subjected to severe deformation processes such as ball milling and high-pressure gas ball milling to form a bimodal structure powder with fine grains on the surface and coarse grains inside, and then metallurgical sintering is performed to form a heterogeneous structural material with a harmonic structure. However, this method is cumbersome and requires precise control of each process in the preparation process. It is inefficient and costly, which is not conducive to industrial production. Therefore, the development of high-strength and tough brass alloy materials with harmonic structures that can be obtained through simple processes has very important theoretical significance and very broad application prospects. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the prior art and provide an α+β dual-phase high-strength and toughness brass alloy material with a harmonic structure.
[0006] In order to achieve the above objectives, one of the technical solutions of the present invention is: an α+β dual-phase high-strength and toughness brass alloy material with a harmonic structure, having a harmonic structure with an α phase as a core and an α+β dual-phase as a shell, and its composition includes, by weight percentage: 65.5-83.5wt% copper, 14-26wt% zinc, 2-5wt% aluminum and 0.5-3.5wt% iron.
[0007] In a preferred embodiment of the present invention, the composition includes, by weight percentage: 68.5-81.5wt% copper, 15-24wt% zinc, 2.5-4.5wt% aluminum, and 1-3wt% iron.
[0008] In a preferred embodiment of the present invention, the composition includes, by weight percentage: 71-79.5 wt % copper, 16-22 wt % zinc, 3-4 wt % aluminum, and 1.5-3 wt % iron.
[0009] In a preferred embodiment of the present invention, the composition includes, by weight percentage: copper 73.5-78wt%, zinc 17-20wt%, aluminum 3-3.5wt%, and iron 2-3wt%.
[0010] In a preferred embodiment of the present invention, the high-strength and toughness brass alloy material is obtained by subjecting the cast alloy to homogenization annealing-hot rolling-annealing.
[0011] In order to achieve the above objectives, the second technical solution of the present invention is: a method for preparing an α+β dual-phase high-strength and toughness brass alloy material with a harmonic structure, comprising the following steps:
[0012] (1) preparing a cast alloy: copper, zinc, aluminum, and iron are mixed according to the raw material composition ratio of a high-strength and tough brass alloy material, and then smelted and cooled to obtain a cast alloy;
[0013] (2) homogenization annealing treatment: homogenization annealing treatment is performed on the cast alloy obtained in step (1), followed by water cooling to complete the homogenization annealing treatment;
[0014] (3) hot rolling: hot rolling the alloy after homogenization annealing in step (2);
[0015] (4) Annealing: The alloy after hot rolling in step (3) is annealed and then air-cooled to obtain an α+β dual-phase high-strength and toughness brass alloy material with a harmonic structure.
[0016] In a preferred embodiment of the present invention, in step (2), the homogenization annealing temperature is 850-900° C., the homogenization annealing time is 12-36 hours, and the cooling method is water cooling.
[0017] In a preferred embodiment of the present invention, in step (3), the hot rolling temperature is 800-900° C., the number of hot rolling passes is 2-8, and the reduction ratio is 70-90%.
[0018] In a preferred embodiment of the present invention, the annealing temperature in step (4) is 800-850° C., the annealing time is 10-30 min, and the cooling method is air cooling.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The microstructure characteristics of the harmonic material prepared by the present invention are that the α phase is the core and the α+β phase is the shell, and the grain size is almost the same; the heterogeneous structure characteristic of the harmonic material prepared by the present invention is the phase gradient, not the grain size gradient, and the heterogeneous structure characteristic of the harmonic material prepared by the present invention is the grain size gradient.
[0021] 2. The present invention is different from the existing harmonic materials which are mainly manufactured by powder metallurgy with severe plastic deformation. The powder is subjected to severe deformation processes such as ball milling and high-pressure gas ball milling to form a bimodal structure powder with fine surface grains and coarse internal grains, and then metallurgical sintering is performed to form a heterogeneous structure material with a harmonic structure; the present invention only requires homogenization annealing-hot rolling-annealing treatment, so the process of the present invention is extremely simple, easy to implement, conducive to industrial production, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a metallographic picture of the copper-zinc-aluminum-iron high-strength and toughness brass alloy material prepared in Example 1 of the present invention.
[0023] Figure 2 This is a BSE picture of the copper-zinc-aluminum-iron high-strength and toughness brass alloy material prepared in Example 1 of the present invention.
[0024] Figure 3 This is a phase distribution picture of the copper-zinc-aluminum-iron high-strength and toughness brass alloy material prepared in Example 1 of the present invention.
[0025] Figure 4 This is a mechanical property curve of the copper-zinc-aluminum-iron high-strength and toughness brass alloy material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is described in more detail below with reference to the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited to these embodiments.
[0027] An α+β dual-phase high-strength and toughness brass alloy material with a harmonic structure has an α phase as a core and an α+β dual-phase as a shell, and its composition includes, by weight percentage, 65.5-83.5wt% copper, 14-26wt% zinc, 2-5wt% aluminum and 0.5-3.5wt% iron.
[0028] The composition includes, by weight percentage: 68.5-81.5wt% copper, 15-24wt% zinc, 2.5-4.5wt% aluminum, and 1-3wt% iron.
[0029] The composition includes, by weight percentage, 71-79.5 wt % copper, 16-22 wt % zinc, 3-4 wt % aluminum, and 1.5-3 wt % iron.
[0030] The composition includes, by weight percentage: 73.5-78wt% copper, 17-20wt% zinc, 3-3.5wt% aluminum, and 2-3wt% iron.
[0031] The high-strength and toughness brass alloy material is obtained by subjecting the cast alloy to homogenization annealing-hot rolling-annealing.
[0032] A method for preparing an α+β dual-phase high-strength and toughness brass alloy material with a harmonic structure comprises the following steps:
[0033] (1) preparing a cast alloy: copper, zinc, aluminum, and iron are mixed according to the raw material composition ratio of a high-strength and tough brass alloy material, and then smelted and cooled to obtain a cast alloy;
[0034] (2) homogenization annealing treatment: homogenization annealing treatment is performed on the cast alloy obtained in step (1), followed by water cooling to complete the homogenization annealing treatment;
[0035] (3) hot rolling: hot rolling the alloy after homogenization annealing in step (2);
[0036] (4) Annealing: The alloy after hot rolling in step (3) is annealed and then air-cooled to obtain an α+β dual-phase high-strength and toughness brass alloy material with a harmonic structure.
[0037] In the step (2), the homogenization annealing temperature is 850-900° C., the homogenization annealing time is 12-36 hours, and the cooling method is water cooling.
[0038] In the step (3), the hot rolling temperature is 800-900° C., the number of hot rolling passes is 2-8, and the reduction ratio is 70-90%.
[0039] In the step (4), the annealing temperature is 800-850° C., the annealing time is 10-30 min, and the cooling method is air cooling.
[0040] Example 1
[0041] An α+β two-phase high-strength and tough brass alloy material with a harmonic structure has an α phase as a core and an α+β phase as a shell, and comprises, by mass percentage, 66wt% copper, 20wt% zinc, 4wt% aluminum and 2.8wt% iron.
[0042] It is prepared by the following preparation method, comprising the following steps:
[0043] (1) preparing a cast alloy: copper, zinc, aluminum, and iron metal raw materials are mixed in a composition ratio of 66 wt% copper, 20 wt% zinc, 4 wt% aluminum, and 2.8 wt% iron, respectively, and then smelted and cooled to obtain a cast alloy;
[0044] (2) homogenization annealing treatment: homogenization annealing treatment is performed on the cast alloy obtained in step (1) at 900° C. for 24 hours, followed by water cooling to complete the homogenization annealing treatment;
[0045] (3) hot rolling: the alloy subjected to homogenization annealing in step (2) was hot rolled at 850° C., and the material thickness was reduced to 1.8 mm after 5 passes of rolling, with a total reduction ratio of 86%;
[0046] (4) Annealing treatment: The sample after hot rolling in step (3) is annealed at 850° C. for 20 minutes, and then air-cooled to obtain an α+β dual-phase high-strength and toughness brass alloy material with a harmonic structure.
[0047] Figure 1 This is a metallographic picture of the copper-zinc-aluminum-iron high-strength and tough brass alloy material obtained. Figure 1It can be seen from a that the alloy presents a non-uniform harmonic structure consisting of an oblate α core (length and width are 168μm-606μm and 44μm-157μm, respectively) and an α+β dual-phase shell. Figure 1 As shown in (b), after hot rolling and annealing, the α core changes from a single coarse grain (homogenization annealing state) to a collection of many small grains, and the α+β two-phase shell region changes from elongated strips to equiaxed grains.
[0048] Figure 2 This is the BSE picture of the copper-zinc-aluminum-iron high-strength and tough brass alloy material obtained. Figure 2 It can be seen from a that the structure of the α+β dual-phase shell in the alloy is composed of delicate equiaxed α phase and β phase, the α core structure is a single α phase, and the nanoprecipitates (NP) β(FeAl) are evenly distributed on the matrix of all alloys, such as Figure 2 b and 2c. Figure 3 This is a phase distribution picture of the prepared copper-zinc-aluminum-iron high-strength and toughness brass alloy material. From the picture, the single-phase α core and the α+β dual-phase shell can be clearly observed. Figure 4 This is the mechanical property curve of the copper-zinc-aluminum-iron high-strength and tough brass alloy material. From the picture, it can be seen that the ultimate tensile strength of the alloy with harmonic structure at room temperature is 473.7 MPa. Its total elongation remains at 50.7%, showing a perfect combination of strength and ductility.
[0049] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. An α+β dual-phase high-strength and tough brass alloy material with a harmonic structure, It is characterized in that The invention has a harmonic structure with an α phase as a core and an α+β dual phase as a shell, and its composition includes, by weight percentage, 65.5-83.5wt% copper, 14-26wt% zinc, 2-5wt% aluminum and 0.5-3.5wt% iron.
2. The α+β dual-phase high-strength and toughness brass alloy material with a harmonic structure as claimed in claim 1, It is characterized in that The composition includes, by weight percentage: 68.5-81.5wt% copper, 15-24wt% zinc, 2.5-4.5wt% aluminum, and 1-3wt% iron.
3. The α+β dual-phase high-strength and toughness brass alloy material with harmonic structure as claimed in claim 1, It is characterized in that The composition includes, by weight percentage, 71-79.5 wt % copper, 16-22 wt % zinc, 3-4 wt % aluminum, and 1.5-3 wt % iron.
4. The α+β dual-phase high-strength and toughness brass alloy material with harmonic structure as claimed in claim 1, It is characterized in that The composition includes, by weight percentage, 73.5-78 wt % copper, 17-20 wt % zinc, 3-3.5 wt % aluminum, and 2-3 wt % iron.
5. The α+β dual-phase high-strength and toughness brass alloy material with harmonic structure as claimed in claim 1, It is characterized in that The high-strength and toughness brass alloy material is obtained by subjecting the cast alloy to homogenization annealing-hot rolling-annealing.
6. A method for preparing the α+β dual-phase high-strength and toughness brass alloy material with a harmonic structure as claimed in any one of claims 1 to 5, It is characterized in that The steps include: (1) preparing a cast alloy: copper, zinc, aluminum, and iron are mixed according to the composition ratio of high-strength and toughness brass alloy raw materials, then smelted, and cooled to obtain a cast alloy; (2) homogenization annealing treatment: homogenization annealing treatment is performed on the cast alloy obtained in step (1), followed by water cooling to complete the homogenization annealing treatment; (3) hot rolling: hot rolling the alloy after homogenization annealing in step (2); (4) Annealing: The alloy after hot rolling in step (3) is annealed and then air-cooled to obtain an α+β dual-phase high-strength and toughness brass alloy material with a harmonic structure.
7. The method for preparing the α+β dual-phase high-strength and toughness brass alloy material with a harmonic structure as claimed in claim 6, It is characterized in that In the step (2), the homogenization annealing temperature is 850-900° C., the homogenization annealing time is 12-36 hours, and the cooling method is water cooling.
8. The method for preparing the α+β dual-phase high-strength and toughness brass alloy material with a harmonic structure as claimed in claim 6, It is characterized in that The hot rolling temperature in step (3) is 800-900°C.
9. The method for preparing the α+β dual-phase high-strength and toughness brass alloy material with a harmonic structure as claimed in claim 6, It is characterized in that In the step (3), the hot rolling times are 2-8 times, and the reduction ratio is 70-90%.
10. The method for preparing the α+β dual-phase high-strength and toughness brass alloy material with a harmonic structure as claimed in claim 6, It is characterized in that In the step (4), the annealing temperature is 800-850° C., the annealing time is 10-30 min, and the cooling method is air cooling.